A kind of anti-corrosion material for oil well cement that resists carbon dioxide and hydrogen sulfide acid corrosion
By using a combination of slag, dust, toughening additives and latex additives in oil well cement, the corrosion problem of oil well cement in carbon dioxide and hydrogen sulfide environment is solved, significantly improving corrosion resistance and durability, and ensuring the solidification of oil wells Quality and production safety.
Patent Information
- Application Number
- CN202411270464.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-11
AI Technical Summary
Oil well cement is susceptible to corrosion in an environment containing carbon dioxide and hydrogen sulfide, resulting in structural damage and loss of sealing capacity. The prior art has poor anti-corrosion effect and low durability, which affects the cementing quality and production safety of oil wells.
Using an anti-corrosion material for oil well cement that resists carbon dioxide and hydrogen sulfide corrosion, including slag, dust, toughening additives and latex additives, the tiny pores of cement stones are filled, high-strength hydration products are generated, network structures are formed and network structures are improved. Depth, enhance corrosion resistance.
It significantly improves the corrosion resistance and durability of cement stone, enhances the stability and mechanical properties in environments containing carbon dioxide and hydrogen sulfide, and extends the service life of oil well cement.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of anti-corrosion cementing materials for oil and gas fields, and in particular relates to an anti-corrosion material for oil well cement that is resistant to carbon dioxide and hydrogen sulfide acid corrosion. Background Art
[0002] Well cement plays a vital role in the process of oil and gas extraction. It is not only used to seal the well wall and prevent pollution of the oil and gas layer, but also needs to withstand the high temperature and high pressure environment in the formation.
[0003] In oil and gas wells containing carbon dioxide (CO2) and hydrogen sulfide (H2S), they corrode oil well cement mainly in the following two ways: Chemical corrosion: CO2 dissolves in water to form carbonic acid, which further reacts with calcium hydroxide in cement to form calcium carbonate, causing the cement paste to expand and crack. H2S can directly react with certain components in cement to form sulfates (such as CaSO4·2H2O) and other corrosion products, which can also cause structural damage to the cement paste. Physical corrosion: The corrosion products of CO2 and H2S will block the pores of the cement paste, reduce its permeability, and at the same time aggravate the expansion and cracking of the cement paste, thereby accelerating the destruction of the physical structure.
[0004] Cement stone is easily corroded by acidic gases, which may lead to changes in cement properties, loss of sealing ability, and even cause annular air leakage. In severe cases, the entire well may be scrapped, resulting in huge economic losses. Studies have shown that there are many factors that affect the corrosion resistance of cement stone. In actual application, a variety of anti-corrosion admixtures are compounded to improve the comprehensive performance of cement stone. Therefore, the present invention proposes an oil well cement anti-corrosion material that can effectively resist CO2 and H2S acid corrosion at the same time, which is used to solve the problems of poor anti-corrosion effect and low durability of cement stone, which is of great significance for improving the cementing quality of oil wells and ensuring production safety. Summary of the invention
[0005] The purpose of the present invention is to provide an anti-corrosion material for oil well cement that is resistant to carbon dioxide and hydrogen sulfide acid corrosion, so as to solve the technical problems of poor anti-corrosion effect and low durability of oil well cement materials in the prior art.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] The invention provides an anti-corrosion material for oil well cement that is resistant to carbon dioxide and hydrogen sulfide corrosion. The anti-corrosion material for oil well cement that is resistant to carbon dioxide and hydrogen sulfide corrosion comprises the following raw materials in parts by weight: 5 to 30 parts of slag, 5 to 40 parts of dust, 2 to 8 parts of toughening additives and 2 to 8 parts of latex additives.
[0008] The slag is a by-product produced in the industrial process, and is one or both of blast furnace slag and steel slag; the dust is one or more of fly ash, silica ash, slag powder, marble and granite waste dust.
[0009] Furthermore, the toughening additive comprises the following raw materials in parts by weight: 2 to 5 parts of steel fiber, 0.2 to 1 part of polypropylene fiber, 1 to 3 parts of modified anti-corrosion and alkali-resistant glass fiber and 0.6 to 1.3 parts of Ni-based amorphous alloy fiber.
[0010] Furthermore, when preparing the modified anti-corrosion and alkali-resistant glass fiber, a polyacrylate emulsion is coated on the surface of the alkali-resistant glass fiber. After uniform coating and drying, the modified anti-corrosion and alkali-resistant glass fiber is obtained; the polyacrylate emulsion comprises the following raw materials in parts by weight: 1000 parts of water, 140-150 parts of polyacrylate, 7-8 parts of polyether polyester, 2-8 parts of polyvinyl alcohol, 3-10 parts of hydroxypropyl methylcellulose, 0.5-1.5 parts of octylphenol polyoxyethylene ether, 0.5-1.5 parts of benzoyl peroxide, 0.5-1.5 parts of hydroxyethyl cellulose and 0.5-1.5 parts of sodium citrate.
[0011] Furthermore, when preparing the polyacrylate emulsion, weighed polyacrylate, polyether polyester, octylphenol polyoxyethylene ether, benzoyl peroxide, hydroxyethyl cellulose and sodium citrate are added into a reaction kettle and stirred evenly. After heating, water, polyvinyl alcohol and hydroxypropyl methylcellulose are added and stirring is continued. After the reaction is completed, the emulsion is cooled to room temperature and filtered to obtain the polyacrylate emulsion.
[0012] Specifically, during the preparation of the polyacrylate emulsion, the polyacrylate emulsion is added into a reaction kettle and heated to 80-100° C., water, polyvinyl alcohol and hydroxypropyl methylcellulose are added, and stirring is continued. The reaction is completed after 1-4 hours.
[0013] Furthermore, the Ni-based amorphous alloy fiber has a diameter of 10-100 μm and a length of 1-5 mm.
[0014] Furthermore, the latex additive comprises the following raw materials in parts by weight: 60 to 90 parts of styrene-butadiene copolymer, 3 to 15 parts of stabilizer, 2 to 5 parts of dispersant and 2 to 13 parts of defoamer.
[0015] Furthermore, the stabilizer is one or more of cellulose ether, polyoxyethylene alkylphenol ether and polyoxyethylene fatty alcohol ether; the dispersant is one or more of melamine sulfonate, polynaphthalene sulfonate, lignin sulfonate and styrene sulfonate; the defoamer is one or two of polydimethylsiloxane and Tween 60.
[0016] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:
[0017] 1. The anti-corrosion material for oil well cement of the present invention, on the basis of the prior art, adds toughening additives of multiple fiber combinations, and is matched with slag, dust and latex additives. Slag with a large specific surface area can fill the tiny pores inside the cement stone, reduce the porosity and improve the density. In addition, the active ingredients of the slag can play a volcanic ash effect during the hydration process, react with calcium hydroxide in cement to generate hydration products such as CSH gel, which have higher strength and lower permeability. After being mixed with toughening additives with good toughness and latex additives with good impermeability and density, the corrosion resistance, strength and durability of the material can be effectively improved.
[0018] 2. When preparing the polyacrylate emulsion of the present invention, a reactive emulsifier and a small amount of nonionic emulsifier are used to replace the traditional emulsification system, which is beneficial to overcome the disadvantage of easy migration of traditional emulsifiers and improve the water resistance of the emulsion. At the same time, the production process combining pre-emulsification and seed polymerization can reduce the amount of emulsifier used, improve water resistance, and is beneficial to the stability of the polymerization system, reduce gel, make the emulsion particle size distribution uniform, and improve the rheological properties of the emulsion. Therefore, coating the polyacrylate emulsion on the surface of the glass fiber makes the modified anti-corrosion and alkali-resistant glass fiber have good wettability and permeability, can penetrate into the tiny pores of the cement slurry, and closely contact with the surface of the cement particles. During the solidification process of the cement slurry, a strong physical adsorption effect is formed between the coating molecules and the surface of the cement particles, which not only improves the stability of the glass fiber in the cement stone, but also enhances the overall mechanical properties of the cement stone, thereby enhancing the corrosion resistance of the material in an environment containing carbon dioxide and hydrogen sulfide.
[0019] 3. The present invention uniformly disperses the latex additive into the cement slurry. The styrene-butadiene copolymer forms a network structure during the solidification of the cement slurry, and is interwoven with other components in the cement stone to form a more compact and stable structure. The stabilizer prevents the cement slurry from stratification or precipitation during stirring and pumping. The dispersant uniformly disperses the cement particles to reduce agglomeration. The defoamer can eliminate bubbles in the cement slurry and reduce the porosity. The synergistic effect of the stabilizer, dispersant and defoamer in the latex additive further improves the density and impermeability of the cement stone, thereby enhancing its corrosion resistance. DETAILED DESCRIPTION
[0020] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0021] Example 1
[0022] This embodiment discloses an anti-corrosion material for oil well cement that is resistant to carbon dioxide and hydrogen sulfide corrosion, comprising the following raw materials: 5g of slag, 5g of dust, 2g of a toughening additive, and 2g of a latex additive.
[0023] Among them, the slag is blast furnace slag; the dust is an equal mixture of fly ash and silica fume; the toughening additive includes the following raw materials: 2g steel fiber, 0.2g polypropylene fiber, 1g modified anti-corrosion and alkali-resistant glass fiber and 0.6g Ni-based amorphous alloy fiber.
[0024] Among them, the diameter of the Ni-based amorphous alloy fiber is 10 μm and the length is 1 mm. When preparing the modified anti-corrosion and alkali-resistant glass fiber, the surface of the alkali-resistant glass fiber is coated with polyacrylate emulsion, and after uniform coating and drying, the modified anti-corrosion and alkali-resistant glass fiber is obtained. Specifically, when preparing the polyacrylate emulsion, 140g of polyacrylate, 7g of polyether polyester, 0.5g of octylphenol polyoxyethylene ether, 0.5g of benzoyl peroxide, 0.5g of hydroxyethyl cellulose and 0.5g of sodium citrate are weighed and added to the reactor and stirred evenly, heated to 80°C, and then 1000g of water, 2g of polyvinyl alcohol and 3g of hydroxypropyl methylcellulose are added, and stirring is continued. After reacting for 4 hours, the emulsion is cooled to room temperature and filtered to obtain a polyacrylate emulsion.
[0025] Specifically, the latex additive includes the following raw materials: 60g of styrene-butadiene copolymer, 3g of stabilizer, 2g of dispersant and 2g of defoamer, wherein the stabilizer is cellulose ether; the dispersant is a mixture of lignin sulfonate and styrene sulfonate in equal amounts; and the defoamer is polydimethylsiloxane.
[0026] Example 2
[0027] This embodiment discloses an anti-corrosion material for oil well cement that is resistant to carbon dioxide and hydrogen sulfide corrosion, comprising the following raw materials: 10 g of slag, 10 g of dust, 4 g of a toughening additive, and 3 g of a latex additive.
[0028] Among them, the slag is steel slag; the dust is silica fume; the toughening additive includes the following raw materials: 3g steel fiber, 0.3g polypropylene fiber, 1.5g modified anti-corrosion and alkali-resistant glass fiber and 0.8g Ni-based amorphous alloy fiber.
[0029] Among them, the diameter of the Ni-based amorphous alloy fiber is 30μm and the length is 2.5mm. When preparing the modified anti-corrosion and alkali-resistant glass fiber, the surface of the alkali-resistant glass fiber is coated with polyacrylate emulsion, and after uniform coating and drying, the modified anti-corrosion and alkali-resistant glass fiber is obtained. Specifically, when preparing the polyacrylate emulsion, weighed 145g polyacrylate, 7g polyether polyester, 0.9g octylphenol polyoxyethylene ether, 1g benzoyl peroxide, 1g hydroxyethyl cellulose and 0.9g sodium citrate are added to the reactor and stirred evenly, heated to 85°C, and then 1000g water, 4g polyvinyl alcohol and 5g hydroxypropyl methylcellulose are added, stirring is continued, and after reacting for 2h, the emulsion is cooled to room temperature and filtered to obtain a polyacrylate emulsion.
[0030] Specifically, the latex additive includes the following raw materials: 70g of styrene-butadiene copolymer, 6g of stabilizer, 3g of dispersant and 8g of defoamer, wherein the stabilizer is polyoxyethylene fatty alcohol ether, the dispersant is melamine sulfonate and the defoamer is polydimethylsiloxane.
[0031] Example 3
[0032] This embodiment discloses an anti-corrosion material for oil well cement that is resistant to carbon dioxide and hydrogen sulfide acid corrosion, comprising the following raw materials: 20 g of slag, 20 g of dust, 7 g of a toughening additive, and 6 g of a latex additive.
[0033] Among them, slag is an equal mixture of blast furnace slag and steel slag; dust is an equal mixture of fly ash and marble and granite waste dust.
[0034] The toughening additive comprises the following raw materials: 5 g of steel fiber, 0.8 g of polypropylene fiber, 2.8 g of modified anti-corrosion and alkali-resistant glass fiber and 1.2 g of Ni-based amorphous alloy fiber.
[0035] Among them, the diameter of the Ni-based amorphous alloy fiber is 100 μm and the length is 4 mm. When preparing the modified anti-corrosion and alkali-resistant glass fiber, the surface of the alkali-resistant glass fiber is coated with polyacrylate emulsion, and after uniform coating and drying, the modified anti-corrosion and alkali-resistant glass fiber is obtained; specifically, when preparing the polyacrylate emulsion, 150g of polyacrylate, 8g of polyether polyester, 1.2g of octylphenol polyoxyethylene ether, 1.3g of benzoyl peroxide, 1.5g of hydroxyethyl cellulose and 1.5g of sodium citrate are weighed and added into the reactor and stirred evenly, and the temperature is raised to 100°C, 1000g of water, 7g of polyvinyl alcohol and 10g of hydroxypropyl methylcellulose are added, and stirring is continued. After reacting for 1 hour, the emulsion is cooled to room temperature and filtered to obtain the polyacrylate emulsion.
[0036] Specifically, the latex additive includes the following raw materials: 90g of styrene-butadiene copolymer, 15g of stabilizer, 5g of dispersant and 13g of defoamer, wherein the stabilizer is polyoxyethylene alkylphenol ether, the dispersant is lignin sulfonate and the defoamer is polydimethylsiloxane.
[0037] Example 4
[0038] This embodiment discloses an anti-corrosion material for oil well cement that is resistant to carbon dioxide and hydrogen sulfide corrosion, comprising the following raw materials: 30 g of slag, 40 g of dust, 8 g of a toughening additive, and 8 g of a latex additive.
[0039] Among them, slag is a by-product produced in the industrial process, which is blast furnace slag; the dust is an equal mixture of fly ash and silica fume; the toughening additive includes the following raw materials: 5g steel fiber, 1g polypropylene fiber, 3g modified anti-corrosion and alkali-resistant glass fiber and 1.3g Ni-based amorphous alloy fiber.
[0040] Among them, the diameter of the Ni-based amorphous alloy fiber is 60 μm and the length is 5 mm. When preparing the modified anti-corrosion and alkali-resistant glass fiber, the surface of the alkali-resistant glass fiber is coated with polyacrylate emulsion, and after uniform coating and drying, the modified anti-corrosion and alkali-resistant glass fiber is obtained; specifically, when preparing the polyacrylate emulsion, 150g of polyacrylate, 8g of polyether polyester, 1.5g of octylphenol polyoxyethylene ether, 1.5g of benzoyl peroxide, 1.5g of hydroxyethyl cellulose and 1.5g of sodium citrate are weighed and added into the reactor and stirred evenly, and the temperature is raised to 100°C, 1000g of water, 8g of polyvinyl alcohol and 10g of hydroxypropyl methylcellulose are added, and stirring is continued. After reacting for 3 hours, the emulsion is cooled to room temperature and filtered to obtain the polyacrylate emulsion.
[0041] Specifically, the latex additive includes the following raw materials: 90g of styrene-butadiene copolymer, 15g of stabilizer, 5g of dispersant and 13g of defoamer, wherein the stabilizer is cellulose ether, the dispersant is styrene sulfonate and the defoamer is Tween 60.
[0042] Example 5
[0043] This embodiment discloses an anti-corrosion material for oil well cement that is resistant to carbon dioxide and hydrogen sulfide corrosion, comprising the following raw materials: 15 g of slag, 40 g of dust, 6.5 g of a toughening additive, and 6.5 g of a latex additive.
[0044] Among them, slag is a by-product produced in the industrial process, which is blast furnace slag; the dust is marble and granite waste dust; the toughening additive includes the following raw materials: 9g steel fiber, 0.8g polypropylene fiber, 5g modified anti-corrosion and alkali-resistant glass fiber and 2g Ni-based amorphous alloy fiber.
[0045] Among them, the diameter of the Ni-based amorphous alloy fiber is 50 μm and the length is 3.5 mm. When preparing the modified anti-corrosion and alkali-resistant glass fiber, the surface of the alkali-resistant glass fiber is coated with polyacrylate emulsion, and after uniform coating and drying, the modified anti-corrosion and alkali-resistant glass fiber is obtained; specifically, when preparing the polyacrylate emulsion, 145g of polyacrylate, 7g of polyether polyester, 1.1g of octylphenol polyoxyethylene ether, 1.1g of benzoyl peroxide, 1.1g of hydroxyethyl cellulose and 1.5g of sodium citrate are weighed and added into the reactor and stirred evenly, and the temperature is raised to 95°C, 1000g of water, 7g of polyvinyl alcohol and 7.5g of hydroxypropyl methylcellulose are added, and stirring is continued. After reacting for 4 hours, the emulsion is cooled to room temperature and filtered to obtain the polyacrylate emulsion.
[0046] Specifically, the latex additive includes the following raw materials: 90g of styrene-butadiene copolymer, 15g of stabilizer, 5g of dispersant and 13g of defoamer, wherein the stabilizer is cellulose ether, the dispersant is styrene sulfonate and the defoamer is Tween 60.
[0047] Example 6
[0048] This embodiment discloses an anti-corrosion material for oil well cement that is resistant to carbon dioxide and hydrogen sulfide corrosion, comprising the following raw materials: 30 g of slag, 25 g of dust, 7 g of a toughening additive, and 7.5 g of a latex additive.
[0049] Among them, slag is a by-product produced in the industrial process, which is blast furnace slag; the dust is an equal mixture of fly ash and silica fume; the toughening additive includes the following raw materials: 5g steel fiber, 1g polypropylene fiber, 3g modified anti-corrosion and alkali-resistant glass fiber and 1.3g Ni-based amorphous alloy fiber.
[0050] Among them, the diameter of the Ni-based amorphous alloy fiber is 65μm and the length is 3.8mm. When preparing the modified anti-corrosion and alkali-resistant glass fiber, the surface of the alkali-resistant glass fiber is coated with polyacrylate emulsion, and after uniform coating and drying, the modified anti-corrosion and alkali-resistant glass fiber is obtained; specifically, when preparing the polyacrylate emulsion, 148g of polyacrylate, 8g of polyether polyester, 1.5g of octylphenol polyoxyethylene ether, 1.3g of benzoyl peroxide, 1.5g of hydroxyethyl cellulose and 1.5g of sodium citrate are weighed and added into the reactor and stirred evenly, and the temperature is raised to 100°C, 1000g of water, 8g of polyvinyl alcohol and 10g of hydroxypropyl methylcellulose are added, and stirring is continued. After reacting for 2h, the emulsion is cooled to room temperature and filtered to obtain the polyacrylate emulsion.
[0051] Specifically, the latex additive includes the following raw materials: 80g of styrene-butadiene copolymer, 15g of stabilizer, 5g of dispersant and 7g of defoamer, wherein the stabilizer is cellulose ether, the dispersant is styrene sulfonate and the defoamer is Tween 60.
[0052] Example 7
[0053] This embodiment discloses an anti-corrosion material for oil well cement that is resistant to carbon dioxide and hydrogen sulfide acid corrosion, comprising the following raw materials: 20 g of slag, 40 g of dust, 5.8 g of a toughening additive, and 7.9 g of a latex additive.
[0054] Among them, slag is a by-product produced in the industrial process, which is blast furnace slag; the dust is an equal mixture of fly ash and silica fume; the toughening additive includes the following raw materials: 4.5g steel fiber, 1g polypropylene fiber, 3g modified anti-corrosion and alkali-resistant glass fiber and 1g Ni-based amorphous alloy fiber.
[0055] Among them, the diameter of the Ni-based amorphous alloy fiber is 60 μm and the length is 5 mm. When preparing the modified anti-corrosion and alkali-resistant glass fiber, the surface of the alkali-resistant glass fiber is coated with polyacrylate emulsion, and after uniform coating and drying, the modified anti-corrosion and alkali-resistant glass fiber is obtained; specifically, when preparing the polyacrylate emulsion, 150g of polyacrylate, 8g of polyether polyester, 1.5g of octylphenol polyoxyethylene ether, 1.5g of benzoyl peroxide, 1.5g of hydroxyethyl cellulose and 1.5g of sodium citrate are weighed and added into the reactor and stirred evenly, and the temperature is raised to 90°C, 1000g of water, 8g of polyvinyl alcohol and 10g of hydroxypropyl methylcellulose are added, and stirring is continued. After reacting for 3 hours, the emulsion is cooled to room temperature and filtered to obtain the polyacrylate emulsion.
[0056] Specifically, the latex additive includes the following raw materials: 90g of styrene-butadiene copolymer, 15g of stabilizer, 5g of dispersant and 10g of defoamer, wherein the stabilizer is cellulose ether, the dispersant is styrene sulfonate and the defoamer is Tween 60.
[0057] Example 8
[0058] This embodiment discloses an anti-corrosion material for oil well cement that is resistant to carbon dioxide and hydrogen sulfide corrosion, comprising the following raw materials: 30 g of slag, 40 g of dust, 7.5 g of a toughening additive, and 6 g of a latex additive.
[0059] Among them, slag is a by-product produced in the industrial process, which is blast furnace slag; the dust is an equal mixture of fly ash and silica fume; the toughening additive includes the following raw materials: 4.5g steel fiber, 1g polypropylene fiber, 3g modified anti-corrosion and alkali-resistant glass fiber and 0.8g Ni-based amorphous alloy fiber.
[0060] Among them, the diameter of the Ni-based amorphous alloy fiber is 60 μm and the length is 2.5 mm. When preparing the modified anti-corrosion and alkali-resistant glass fiber, the surface of the alkali-resistant glass fiber is coated with polyacrylate emulsion, and after uniform coating and drying, the modified anti-corrosion and alkali-resistant glass fiber is obtained; specifically, when preparing the polyacrylate emulsion, 150g of polyacrylate, 8g of polyether polyester, 1.5g of octylphenol polyoxyethylene ether, 1.5g of benzoyl peroxide, 1.5g of hydroxyethyl cellulose and 1.5g of sodium citrate are weighed and added into the reactor and stirred evenly, and the temperature is raised to 100°C, 1000g of water, 8g of polyvinyl alcohol and 10g of hydroxypropyl methylcellulose are added, and stirring is continued. After reacting for 3 hours, the emulsion is cooled to room temperature and filtered to obtain the polyacrylate emulsion.
[0061] Specifically, the latex additive includes the following raw materials: 90g of styrene-butadiene copolymer, 15g of stabilizer, 5g of dispersant and 13g of defoamer, wherein the stabilizer is cellulose ether, the dispersant is melamine sulfonate and the defoamer is polydimethylsiloxane.
[0062] Example 9
[0063] This embodiment discloses an anti-corrosion material for oil well cement that is resistant to carbon dioxide and hydrogen sulfide acid corrosion, comprising the following raw materials: 28 g of slag, 40 g of dust, 6.8 g of a toughening additive, and 7.2 g of a latex additive.
[0064] Among them, slag is a by-product produced in the industrial process, which is blast furnace slag; the dust is an equal mixture of fly ash and silica fume; the toughening additive includes the following raw materials: 5g steel fiber, 1g polypropylene fiber, 3g modified anti-corrosion and alkali-resistant glass fiber and 0.7g Ni-based amorphous alloy fiber.
[0065] Among them, the diameter of the Ni-based amorphous alloy fiber is 85 μm and the length is 2 mm. When preparing the modified anti-corrosion and alkali-resistant glass fiber, the surface of the alkali-resistant glass fiber is coated with polyacrylate emulsion, and after uniform coating and drying, the modified anti-corrosion and alkali-resistant glass fiber is obtained; specifically, when preparing the polyacrylate emulsion, 150g of polyacrylate, 8g of polyether polyester, 1.5g of octylphenol polyoxyethylene ether, 1.5g of benzoyl peroxide, 1.5g of hydroxyethyl cellulose and 1.5g of sodium citrate are weighed and added into a reactor and stirred evenly, and the temperature is raised to 100°C, 1000g of water, 8g of polyvinyl alcohol and 10g of hydroxypropyl methylcellulose are added, and stirring is continued. After reacting for 3 hours, the emulsion is cooled to room temperature and filtered to obtain the polyacrylate emulsion.
[0066] Specifically, the latex additive includes the following raw materials: 90g of styrene-butadiene copolymer, 15g of stabilizer, 3g of dispersant and 13g of defoamer, wherein the stabilizer is polyoxyethylene fatty alcohol ether; the dispersant is an equal mixture of melamine sulfonate, polynaphthalene sulfonate and lignin sulfonate; and the defoamer is Tween 60.
[0067] Comparative Example 1
[0068] Compared with Example 4, in Comparative Example 1, no modified anti-corrosion and alkali-resistant glass fiber is added to the anti-corrosion material resistant to carbon dioxide and hydrogen sulfide acid corrosion for oil well cement, and other conditions remain unchanged.
[0069] Comparative Example 2
[0070] Compared with Example 4, in Comparative Example 2, alkali-resistant glass fiber is used instead of modified anti-corrosion alkali-resistant glass fiber in the anti-corrosion material resistant to carbon dioxide and hydrogen sulfide acid corrosion for oil well cement, and other conditions remain unchanged.
[0071] Comparative Example 3
[0072] Compared with Example 4, in Comparative Example 3, no Ni-based amorphous alloy fiber is added to the anti-corrosion material for oil well cement resistant to carbon dioxide and hydrogen sulfide acid corrosion, and other conditions remain unchanged.
[0073] Comparative Example 4
[0074] Comparative Example 4 Compared with Example 4, in Comparative Example 4, no latex additive is added to the anti-corrosion material for oil well cement resistant to carbon dioxide and hydrogen sulfide acid corrosion, and other conditions remain unchanged.
[0075] Experimental example
[0076] The anti-corrosion materials for oil well cement resistant to carbon dioxide and hydrogen sulfide corrosion of Examples 1-9 of the present invention and Comparative Examples 1-4 are prepared into a cementing cement slurry system, which includes the following components: 60g of Class G oil well cement, 35g of anti-corrosion materials for oil well cement resistant to carbon dioxide and hydrogen sulfide corrosion, and 65g of water.
[0077] Prepare cement slurry according to API Standard 10 and pour it into the test mold, place it in a high-temperature and high-pressure curing kettle for curing for 24 hours, and then take it out and demold it; after marking the prepared cement stone with group numbers, put it into the corrosion curing kettle, fill it with water and seal it; introduce CO2 or H2S and heat it to the experimental temperature, pay attention to the changes in temperature and pressure at any time, and adjust them in time; after the experiment, test the corrosion performance of the sample, including changes in compressive strength and permeability.
[0078] 1. Testing the anti-CO2 corrosion performance of cementing slurry system
[0079] Under the conditions of CO2 partial pressure of 4.0 MPa, experimental time of 70 days and experimental temperature of 100°C, the CO2 corrosion resistance of the cement slurry system prepared with the anti-corrosion materials resistant to carbon dioxide and hydrogen sulfide acid corrosion for oil well cement of Examples 1-9 of the present invention and Comparative Examples 1-4 was tested. The results are shown in Table 1.
[0080] Table 1
[0081]
[0082] It can be seen from the test results in Table 1 that the cementing cement slurry systems prepared by adding the anti-corrosion materials for oil well cement resistant to carbon dioxide and hydrogen sulfide acid corrosion of Examples 1-9 of the present invention all have high CO2 corrosion resistance, and the strength of cement stone increases and the permeability decreases after corrosion. It can be seen from the comparison between Comparative Examples 1-4 and Examples 1-9 that the addition of modified anti-corrosion and alkali-resistant glass fibers, Ni-based amorphous alloy fibers and latex additives can improve their CO2 corrosion resistance, among which the synergistic effect of the three together has the best CO2 corrosion resistance.
[0083] 2. Testing the H2S corrosion resistance of cement slurry system
[0084] Under the conditions of H2S partial pressure of 2.0 MPa, experimental time of 70 days and experimental temperature of 100°C, the H2S corrosion resistance of the cement slurry system prepared with the anti-corrosion materials resistant to carbon dioxide and hydrogen sulfide acid corrosion for oil well cement of Examples 1-9 of the present invention and Comparative Examples 1-4 was tested. The results are shown in Table 2.
[0085] Table 2
[0086]
[0087] From the test results in Table 2, it can be seen that the cementing cement slurry systems prepared by adding the anti-corrosion materials for oil well cement resistant to carbon dioxide and hydrogen sulfide acid corrosion of Examples 1-9 of the present invention all have high H2S corrosion resistance, and the strength of cement stone increases and the permeability decreases after corrosion. From the comparison between Comparative Examples 1-4 and Examples 1-9, it can be seen that the addition of modified anti-corrosion and alkali-resistant glass fibers, Ni-based amorphous alloy fibers and latex additives can improve their H2S corrosion resistance.
[0088] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
[0089] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. An anti-corrosion material for oil well cement that is resistant to carbon dioxide and hydrogen sulfide acid corrosion, characterized in that: The anti-corrosion material for oil well cement resistant to carbon dioxide and hydrogen sulfide acid corrosion comprises the following raw materials in parts by weight: 5-30 parts of slag, 5-40 parts of dust, 2-8 parts of toughening additives and 2-8 parts of latex additives; the toughening additives comprise the following raw materials in parts by weight: 2-5 parts of steel fiber, 0.2-1 part of polypropylene fiber, 1-3 parts of modified anti-corrosion and alkali-resistant glass fiber and 0.6-1.3 parts of Ni-based amorphous alloy fiber; When preparing the modified anti-corrosion and alkali-resistant glass fiber, a polyacrylate emulsion is coated on the surface of the alkali-resistant glass fiber, and after uniform coating and drying, the modified anti-corrosion and alkali-resistant glass fiber is obtained; the polyacrylate emulsion comprises the following raw materials in parts by weight: 1000 parts of water, 140-150 parts of polyacrylate, 7-8 parts of polyether polyester, 2-8 parts of polyvinyl alcohol, 3-10 parts of hydroxypropyl methylcellulose, 0.5-1.5 parts of octylphenol polyoxyethylene ether, 0.5-1.5 parts of benzoyl peroxide, 0.5-1.5 parts of hydroxyethyl cellulose and 0.5-1.5 parts of sodium citrate; When preparing the polyacrylate emulsion, weighed polyacrylate, polyether polyester, octylphenol polyoxyethylene ether, benzoyl peroxide, hydroxyethyl cellulose and sodium citrate are added into a reaction kettle and stirred evenly. After heating, water, polyvinyl alcohol and hydroxypropyl methylcellulose are added and stirred continuously. After the reaction is completed, the emulsion is cooled to room temperature and filtered to obtain the polyacrylate emulsion. When preparing the polyacrylate emulsion, add it into a reaction kettle and heat it to 80-100° C., add water, polyvinyl alcohol and hydroxypropyl methylcellulose, continue stirring, and react for 1-4 hours; The latex additive comprises the following raw materials in parts by weight: 60-90 parts of styrene-butadiene copolymer, 3-15 parts of stabilizer, 2-5 parts of dispersant and 2-13 parts of defoamer.
2. The anti-corrosion material for oil well cement resistant to carbon dioxide and hydrogen sulfide corrosion according to claim 1, characterized in that: The slag is one or both of blast furnace slag and steel slag; the dust is one or more of fly ash, silica ash, slag powder, marble and granite waste dust.
3. The anti-corrosion material for oil well cement resistant to carbon dioxide and hydrogen sulfide corrosion according to claim 1, characterized in that: The Ni-based amorphous alloy fiber has a diameter of 10-100 μm and a length of 1-5 mm.
4. The anti-corrosion material for oil well cement resistant to carbon dioxide and hydrogen sulfide corrosion according to claim 1, characterized in that: The stabilizer is one or more of cellulose ether, polyoxyethylene alkylphenol ether and polyoxyethylene fatty alcohol ether.
5. The anti-corrosion material for oil well cement resistant to carbon dioxide and hydrogen sulfide corrosion according to claim 1, characterized in that: The dispersant is one or more of melamine sulfonate, polynaphthalene sulfonate, lignin sulfonate and styrene sulfonate.
6. The anti-corrosion material for oil well cement resistant to carbon dioxide and hydrogen sulfide acid corrosion according to claim 1, characterized in that: The defoaming agent is one or both of polydimethylsiloxane and Tween 60.
Citation Information
Patent Citations
Efficient erosion-resistant anti-gas-channeling cement paste system
CN107216070A
Oil well cement paste containing elastic particles
CN117024075A