Elastic gel particle and preparation method thereof

Through the combination of silicate, cross-linking agent, sulfonated phenolic resin and polyvinyl alcohol, elastic jelly particles that are resistant to high temperature and high salt are prepared, which solves the problem of ineffective use of existing granular profile control agents in high temperature and high salt environments. It solves the problem effectively and achieves effective injection and stable plugging effect in fracture-cavity reservoirs.

CN118772447AActive Publication Date: 2024-10-15CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310344855.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-03
Publication Date
2024-10-15
Estimated Expiration
2043-04-03

AI Technical Summary

Technical Problem

Existing granular profile control agents have problems such as high density, poor deformation ability, insufficient temperature and salt resistance, and low strength in high-temperature and high-salt environments, resulting in difficulty in injection and poor use results in fracture-cavity reservoirs.

Method used

Using elastic jelly particles prepared from silicate, cross-linking agent, sulfonated phenolic resin and polyvinyl alcohol under the action of acid catalyst, through stirring, mixing and granulation processes, a product with a temperature resistance of 130°C and a salt resistance of 210,000 mg/L was prepared. Elastic gel particles with high strength, elasticity and strong deformation ability.

Benefits of technology

The prepared elastic jelly particles remain stable under high-temperature and high-salt conditions, have good toughness and deformation recovery capabilities, are suitable for flow channel adjustment in fracture-cavity reservoirs, and have low density for easy suspension and injection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004159244370000071
    Figure BDA0004159244370000071
  • Figure BDA0004159244370000081
    Figure BDA0004159244370000081
  • Figure BDA0004159244370000082
    Figure BDA0004159244370000082
Patent Text Reader

Abstract

The invention provides elastic gel particles and a preparation method thereof. The elastic gel particles are obtained by granulating gel prepared from silicate, a cross-linking agent, sulfonated phenolic resin and polyvinyl alcohol under the action of an acid catalyst, and the particle size is 1 * 10 < 1 >-3 * 10 < 6 > nm. The gel storage modulus of the prepared elastic gel particle is 780-1953Pa, the temperature resistance reaches 130 DEG C, the mineralization resistance reaches 214812.46 mg / L, and the elastic gel particle is good in toughness and stability: after the elastic gel particle is soaked for 90 days at the temperature of 130 DEG C and the mineralization resistance reaches 214812.46 mg / L, the deformation recovery rate is 60-87%, the dehydration rate is 15-30%, and the volume shrinkage rate is 29-45% after the elastic gel particle is extruded for five times, so that the elastic gel particle has a good and long-term stable plugging adjusting effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of oilfield chemistry, and in particular relates to elastic jelly particles and a preparation method thereof. Background Art

[0002] Most of the oil fields in western my country are high-temperature, high-salinity fracture-cave reservoirs with well-developed millimeter-level fractures. The heterogeneity of the formation is particularly prominent. Due to the presence of large fractures and caves, the injected water flows seriously along the large pores and micro-fractures, the sweep coefficient is low, and the water drive recovery rate is low. Granular profile control agent is a widely available, cost-effective profile control agent, especially for large pore blockage in fracture-cave reservoirs. And because it is already a finished product under ground conditions, it does not need to react or cross-link under formation conditions, which can partially avoid a series of adverse effects caused by formation factors. However, granular profile control agents used for fracture and large pore blockage in fracture-cave reservoirs face the problem of plugging agent injection during application, as well as poor temperature and salt resistance, insufficient deformation and suspension capabilities, and other challenges. The types of particles in the prior art are mainly divided into inorganic particles and cross-linked polymer particles. They are the most widely used particle profile control agents in the current oilfield development process. However, they still have many problems when facing the harsh reservoir environment of the oilfield. Inorganic particles have high strength and can remain stable for a long time under high temperature and high salt conditions, but they have high density and are difficult to be suspended and carried. The particles are difficult to inject and easily clog the wells, causing operational accidents. Cross-linked polymer particles have poor heat and salt resistance and are easily degraded and shrunk in high temperature environments. At the same time, these polymers have high molecular weights and are difficult to prepare high-concentration gel solutions. Therefore, the strength of the formed gel is limited, and the strength of the particles prepared thereby is also limited, making it difficult to meet the use requirements. Summary of the invention

[0003] In view of the problems of high density, poor deformation ability, insufficient temperature and salt resistance, and low strength of the particle-type profile control agent in the prior art, the purpose of the present invention is to provide an elastic jelly particle with a temperature resistance of 130°C, a salt resistance of 210,000 mg / L, high strength, strong elasticity and deformation ability, low shrinkage rate when encountering salt water, easy suspension, and easy injection, and a preparation method thereof. The elastic jelly particle is a particle-type profile control agent, which provides support for the flow channel adjustment of high-temperature and high-salt fracture-cavity reservoirs.

[0004] To achieve the above object, one of the present inventions provides a method for preparing elastic jelly particles, which comprises the following steps:

[0005] 1) mixing silicate and water to obtain a first dispersion;

[0006] 2) mixing the crosslinking agent, the sulfonated phenolic resin and the first dispersion to obtain a second dispersion;

[0007] 3) mixing polyvinyl alcohol and the second dispersion to obtain a third dispersion;

[0008] 4) mixing the acid catalyst and the third dispersion, reacting to obtain jelly, and granulating to obtain the elastic jelly particles.

[0009] According to a specific embodiment of the present invention, the mass of the elastic jelly particles is calculated as 100%, the amount of the silicate is 2wt% to 6wt%, the amount of the cross-linking agent is 0.3wt% to 0.7wt%, the amount of the sulfonated phenolic resin is 1wt% to 3wt%, the amount of the polyvinyl alcohol is 4wt% to 10wt%, the amount of the acid catalyst is 0.5wt% to 1.5wt%, and the amount of water is 78.8wt% to 92.2wt%;

[0010] Preferably, taking the mass of the elastic jelly particles as 100%, the amount of the silicate is 2wt% to 4wt%, the amount of the cross-linking agent is 0.3wt% to 0.5wt%, the amount of the sulfonated phenol-formaldehyde resin is 1wt% to 2wt%, the amount of the polyvinyl alcohol is 4wt% to 10wt%, the amount of the acid catalyst is 1wt%, and the amount of water is 82.5wt% to 88.7wt%.

[0011] According to a specific embodiment of the present invention, the silicate is sodium bentonite; and / or

[0012] The cross-linking agent is selected from aldehyde cross-linking agents and / or hexamethylenetetramine; and / or

[0013] The acid catalyst is an inorganic acid and / or an organic acid; and / or

[0014] The mineralization of the water is less than 1000 mg / L;

[0015] Preferably, the aldehyde cross-linking agent is selected from at least one of formaldehyde, paraformaldehyde, glyoxal, glutaraldehyde and terephthalaldehyde; and / or

[0016] The organic acid comprises halogenated acetic acid and / or alkylbenzene sulfonic acid;

[0017] Preferably, the inorganic acid is hydrochloric acid and / or sulfuric acid; and / or the halogenated acetic acid is chloroacetic acid; and / or the alkylbenzenesulfonic acid is p-toluenesulfonic acid.

[0018] According to a specific embodiment of the present invention, the sulfur content of the sulfonated phenolic resin is 8wt% to 10wt%; and / or the solid content is not less than 90wt%; and / or

[0019] The polyvinyl alcohol has a degree of alcoholysis of 87% to 89%; and / or a molecular weight of 100,000 to 1,200,000;

[0020] Preferably, the polyvinyl alcohol is polyvinyl alcohol 2488.

[0021] According to a specific embodiment of the present invention, in step 4), the reaction condition is to stand at 22° C. to 25° C. for 4 to 8 hours.

[0022] According to a specific embodiment of the present invention, in step 4), the strength of the jelly reaches level I according to the visual code evaluation method; and / or

[0023] During the granulation process, spraying an alkali solution onto the surface of the elastic jelly particles to adjust the pH value on the surface of the elastic jelly particles to neutral;

[0024] Preferably, the alkali solution is selected from at least one of sodium hydroxide solution, sodium carbonate solution, triethanolamine and sodium bicarbonate solution;

[0025] Preferably, the alkali solution is selected from at least one of an aqueous sodium hydroxide solution, an aqueous sodium carbonate solution, triethanolamine and an aqueous sodium bicarbonate solution;

[0026] Preferably, the solute mass fraction of the sodium hydroxide aqueous solution, the sodium carbonate aqueous solution and the sodium bicarbonate aqueous solution is 1 wt %.

[0027] According to a specific embodiment of the present invention, the steps 1) to 4) are all mixed by stirring;

[0028] Preferably, the stirring speed in steps 1) to 4) is independently 300 rpm to 600 rpm.

[0029] The visual code evaluation method described in the present invention refers to the classification of plugging agent gel strength (Gel Strength Codes for short GSC) by Sydansk et al. into 10 levels based on visual inspection results. Among them, level I refers to the gel strength of rigid gel that does not deform on the gel surface when flipped.

[0030] The second aspect of the present invention provides elastic jelly particles prepared by the method described in the first aspect of the present invention.

[0031] According to a specific embodiment of the present invention, the particle size of the elastic jelly particles is 1×10 1 nm to 3×10 6 nm.

[0032] Application of the elastic jelly particles prepared by the method according to one of the present inventions or the elastic jelly particles according to the second present invention in high-temperature and high-salinity fracture-cavern oil reservoirs, especially in flow channel adjustment of high-temperature and high-salinity fracture-cavern oil reservoirs.

[0033] According to a specific embodiment of the present invention, the high temperature is not less than 130° C.; and / or

[0034] The high salt has a mineralization of not less than 210000 mg / L.

[0035] Beneficial effects of the present invention:

[0036] Aiming at the problems of high density, poor deformation ability, insufficient temperature and salt resistance, and low strength of the particle-type profile control agent in the prior art, the elastic jelly particles provided by the present invention are prepared by granulation of jelly prepared by silicate, cross-linking agent, sulfonated phenolic resin, and polyvinyl alcohol under the action of an acid catalyst. The jelly storage modulus for preparing the elastic jelly particles is 780 to 1953Pa, the temperature resistance reaches 130°C, the mineralization resistance reaches 214812.46mg / L, the toughness is good, and the stability is good: after soaking for 90 days under the conditions of 130°C and a mineralization of 214812.46mg / L, the deformation recovery rate after 5 extrusions is 60% to 87%, the dehydration rate is 15% to 30%, and the volume shrinkage rate is 29% to 45%, which can maintain its own stability under the conditions of 130°C and a mineralization of 214812.46mg / L to ensure a good, long-term and stable plugging effect. The elastic jelly particles prepared by the present invention have low density, good suspension in high-mineralization formation water, and are easy to carry and inject into deep formations. The preparation method provided by the present invention can prepare elastic jelly particles of different particle sizes according to needs under room temperature conditions, has a simple process, and is easy to store, transport and apply on site. DETAILED DESCRIPTION

[0037] The present invention will be further described below in conjunction with examples, but the examples of the present invention are only exemplary descriptions, and the implementation methods do not constitute limitations of the present invention under any circumstances.

[0038] The sulfonated phenolic resins used in Examples 1 to 6, Comparative Example 1, and Comparative Example 3 are all sulfonated phenolic resins SMP-I, with a solid content of ≧90% and a sulfur content of 8wt% to 10wt%;

[0039] The polyvinyl alcohol used in Examples 1 to 6 and Comparative Examples 1 to 3 is polyvinyl alcohol 2488, with a molecular weight of 117,000.

[0040] Example 1

[0041] 1) Weigh 40 g of sodium bentonite and 846 g of water, mix them, and stir them at a speed of 500 rpm for 2 h to evenly disperse the sodium bentonite in the water to obtain a first dispersion;

[0042] 2) mixing the first dispersion with 4 g of glyoxal and 20 g of sulfonated phenolic resin SMP-Ⅰ, and stirring at a speed of 500 rpm for 30 min to fully dissolve the glyoxal and sulfonated phenolic resin SMP-Ⅰ to obtain a second dispersion;

[0043] 3) 80 g of polyvinyl alcohol 2488 was mixed with the second dispersion, and stirred at 500 rpm for 2 h to fully dissolve the polyvinyl alcohol 2488 to obtain a third dispersion;

[0044] 4) Add 10 g of p-toluenesulfonic acid to the third dispersion, stir at a speed of 300 rpm for 5 min, and prepare a gel solution after the p-toluenesulfonic acid is fully dissolved. The solution is allowed to stand at room temperature for 6 h to obtain a gel. The gel strength is determined to reach Grade I by visual code evaluation method. The obtained gel is ground and granulated by a granulator. During the granulation process, 2262.5 g of a 1 wt% NaOH aqueous solution is evenly sprayed on the surface of the elastic gel particles to adjust the pH of the surface of the elastic gel particles to neutral, thereby obtaining elastic gel particles with a particle size of 10 to 300000 nm.

[0045] Example 2

[0046] 1) Weigh 40 g of sodium bentonite and 825 g of water, mix them, and stir them at a speed of 500 rpm for 2 h to evenly disperse the sodium bentonite in the water to obtain a first dispersion;

[0047] 2) mixing the first dispersion with 5 g of glyoxal and 20 g of sulfonated phenolic resin SMP-Ⅰ, and stirring at 500 rpm for 30 min to fully dissolve glyoxal and sulfonated phenolic resin SMP-Ⅰ to obtain a second dispersion;

[0048] 3) 100 g of polyvinyl alcohol 2488 was mixed with the second dispersion, and stirred at 500 rpm for 2 h to fully dissolve the polyvinyl alcohol 2488 to obtain a third dispersion;

[0049] 4) Add 10 g of p-toluenesulfonic acid to the third dispersion, stir at a speed of 300 rpm for 5 min, and prepare a gel solution after the p-toluenesulfonic acid is fully dissolved. The solution is allowed to stand at room temperature for 6 h to obtain a gel. The gel strength is determined to reach Grade I by visual code evaluation method. The obtained gel is ground and granulated by a granulator. During the granulation process, 2262.5 g of a 1 wt% NaOH aqueous solution is evenly sprayed on the surface of the elastic gel particles to adjust the pH of the surface of the elastic gel particles to neutral, thereby obtaining elastic gel particles with a particle size of 10 to 300000 nm.

[0050] Example 3

[0051] 1) Weigh 40 g of sodium bentonite and 887 g of water, mix them, and stir them at a speed of 500 rpm for 2 h to evenly disperse the sodium bentonite in the water to obtain a first dispersion;

[0052] 2) mixing the first dispersion with 3 g of glyoxal and 20 g of sulfonated phenolic resin SMP-Ⅰ, and stirring at a speed of 500 rpm for 30 min to fully dissolve the glyoxal and sulfonated phenolic resin SMP-Ⅰ to obtain a second dispersion;

[0053] 3) 40 g of polyvinyl alcohol 2488 was mixed with the second dispersion, and stirred at 500 rpm for 2 h to fully dissolve the polyvinyl alcohol 2488 to obtain a third dispersion;

[0054] 4) Add 10 g of p-toluenesulfonic acid to the third dispersion, stir at a speed of 300 rpm for 5 min, and prepare a gel solution after the p-toluenesulfonic acid is fully dissolved. The solution is allowed to stand at room temperature for 6.5 h to obtain a gel. The gel strength is judged to reach Grade I by visual code evaluation method. The obtained gel is ground and granulated by a granulator. During the granulation process, 2262.5 g of a 1 wt% NaOH aqueous solution is evenly sprayed on the surface of the elastic gel particles to adjust the pH of the surface of the elastic gel particles to neutral, thereby obtaining elastic gel particles with a particle size of 10 to 300000 nm.

[0055] Example 4

[0056] 1) Weigh 20 g of sodium bentonite and 866 g of water, mix them, and stir them at a speed of 500 rpm for 2 h to evenly disperse the sodium bentonite in the water to obtain a first dispersion;

[0057] 2) mixing the first dispersion with 4 g of glyoxal and 20 g of sulfonated phenolic resin SMP-Ⅰ, and stirring at a speed of 500 rpm for 30 min to fully dissolve the glyoxal and sulfonated phenolic resin SMP-Ⅰ to obtain a second dispersion;

[0058] 3) 80 g of polyvinyl alcohol 2488 was mixed with the second dispersion, and stirred at 500 rpm for 2 h to fully dissolve the polyvinyl alcohol 2488 to obtain a third dispersion;

[0059] 4) Add 10 g of p-toluenesulfonic acid to the third dispersion, stir at a speed of 300 rpm for 5 min, and prepare a gel solution after the p-toluenesulfonic acid is fully dissolved. The solution is allowed to stand at room temperature for 5 h to obtain a gel. The gel strength is judged to reach Grade I by visual code evaluation method. The obtained gel is ground and granulated by a granulator. During the granulation process, 2262.5 g of a 1 wt% NaOH aqueous solution is evenly sprayed on the surface of the elastic gel particles to adjust the pH of the surface of the elastic gel particles to neutral, thereby obtaining elastic gel particles with a particle size of 10 to 300000 nm.

[0060] Example 5

[0061] 1) Weigh 40 g of sodium bentonite and 846 g of water, mix them, and stir them at a speed of 500 rpm for 2 h to evenly disperse the sodium bentonite in the water to obtain a first dispersion;

[0062] 2) mixing the first dispersion with 4 g of glyoxal and 20 g of sulfonated phenolic resin SMP-Ⅰ, and stirring at a speed of 500 rpm for 30 min to fully dissolve the glyoxal and sulfonated phenolic resin SMP-Ⅰ to obtain a second dispersion;

[0063] 3) 80 g of polyvinyl alcohol 2488 was mixed with the second dispersion, and stirred at 500 rpm for 2 h to fully dissolve the polyvinyl alcohol 2488 to obtain a third dispersion;

[0064] 4) 10 g of chloroacetic acid was added to the third dispersion, and the mixture was stirred at a speed of 300 rpm for 5 min. After the p-toluenesulfonic acid was fully dissolved, a gel solution was obtained. The mixture was allowed to stand at room temperature for 8 h to obtain a gel. The gel strength was determined to reach Grade I by visual code evaluation method. The obtained gel was ground and granulated by a granulator. During the granulation process, 2262.5 g of a 1 wt% NaOH aqueous solution was evenly sprayed on the surface of the elastic gel particles to adjust the pH value of the elastic gel particles to neutral, thereby obtaining elastic gel particles with a particle size of 10 to 300000 nm.

[0065] Example 6

[0066] 1) Weigh 40 g of sodium bentonite and 856 g of water, mix them, and stir them at a speed of 500 rpm for 2 h to evenly disperse the sodium bentonite in the water to obtain a first dispersion;

[0067] 2) mixing the first dispersion with 4 g of glyoxal and 10 g of sulfonated phenolic resin SMP-Ⅰ, and stirring at 500 rpm for 30 min to fully dissolve glyoxal and sulfonated phenolic resin SMP-Ⅰ to obtain a second dispersion;

[0068] 3) 80 g of polyvinyl alcohol 2488 was mixed with the second dispersion, and stirred at 500 rpm for 2 h to fully dissolve the polyvinyl alcohol 2488 to obtain a third dispersion;

[0069] 4) Add 10 g of p-toluenesulfonic acid to the third dispersion, stir at a speed of 300 rpm for 5 min, and prepare a gel solution after the p-toluenesulfonic acid is fully dissolved. The solution is allowed to stand at room temperature for 4 h to obtain a gel. The gel strength is determined to reach Grade I by visual code evaluation method. The obtained gel is ground and granulated by a granulator. During the granulation process, 2262.5 g of a 1 wt% NaOH aqueous solution is evenly sprayed on the surface of the elastic gel particles to adjust the pH of the surface of the elastic gel particles to neutral, thereby obtaining elastic gel particles with a particle size of 10 to 300000 nm.

[0070] Comparative Example 1

[0071] 1) Weigh 4 g of glyoxal, 20 g of sulfonated phenolic resin SMP-Ⅰ and 886 g of water, and stir at a speed of 500 rpm for 30 min to fully dissolve glyoxal and sulfonated phenolic resin SMP-Ⅰ to obtain a first dispersion;

[0072] 2) 80 g of polyvinyl alcohol 2488 was mixed with the first dispersion, and stirred at 500 rpm for 2 h to fully dissolve the polyvinyl alcohol 2488 to obtain a second dispersion;

[0073] 3) adding 10 g of p-toluenesulfonic acid to the second dispersion, stirring at a speed of 300 rpm for 5 min, preparing a gel solution after the p-toluenesulfonic acid is fully dissolved, and standing at room temperature for 4.5 h to obtain a gel. The gel strength is judged to reach Grade I by visual code evaluation method. The obtained gel is ground and granulated by a granulator. During the granulation process, 2262.5 g of a 1 wt% NaOH aqueous solution is evenly sprayed on the surface of the elastic gel particles to adjust the pH of the surface of the elastic gel particles to neutral, thereby obtaining elastic gel particles with a particle size of 10 to 300000 nm.

[0074] Comparative Example 2

[0075] 1) Weigh 40 g of sodium bentonite and 866 g of water, mix them, and stir them at a speed of 500 rpm for 2 h to evenly disperse the sodium bentonite in the water to obtain a first dispersion;

[0076] 2) mixing the first dispersion and 4 g of glyoxal, and stirring at 500 rpm for 30 min to fully dissolve the glyoxal to obtain a second dispersion;

[0077] 3) 80 g of polyvinyl alcohol 2488 was mixed with the second dispersion, and stirred at 500 rpm for 2 h to fully dissolve the polyvinyl alcohol 2488 to obtain a third dispersion;

[0078] 4) Add 10 g of p-toluenesulfonic acid to the third dispersion, stir at a speed of 300 rpm for 5 min, and prepare a gel solution after the p-toluenesulfonic acid is fully dissolved. The solution is allowed to stand at room temperature for 3 h to obtain a gel. The gel strength is determined to reach Grade I by visual code evaluation method. The obtained gel is ground and granulated by a granulator. During the granulation process, 2262.5 g of a 1 wt% NaOH aqueous solution is evenly sprayed on the surface of the elastic gel particles to adjust the pH of the surface of the elastic gel particles to neutral, thereby obtaining elastic gel particles with a particle size of 10 to 300000 nm.

[0079] Comparative Example 3

[0080] 1) Weigh 40 g of sodium bentonite and 846 g of water, mix them, and stir them at a speed of 500 rpm for 2 h to evenly disperse the sodium bentonite in the water to obtain a first dispersion;

[0081] 2) mixing the first dispersion with 4 g of glyoxal and 20 g of sulfonated phenolic resin SMP-Ⅰ, and stirring at a speed of 500 rpm for 30 min to fully dissolve the glyoxal and sulfonated phenolic resin SMP-Ⅰ to obtain a second dispersion;

[0082] 3) 80 g of polyvinyl alcohol 2488 was mixed with the second dispersion, and stirred at 500 rpm for 2 h to fully dissolve the polyvinyl alcohol 2488 to obtain a third dispersion;

[0083] 4) Add 10 g of p-toluenesulfonic acid to the third dispersion and stir at 300 rpm for 5 min. After the p-toluenesulfonic acid is fully dissolved, a gel solution is obtained. The solution is allowed to stand at room temperature for 6 h to obtain a gel. The gel strength is determined to reach Grade I by visual code evaluation. The obtained gel is ground and pulverized by a granulator to obtain elastic gel particles with a particle size of 10 to 300,000 nm.

[0084] Performance evaluation of elastic jelly particles

[0085] For the convenience of the experiment and the accuracy of the experimental results, the gelling time, storage modulus, room temperature toughness, toughness after 90 days of high temperature and high salt immersion, dehydration rate after 30 days of high temperature and high salt immersion, volume shrinkage rate after 30 days of high temperature and high salt immersion, dehydration rate after 90 days of high temperature and high salt immersion, and volume shrinkage rate after 90 days of high temperature and high salt immersion of the elastic jelly particles prepared in Examples 1 to 6 and Comparative Examples 1 to 3 were directly measured to evaluate the performance of the jelly. Further, since the elastic jelly particles are obtained by physical granulation of the jelly, the performance of the jelly can represent the performance of the elastic jelly particles. It should be noted that the high temperature and high salt environment (specifically 130°C, saline with a mineralization of 214812.46 mg / L) refers to the conditions for experimental treatment of the jelly, and the determination of each experimental data is carried out at room temperature (25°C); before the experiment begins, it is necessary to evenly spray a 1wt% NaOH aqueous solution on the surface of the jelly to be tested to adjust the pH to neutral.

[0086] Among them, in the test of measuring the toughness of elastic jelly particles after 90 days of high temperature and high salt immersion, the dehydration rate after 30 days of high temperature and high salt immersion, the volume shrinkage rate after 30 days of high temperature and high salt immersion, the dehydration rate after 90 days of high temperature and high salt immersion, and the volume shrinkage rate after 90 days of high temperature and high salt immersion, the preparation method of 1L salt water with a mineralization of 214812.46 mg / L is as follows:

[0087] i. Take 500 mL of distilled water, weigh CaCl2, MgCl2·6H2O, Na2SO4, NaHCO3, KI, KBr and NaCl according to the amounts of various salts listed in Table 1, add them into the distilled water, and stir them thoroughly to dissolve to obtain the salt solution to be diluted;

[0088] Table 1. The amount of various salts required to prepare 1L of brine

[0089]

[0090]

[0091] ii. Transfer the salt solution to be diluted obtained in ii to a 1 L volumetric flask, add distilled water to make the volume to 1 L, and obtain 1 L of salt water with a mineralization of 214812.46 mg / L. The specific components are shown in Table 2.

[0092] Table 2. Components of brine with a mineralization of 214812.46 mg / L

[0093] project Content mg / L <![CDATA[Ca 2+ ]]> 11598.6 <![CDATA[Mg 2+ ]]> 1224.5 <![CDATA[K + +That + ]]> 69831.7 <![CDATA[Cl - ]]> 131489.2 <![CDATA[SO4 2- ]]> 264.3 <![CDATA[I - ]]> 7.43 <![CDATA[Br - ]]> 251.43 <![CDATA[HCO3 - ]]> 145.3 Total mineralization 214812.46 Water Type <![CDATA[CaCl2]]>

[0094] The specific determination method is as follows:

[0095] (1) Determination of gelling time for preparing elastic jelly particles

[0096] First, a 1 wt% NaOH aqueous solution was uniformly sprayed on the surface of the gel prepared in Examples 1 to 6 and Comparative Examples 1 to 3 to adjust the pH to neutral, and then the visual code evaluation method of Sydansk et al., which divides the gel strength of the plugging agent (Gel Strength Codes for short GSC) into 10 levels according to the visual results, was used to judge the time when the gel strength of the gel prepared in Examples 1 to 6 and Comparative Examples 1 to 3 reached level I in combination with Table 3, which is the gelation time. The specific results are shown in Table 4.

[0097] Table 3. Gel Strength Code Standards

[0098]

[0099]

[0100] (2) Preparation of elastic jelly particles and determination of jelly storage modulus

[0101] First, a 1 wt% NaOH aqueous solution was uniformly sprayed on the surface of the jelly prepared in Examples 1 to 6 and Comparative Examples 1 to 3 to adjust the pH to neutral, and then the storage modulus of the jelly was measured at room temperature (25°C) and normal pressure (0.1 MPa) using a MARSⅢ high temperature and high pressure acid-resistant rheometer and referring to the standard SY-T6296-2013 "Rheological parameter method for determination of jelly strength for oil production". The specific results are shown in Table 4.

[0102] Table 4. Gel gelling time and gel storage modulus for preparing elastic gel particles

[0103] Serial number Gel gelling time / h Gel storage modulus / Pa Example 1 6 1275 Example 2 6 1953 Example 3 6.5 859 Example 4 5 780 Example 5 8 1112 Example 6 4 1320 Comparative Example 1 4.5 600 Comparative Example 2 3 1413 Comparative Example 3 6 1250

[0104] As shown in Table 4, the gelling time of the elastic jelly particles prepared in Examples 1 to 6 is 4 to 8 hours, and the storage modulus is 780 to 1953 Pa; the storage modulus of the elastic jelly particles prepared in Comparative Example 1 is only 600 Pa; the gelling time of the elastic jelly particles prepared in Comparative Example 2 is 3 hours; from the formula, compared with Example 1, Comparative Example 1 lacks sodium bentonite; compared with Example 1, Comparative Example 2 lacks sulfonated phenolic resin. This indicates that the lack of raw material types will affect the elastic modulus of the jelly, resulting in the problem that the elastic modulus is too low and easy to break, thus affecting the plugging strength.

[0105] (3) Determination of the toughness of the jelly prepared from elastic jelly particles at room temperature (i.e., 25°C) (i.e., the deformation recovery rate η1 of the jelly after 5 extrusions at room temperature)

[0106] First, the surface of the jelly prepared in Examples 1 to 6 and Comparative Examples 1 to 3 was uniformly sprayed with a 1 wt % NaOH aqueous solution to adjust the pH to neutral, and then cut into cylindrical jelly blocks with a diameter of 2 cm and a height of 3 cm, respectively, and the initial height of the cylindrical jelly block was recorded as L0; a HY-01 microcomputer electronic compression tester was used to compress downward at a speed of 12.5 mm / min until the height of the cylindrical jelly block became 1 cm, and then the pressure was released until the jelly block could no longer be deformed, and then it was compressed again and then recovered. After repeating 5 times, the height recovered after deformation was measured and recorded as L1.

[0107] pass The deformation recovery rate η1 after 5 extrusions at room temperature was calculated by (Formula I). ​​The specific results are shown in Table 5.

[0108] (4) Preparation of elastic jelly particles: toughness of jelly after high temperature and high salt immersion for 90 days (i.e., the deformation recovery rate η2 of jelly after 5 extrusions at room temperature (i.e., 25°C) after immersion in salt water at 130°C and a mineralization degree of 214812.46 mg / L for 90 days)

[0109] First, the surface of the jelly prepared in Examples 1 to 6 and Comparative Examples 1 to 3 was uniformly sprayed with a 1 wt % NaOH aqueous solution to adjust the pH to neutral, and then the jelly blocks were respectively placed in beakers containing salt water with a mineralization degree of 214812.46 mg / L, so that the jelly blocks were completely immersed in the salt water; after the beakers were placed in a constant temperature oven at 130° C. for 90 days, the soaked jelly blocks were taken out from each beaker, cut into cylindrical jelly blocks with a diameter of 2 cm and a height of 3 cm, and the initial height of the cylindrical jelly block was recorded as L0; a HY-01 microcomputer electronic compression tester was used to compress downward at a speed of 12.5 mm / min until the height of the cylindrical jelly block became 1 cm, and the pressure was released until the jelly block was deformed and no longer recovered, and then compressed again and recovered, and after repeating 5 times, the height recovered after deformation was measured and recorded as L2.

[0110] pass (Formula II) calculated the deformation recovery rate η1 after immersion for 90 days and 5 extrusions at room temperature. The specific results are shown in Table 5.

[0111] Table 5. Toughness of the prepared elastic jelly particles after immersion in room temperature and high temperature and high salt environment

[0112]

[0113] The data in Table 5 show that the elastic jelly particles prepared in Examples 1 to 6 have a deformation recovery rate of 85% to 96.5% after 5 extrusions at room temperature; and a deformation recovery rate of 60% to 87% after immersion at 130°C and a salinity of 214812.46 mg / L for 90 days after 5 extrusions, indicating that the elastic jelly particles prepared in Examples 1 to 6 have good toughness at room temperature or after immersion in a saline solution at 130°C and a salinity of 214812.46 mg / L. The elastic jelly particles prepared in Comparative Example 1 were broken at room temperature and after immersion in a saline solution at 130°C and a salinity of 214812.46 mg / L, and had poor toughness; the elastic jelly particles prepared in Comparative Example 2 had a deformation recovery rate of only 30% after 5 extrusions at room temperature (i.e., 25°C) after immersion in a saline solution at 130°C and a salinity of 214812.46 mg / L for 90 days, and had poor toughness.

[0114] (5) Dehydration rate and volume shrinkage rate of the prepared elastic jelly particles after immersion in high temperature and high salt for 30 days

[0115] First, the jelly surfaces prepared in Examples 1 to 6 and Comparative Examples 1 to 3 were uniformly sprayed with a 1 wt% NaOH aqueous solution to adjust the pH to neutral. Then, the jelly blocks were cut into cubes with an edge length of 5 cm, and their initial mass was recorded as m0 and initial volume V0 (i.e., 125 cm 3); put the gel blocks into beakers filled with saline solution with a mineralization degree of 214812.46 mg / L, so that the gel blocks are completely immersed in the saline solution; after placing the beakers in a constant temperature oven at 130°C for 30 days, take out the soaked gel blocks from each beaker, rinse the soaked gel blocks with deionized water for 3 times, wipe the surface water of the rinsed gel blocks with absorbent paper and cool them to room temperature (i.e., 25°C), then weigh and measure their volume, and record the mass m1 and volume V1 of the gel blocks after dehydration.

[0116] pass (Formula III) The dehydration rate η3 after immersion for 30 days was calculated;

[0117] pass The volume shrinkage rate η4 after immersion for 30 days was calculated by (Formula IV). The specific results are shown in Table 6.

[0118] (6) Dehydration rate and volume shrinkage rate of the prepared elastic jelly particles after 90-day immersion in high-temperature and high-salt jelly

[0119] First, the jelly surfaces prepared in Examples 1 to 6 and Comparative Examples 1 to 3 were uniformly sprayed with a 1 wt% NaOH aqueous solution to adjust the pH to neutral. Then, the jelly blocks were cut into cubes with an edge length of 5 cm, and their initial mass was recorded as m0 and initial volume V0 (i.e., 125 cm 3 ); put the gel blocks into beakers filled with saline solution with a mineralization degree of 214812.46 mg / L, so that the gel blocks are completely immersed in the saline solution; after placing the beakers in a constant temperature oven at 130°C for 90 days, take out the soaked gel blocks from each beaker, rinse the soaked gel blocks with deionized water for 3 times, wipe the surface water of the rinsed gel blocks with absorbent paper and cool them to room temperature (i.e. 25°C), then weigh and measure their volume, and record the mass m2 and volume V2 of the gel blocks after water loss.

[0120] pass (Formula V) The dehydration rate η5 after 90 days of immersion is calculated;

[0121] pass The volume shrinkage rate η6 after 90 days of immersion was calculated by (Formula VI). The specific results are shown in Table 6.

[0122] Table 6. Dehydration rate and volume shrinkage rate of the jelly particles prepared after high temperature and high salt immersion for 30 days and 90 days

[0123]

[0124] The data in Table 6 show that the jelly blocks of elastic jelly particles prepared in Examples 1 to 6 have a dehydration rate of 10% to 24.5% and a volume shrinkage rate of 20% to 33% after immersion in brine at 130°C and 214812.46 mg / L for 30 days; and a dehydration rate of 15% to 30% and a volume shrinkage rate of 29% to 45% after immersion for 90 days. This proves that the jelly blocks of elastic jelly particles prepared in Examples 1 to 6 can maintain their stability for a long time at high temperature and high mineralization at 130°C and 214812.46 mg / L, ensuring a good and stable plugging effect in a high temperature and high salt environment. The jelly blocks of elastic jelly particles prepared in Comparative Examples 1 and 2 were immersed in 130°C, 214812.46 mg / L brine: after immersion for 30 days, the dehydration rate was 36% to 45%, and the volume shrinkage rate was 42.5% to 50%; after immersion for 90 days, the dehydration rate was 55% to 60%, and the volume shrinkage rate was 60% to 65%. The stability was poor under high temperature and high mineralization. The dehydration rate and volume shrinkage rate of the jelly blocks of elastic jelly particles prepared by immersion for 30 days and 90 days were higher than those of the jelly blocks of elastic jelly particles prepared in Examples 1 to 6. The stability of the jelly blocks of elastic jelly particles prepared in Comparative Example 3 at a high temperature and high mineralization of 130°C and 214812.46 mg / L is slightly better than that of Comparative Example 1 and Comparative Example 2, but its dehydration rate and volume shrinkage rate after 90 days of immersion are 35% and 50%, respectively, which are higher than those of the jelly blocks of elastic jelly particles prepared in Examples 1 to 6. Therefore, the stability of the jelly blocks of elastic jelly particles prepared in Comparative Example 3 at a high temperature and high mineralization of 130°C and 214812.46 mg / L is inferior to that of the jelly blocks of elastic jelly particles prepared in Examples 1 to 6.

[0125] Although the present invention has been described with reference to specific embodiments, it will be appreciated by those skilled in the art that various changes may be made without departing from the true spirit and scope of the present invention. In addition, the subject matter, spirit and scope of the present invention may be varied to accommodate specific situations, materials, material combinations and methods. All of these changes are included within the scope of the claims of the present invention.

Claims

1. A method for preparing elastic jelly particles, comprising the following steps: 1) mixing silicate and water to obtain a first dispersion; 2) mixing the crosslinking agent, the sulfonated phenolic resin and the first dispersion to obtain a second dispersion; 3) mixing polyvinyl alcohol and the second dispersion to obtain a third dispersion; 4) mixing the acid catalyst and the third dispersion, reacting to obtain jelly, and granulating to obtain the elastic jelly particles.

2. The method according to claim 1, characterized in that Taking the mass of the elastic jelly particles as 100%, the amount of the silicate is 2wt% to 6wt%, the amount of the cross-linking agent is 0.3wt% to 0.7wt%, the amount of the sulfonated phenol-formaldehyde resin is 1wt% to 3wt%, the amount of the polyvinyl alcohol is 4wt% to 10wt%, the amount of the acid catalyst is 0.5wt% to 1.5wt%, and the amount of water is 78.8wt% to 92.2wt%.

3. The method according to claim 1 or 2, characterized in that: The silicate is sodium bentonite; and / or The cross-linking agent is selected from aldehyde cross-linking agents and / or hexamethylenetetramine; and / or The acid catalyst is an inorganic acid and / or an organic acid; and / or The mineralization of the water is less than 1000 mg / L; Preferably, the aldehyde cross-linking agent is selected from at least one of formaldehyde, paraformaldehyde, glyoxal, glutaraldehyde and terephthalaldehyde; and / or The organic acid comprises halogenated acetic acid and / or alkylbenzene sulfonic acid; Preferably, the inorganic acid is hydrochloric acid and / or sulfuric acid; and / or the halogenated acetic acid is chloroacetic acid; and / or the alkylbenzenesulfonic acid is p-toluenesulfonic acid.

4. The method according to any one of claims 1 to 3, characterized in that The sulfonated phenolic resin has a sulfur content of 8wt% to 10wt%; and / or a solid content of not less than 90wt%; and / or The polyvinyl alcohol has a degree of alcoholysis of 87% to 89% and / or a molecular weight of 100,000 to 1,200,000.

5. The method according to any one of claims 1 to 4, characterized in that In step 4), the reaction is carried out at 22° C. to 25° C. for 4 to 8 hours.

6. The method according to any one of claims 1 to 5, characterized in that In step 4), the strength of the jelly reaches Grade I according to the visual code evaluation method; and / or During the granulation process, spraying an alkali solution onto the surface of the elastic jelly particles to adjust the pH value on the surface of the elastic jelly particles to neutral; Preferably, the alkali solution is selected from at least one of sodium hydroxide solution, sodium carbonate solution, triethanolamine and sodium bicarbonate solution.

7. Elastic jelly particles prepared by the method according to any one of claims 1 to 6.

8. The elastic jelly particles according to claim 7, characterized in that: The particle size of the elastic jelly particles is 1×10 1 nm to 3×10 6 nm.

9. Use of the elastic jelly particles prepared according to any one of claims 1 to 6 or the elastic jelly particles according to claim 7 or 8 in high-temperature and high-salinity fracture-cavern oil reservoirs, especially in flow channel adjustment in high-temperature and high-salinity fracture-cavern oil reservoirs.

10. The use according to claim 9, characterized in that: The high temperature is not less than 130°C; and / or The high salt has a mineralization of not less than 210000 mg / L.

Citation Information

Patent Citations

  • Frozen-soil hydrate deposit polyvinyl alcohol type drilling fluid

    CN108359431A

  • Slow-crosslinking temperature-resistant salt type high-strength gel, and preparation method and application thereof

    CN111808585A

  • Preparation method of cross-linking agent for oil field, cross-linking agent for oil field, blocking agent and preparation method and application of blocking agent

    CN115725033A

  • High-strength particle temporary plugging agent for fracturing diverting as well as preparation method and application of high-strength particle temporary plugging agent

    CN115838589A

  • Organically crosslinked polyvinyl alcohol copolymeric gels for use under harsh reservoir conditions

    US4940090A