Preparation method of silicone structural sealant

Through the combination of modified hollow glass beads, fumed silica and aluminosilicate, as well as hexamethyldisilazane and modified nano-calcium carbonate, the heat resistance and waterproof performance of the sealant in high temperature environments are solved. This problem is eliminated and a more stable sealing effect is achieved.

CN118772833AInactive Publication Date: 2024-10-15GUANGZHOU BAORUI NEW MATERIALS CO LTD

Patent Information

Application Number
CN202410914141.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing sealants have insufficient heat resistance in high-temperature environments and poor waterproof performance, leading to sealing failure and water seepage problems.

Method used

Modified hollow glass beads, fumed silica and aluminosilicate are used as fillers, and hexamethyldisilazane and modified nano-calcium carbonate are added, and silicone is prepared through temperature-controlled kneading and vacuum stirring. Structural sealants.

Benefits of technology

Significantly improves the heat resistance and waterproof performance of the sealant, ensuring that the sealant maintains stable performance in high temperature environments and prevents water seepage and mold corrosion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004934588880000101
    Figure BDA0004934588880000101
Patent Text Reader

Abstract

The invention relates to a preparation method of a silicone structural sealant, and belongs to the technical field of sealants, the preparation method comprises the following steps: S1, pretreatment A; pretreatment B; s3, preparing base rubber; and S4, preparing a sealant finished product. According to the invention, the modified hollow glass beads, fumed silica and aluminosilicate are compounded as a sealant filler, so that the prepared sealant has excellent heat resistance through synergism; on the basis, hexamethyldisilazane is added, so that the thermal rearrangement degradation reaction of a main chain of a system at a high temperature is effectively inhibited, the thermal stability of the system is improved, and the heat resistance of a finished product of the sealant is further enhanced; besides, hexadecyl phosphate and lauric acid are further added to modify the nano calcium carbonate, the hydrophobic capacity of the nano calcium carbonate is effectively improved, and the modified nano calcium carbonate is applied to preparation of the sealant, so that the waterproof performance of a finished product of the sealant can be greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of sealants, and in particular, relates to a method for preparing a silicone structural sealant. Background Art

[0002] As a high-performance sealing material, silicone structural sealant has been widely used in the field of modern construction due to its unique chemical structure and physical properties. With the rapid development of modern construction technology, the requirements for building materials and sealing materials are also increasing. Especially in high temperature and high humidity environments, traditional sealing materials are often difficult to meet long-term stable performance requirements. Taking most of the current commercially available sealants as an example, in high temperature environments, they are prone to lose their original mechanical properties and adhesion due to their lack of heat resistance, resulting in sealing failure; and many commercially available sealants also have the problem of poor waterproofness, which cannot effectively prevent moisture or other liquids from entering the sealing area, and easily cause the adhered materials to encounter water seepage, which in turn causes mold or corrosion problems. Therefore, in order to solve these problems, it is of great practical significance to develop a silicone structural sealant with better heat resistance and waterproofness. Summary of the invention

[0003] The purpose of the present invention is to provide a method for preparing a silicone structural sealant, which solves the problem of poor heat resistance and waterproof performance in the existing sealant technology.

[0004] The purpose of the present invention can be achieved through the following technical solutions:

[0005] A method for preparing a silicone structural sealant, the preparation method specifically comprising the following steps:

[0006] S1, pretreatment A: pretreating the hollow glass microspheres to obtain pretreated hollow glass microspheres;

[0007] S2, pretreatment B: pretreating the nano calcium carbonate to obtain pretreated nano calcium carbonate;

[0008] S3, preparing a base glue: kneading α, ω-dihydroxy polydimethylsiloxane, polydimethylsiloxane, pretreated hollow glass microspheres, fumed silica and aluminosilicate uniformly at room temperature, adding pretreated nano-calcium carbonate, kneading and stirring under controlled temperature, and dehydrating and drying under controlled temperature to obtain a base glue;

[0009] S4. Prepare the finished sealant product: stir the base glue, hexamethyldisilazane and the cross-linking agent evenly, then add the catalyst and stir in vacuum to remove bubbles to obtain the finished sealant product.

[0010] As a preferred technical solution of the present invention, step S1 is specifically:

[0011] The hollow glass microspheres and the sodium hydroxide solution are mixed evenly and stirred under controlled temperature, washed once, filtered, and the hollow glass microspheres are dried under controlled temperature to obtain dried hollow glass microspheres. The dried hollow glass microspheres and ethyl acetate are ultrasonically dispersed, dodecyltrimethoxysilane is added, mixed evenly, and heated to reflux under controlled temperature. After the reflux is completed, the product is washed twice, filtered, and dried under controlled temperature in a vacuum to obtain pretreated hollow glass microspheres.

[0012] Furthermore, the usage ratio of the hollow glass microspheres to the sodium hydroxide solution is 1-1.2 g:30-35 mL; the usage ratio of the dried hollow glass microspheres, ethyl acetate and dodecyltrimethoxysilane is 1-1.3 g:100-135 mL:0.15-0.2 g.

[0013] Furthermore, the concentration of the sodium hydroxide solution is 0.2 mol / L; the temperature of the temperature-controlled stirring is 75-80°C, and the time is 1.5-2h; the primary washing is washing with deionized water until the solution pH is 7; the temperature of the temperature-controlled drying is 95-100°C, and the time is 10-12h; the time of the ultrasonic dispersion is 30-35min; the temperature of the temperature-controlled heating reflux is 75-80°C, and the time is 3-3.5h; the secondary washing is washing with ethyl acetate for 3-5 times; the temperature of the temperature-controlled vacuum drying is 50-55°C, and the time is 48-54h.

[0014] As a preferred technical solution of the present invention, step S2 is specifically:

[0015] Nano calcium carbonate and deionized water are mixed evenly to obtain mixture A; hexadecyl phosphate and anhydrous ethanol are mixed evenly to obtain mixture B; lauric acid and anhydrous ethanol are mixed evenly to obtain mixture C; mixture A and mixture B are mixed evenly and stirred under controlled temperature, after stirring, mixture C is added and stirred under controlled temperature, cooled, filtered, washed, filtered, and dried under controlled temperature to obtain pretreated nano calcium carbonate.

[0016] Furthermore, the dosage ratio of the nano-calcium carbonate and deionized water is 1-1.2g:12.5-15mL; the mass ratio of the hexadecyl phosphate and anhydrous ethanol is 0.04-0.05:10-12; the molar ratio of the lauric acid and anhydrous ethanol is 1:8-8.5; the mass ratio of the mixture A, the mixture B and the mixture C is 1:0.03-0.04:0.04-0.05.

[0017] Furthermore, the temperature of the temperature-controlled stirring is 70-75°C, and the time is 1-1.5h; the cooling is cooling to 23-25°C; the washing is washing with anhydrous ethanol and then with deionized water for 2-3 times respectively; the temperature of the temperature-controlled drying is 100-110°C.

[0018] As a preferred technical solution of the present invention, the mass ratio of α,ω-dihydroxypolydimethylsiloxane, polydimethylsiloxane, pretreated hollow glass microspheres, fumed silica, aluminosilicate and pretreated nano-calcium carbonate in step S3 is 100-110:5-10:8-10:3-5:7-11:20-30.

[0019] As a preferred technical solution of the present invention, the viscosity of the α,ω-dihydroxypolydimethylsiloxane in step S3 is 20-25 Pa·s; the viscosity of the polydimethylsiloxane is 0.5 Pa·s.

[0020] As a preferred technical solution of the present invention, the method of adding pretreated nano-calcium carbonate in step S3 is to evenly add the pretreated nano-calcium carbonate in three times; the temperature of the temperature-controlled kneading and stirring is 100-110°C, and the time is 2-3h; the temperature of the temperature-controlled dehydration and drying is 130-140°C, and the time is 3-4h.

[0021] As a preferred technical solution of the present invention, the mass ratio of the base glue, hexamethyldisilazane, cross-linking agent and catalyst in step S4 is 100:0.3-0.35:6-8:1.5-2.

[0022] As a preferred technical solution of the present invention, the cross-linking agent in step S4 is methyltrimethoxysilane; and the catalyst is dibutyltin dilaurate.

[0023] As a preferred technical solution of the present invention, the vacuum stirring time in step S4 is 15-20 minutes.

[0024] Beneficial effects of the present invention:

[0025] (1) The present invention uses modified hollow glass microspheres, fumed silica and aluminosilicate as sealant fillers, which solves the problem of insufficient heat resistance when the fillers are used alone, and synergistically makes the prepared sealant have excellent heat resistance. Specifically, it is because the hollow glass microspheres themselves are inorganic rigid materials with high decomposition temperature and outstanding heat resistance. Secondly, the hollow glass microspheres are modified by dodecyltrimethoxysilane, which increases the affinity between the hollow glass microspheres and the matrix, so that they are evenly dispersed in the matrix and effectively exert their own performance; the fumed silica itself has excellent weather resistance and is an ideal reinforcing material. The fumed silica and α, ω-dihydroxy polysiloxane are similar in structure and can form hydrogen bonds between the two, which improves the heat resistance of the system to a certain extent; the aluminosilicate has the characteristics of low thermal conductivity and excellent thermal stability, and can be used as an auxiliary filler to assist the hollow glass microspheres and fumed silica in consolidating the thermal stability of the system, thereby making the finished sealant have better heat resistance.

[0026] (2) The present invention also adds hexamethyldisilazane, which effectively inhibits the main chain degradation of α, ω-dihydroxy polysiloxane that easily occurs under the action of water or silanol at too high a temperature, that is, effectively inhibits the thermal rearrangement degradation reaction of the main chain of the system, improves the thermal stability of the system, and further enhances the heat resistance of the sealant product.

[0027] (3) The present invention adds nano-calcium carbonate and uses hexadecyl phosphate to react with calcium ions on its surface to generate calcium salt, so that the long-chain alkyl groups of the nano-calcium carbonate are arranged outward and are hydrophobic. On this basis, lauric acid is added for modification, which improves the dispersion degree of the nano-calcium carbonate and makes it dispersed evenly. At the same time, the activation degree of the nano-calcium carbonate is increased, the static contact angle is increased, and the hydrophobicity of the nano-calcium carbonate is effectively increased. The nano-calcium carbonate after composite modification by hexadecyl phosphate and lauric acid is applied to the preparation of sealant, which can greatly increase the waterproof performance of the finished sealant. DETAILED DESCRIPTION

[0028] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] Example 1

[0030] A method for preparing a silicone structural sealant, the preparation method specifically comprising the following steps:

[0031] S1, pretreatment A: pretreating the hollow glass microspheres to obtain pretreated hollow glass microspheres;

[0032] S2, pretreatment B: pretreating the nano calcium carbonate to obtain pretreated nano calcium carbonate;

[0033] S3, preparing base glue: knead α, ω-dihydroxy polydimethylsiloxane with a viscosity of 20 Pa·s, polydimethylsiloxane with a viscosity of 0.5 Pa·s, pretreated hollow glass microspheres, fumed silica and aluminosilicate at room temperature, add pretreated nano-calcium carbonate, control the temperature at 100°C, knead and stir for 2 hours, control the temperature at 140°C for dehydration and drying for 3 hours to obtain base glue;

[0034] S4, preparing a finished sealant product: mixing the base glue, hexamethyldisilazane and methyltrimethoxysilane evenly, then adding dibutyltin dilaurate and stirring in vacuum for 15 minutes to remove bubbles, thereby obtaining a finished sealant product;

[0035] The above step S1 is specifically as follows: the hollow glass microspheres and the sodium hydroxide solution with a concentration of 0.2 mol / L are mixed evenly and stirred at 80°C for 1.5 hours, washed with deionized water until the solution pH is 7, filtered, and the hollow glass microspheres are dried at 95°C for 10 hours to obtain dried hollow glass microspheres, the dried hollow glass microspheres and ethyl acetate are ultrasonically dispersed for 30 minutes, dodecyltrimethoxysilane is added, mixed evenly, and heated to 78°C for reflux for 3 hours. After the reflux is completed, the product is washed 5 times with ethyl acetate, filtered, and vacuum dried at 50°C for 48 hours to obtain pretreated hollow glass microspheres;

[0036] The usage ratio of the hollow glass microspheres and the sodium hydroxide solution is 1 g:30 mL; the usage ratio of the dried hollow glass microspheres, ethyl acetate and dodecyltrimethoxysilane is 1 g:118 mL:0.2 g;

[0037] The above step S2 is specifically as follows: mixing nano-calcium carbonate and deionized water evenly to obtain a mixture A; mixing hexadecyl phosphate and anhydrous ethanol evenly to obtain a mixture B; mixing lauric acid and anhydrous ethanol evenly to obtain a mixture C; mixing the mixture A and the mixture B evenly, stirring at 70°C for 1h, adding the mixture C after stirring, stirring at the same temperature, cooling to 25°C, filtering, washing twice with anhydrous ethanol and then with deionized water, filtering, and drying at 100°C to obtain pretreated nano-calcium carbonate;

[0038] The dosage ratio of the nano-calcium carbonate and deionized water is 1 g:12.5 mL; the mass ratio of the hexadecyl phosphate and anhydrous ethanol is 0.045:10; the molar ratio of the lauric acid and anhydrous ethanol is 1:8.3; the mass ratio of the mixture A, the mixture B and the mixture C is 1:0.03:0.045;

[0039] Wherein, the mass ratio of α,ω-dihydroxypolydimethylsiloxane, polydimethylsiloxane, pretreated hollow glass microspheres, fumed silica, aluminosilicate and pretreated nano-calcium carbonate in step S3 is 100:7.5:8:3:9:20;

[0040] The method of adding the pretreated nano-calcium carbonate in step S3 is to add the pretreated nano-calcium carbonate evenly in three times;

[0041] Wherein, the mass ratio of the base glue, hexamethyldisilazane, methyltrimethoxysilane and dibutyltin dilaurate in step S4 is 100:0.3:6:1.5.

[0042] Example 2

[0043] A method for preparing a silicone structural sealant, the preparation method specifically comprising the following steps:

[0044] S1, pretreatment A: pretreating the hollow glass microspheres to obtain pretreated hollow glass microspheres;

[0045] S2, pretreatment B: pretreating the nano calcium carbonate to obtain pretreated nano calcium carbonate;

[0046] S3, preparing base glue: knead α, ω-dihydroxy polydimethylsiloxane with a viscosity of 20 Pa·s, polydimethylsiloxane with a viscosity of 0.5 Pa·s, pretreated hollow glass microspheres, fumed silica and aluminosilicate at room temperature, add pretreated nano-calcium carbonate, control the temperature at 105°C, knead and stir for 2h, control the temperature at 130°C for dehydration and drying for 3.5h to obtain base glue;

[0047] S4, preparing a finished sealant product: mixing the base glue, hexamethyldisilazane and methyltrimethoxysilane evenly, then adding dibutyltin dilaurate and stirring in vacuum for 18 minutes to remove bubbles, thereby obtaining a finished sealant product;

[0048] The above step S1 is specifically as follows: the hollow glass microspheres and the sodium hydroxide solution with a concentration of 0.2 mol / L are mixed evenly and stirred at 78°C for 2h, washed with deionized water until the solution pH is 7, filtered, and the hollow glass microspheres are dried at 98°C for 11h to obtain dried hollow glass microspheres, the dried hollow glass microspheres and ethyl acetate are ultrasonically dispersed for 33min, dodecyltrimethoxysilane is added, mixed evenly, and heated to 75°C for reflux for 3h, after the reflux is completed, the product is washed with ethyl acetate 3 times, filtered, and vacuum dried at 53°C for 54h to obtain pretreated hollow glass microspheres;

[0049] The usage ratio of the hollow glass microspheres and the sodium hydroxide solution is 1.1 g:35 mL; the usage ratio of the dried hollow glass microspheres, ethyl acetate and dodecyltrimethoxysilane is 1.1 g:100 mL:0.15 g;

[0050] The above step S2 is specifically as follows: mixing nano-calcium carbonate and deionized water evenly to obtain a mixture A; mixing hexadecyl phosphate and anhydrous ethanol evenly to obtain a mixture B; mixing lauric acid and anhydrous ethanol evenly to obtain a mixture C; mixing the mixture A and the mixture B evenly, stirring at 72° C. for 1 hour, adding the mixture C after stirring, stirring at the same temperature, cooling to 23° C., filtering, washing twice with anhydrous ethanol and then with deionized water, filtering, and drying at 105° C. to obtain pretreated nano-calcium carbonate;

[0051] The dosage ratio of the nano-calcium carbonate and deionized water is 1.1 g:15 mL; the mass ratio of the hexadecyl phosphate and anhydrous ethanol is 0.05:11; the molar ratio of lauric acid and anhydrous ethanol is 1:8.5; the mass ratio of the mixture A, the mixture B and the mixture C is 1:0.04:0.05;

[0052] Wherein, the mass ratio of α,ω-dihydroxypolydimethylsiloxane, polydimethylsiloxane, pretreated hollow glass microspheres, fumed silica, aluminosilicate and pretreated nano-calcium carbonate in step S3 is 105:5:10:4:7:25;

[0053] The method of adding the pretreated nano-calcium carbonate in step S3 is to add the pretreated nano-calcium carbonate evenly in three times;

[0054] Wherein, the mass ratio of the base glue, hexamethyldisilazane, methyltrimethoxysilane and dibutyltin dilaurate in step S4 is 100:0.35:7:2.

[0055] Example 3

[0056] A method for preparing a silicone structural sealant, the preparation method specifically comprising the following steps:

[0057] S1, pretreatment A: pretreating the hollow glass microspheres to obtain pretreated hollow glass microspheres;

[0058] S2, pretreatment B: pretreating the nano calcium carbonate to obtain pretreated nano calcium carbonate;

[0059] S3, preparing base glue: knead α, ω-dihydroxy polydimethylsiloxane with a viscosity of 25 Pa·s, polydimethylsiloxane with a viscosity of 0.5 Pa·s, pretreated hollow glass microspheres, fumed silica and aluminosilicate at room temperature, add pretreated nano-calcium carbonate, control the temperature at 110°C, knead and stir for 3 hours, control the temperature at 135°C for dehydration and drying for 4 hours to obtain base glue;

[0060] S4, preparing a finished sealant product: mixing the base glue, hexamethyldisilazane and methyltrimethoxysilane evenly, then adding dibutyltin dilaurate and stirring in a vacuum for 20 minutes to remove bubbles, thereby obtaining a finished sealant product;

[0061] The above step S1 is specifically as follows: the hollow glass microspheres and the sodium hydroxide solution with a concentration of 0.2 mol / L are mixed evenly and stirred at 75°C for 2h, washed with deionized water until the solution pH is 7, filtered, and the hollow glass microspheres are dried at 100°C for 12h to obtain dried hollow glass microspheres, the dried hollow glass microspheres and ethyl acetate are ultrasonically dispersed for 35min, dodecyltrimethoxysilane is added, mixed evenly, and heated to 80°C for reflux for 3.5h, and after the reflux is completed, the product is washed 4 times with ethyl acetate, filtered, and vacuum dried at 55°C for 51h to obtain pretreated hollow glass microspheres;

[0062] The usage ratio of the hollow glass microspheres and the sodium hydroxide solution is 1.2 g:32 mL; the usage ratio of the dried hollow glass microspheres, ethyl acetate and dodecyltrimethoxysilane is 1.3 g:135 mL:0.18 g;

[0063] The above step S2 is specifically as follows: mixing nano-calcium carbonate and deionized water evenly to obtain a mixture A; mixing hexadecyl phosphate and anhydrous ethanol evenly to obtain a mixture B; mixing lauric acid and anhydrous ethanol evenly to obtain a mixture C; mixing the mixture A and the mixture B evenly, stirring at 75°C for 1.5h, adding the mixture C after stirring, stirring at the same temperature, cooling to 24°C, filtering, washing with anhydrous ethanol and then with deionized water for three times, filtering, and drying at 110°C to obtain pretreated nano-calcium carbonate;

[0064] The dosage ratio of the nano-calcium carbonate and deionized water is 1.2 g:14 mL; the mass ratio of the hexadecyl phosphate and anhydrous ethanol is 0.04:12; the molar ratio of the lauric acid and anhydrous ethanol is 1:8; the mass ratio of the mixture A, the mixture B and the mixture C is 1:0.035:0.04;

[0065] Wherein, the mass ratio of α,ω-dihydroxypolydimethylsiloxane, polydimethylsiloxane, pretreated hollow glass microspheres, fumed silica, aluminosilicate and pretreated nano-calcium carbonate in step S3 is 110:10:9:5:11:30;

[0066] The method of adding the pretreated nano-calcium carbonate in step S3 is to add the pretreated nano-calcium carbonate evenly in three times;

[0067] Wherein, the mass ratio of the base glue, hexamethyldisilazane, methyltrimethoxysilane and dibutyltin dilaurate in step S4 is 100:0.32:8:1.75.

[0068] Comparative Example 1

[0069] Compared with Example 3, the difference is that in step S3 of Comparative Example 1, no pretreated hollow glass microspheres are added, and the mass ratio of the α, ω-dihydroxypolydimethylsiloxane, polydimethylsiloxane, fumed silica, aluminosilicate and pretreated nano-calcium carbonate is 110:10:9.5:15.5:30; the other operating steps and parameters remain unchanged.

[0070] Comparative Example 2

[0071] Compared with Example 3, the difference is that in step S3 of Comparative Example 2, no fumed silica is added, and the mass ratio of the α, ω-dihydroxypolydimethylsiloxane, polydimethylsiloxane, pretreated hollow glass microspheres, aluminosilicate and pretreated nano-calcium carbonate is 110:10:11.5:13.5:30; the other operating steps and parameters remain unchanged.

[0072] Comparative Example 3

[0073] Compared with Example 3, the difference is that in step S3 of Comparative Example 3, no aluminosilicate is added, and the mass ratio of the α, ω-dihydroxypolydimethylsiloxane, polydimethylsiloxane, pretreated hollow glass microspheres, fumed silica and pretreated nano-calcium carbonate is 110:10:14.5:10.5:30; the other operating steps and parameters remain unchanged.

[0074] Comparative Example 4

[0075] Compared with Example 3, the difference is that in step S4 of Comparative Example 4, hexamethyldisilazane is not added, and the other operating steps and parameters remain unchanged.

[0076] Test Example 1

[0077] According to GB / T13477, the sealants prepared in Examples 1-3 and Comparative Examples 1-4 were subjected to tensile strength tests under different baking conditions to reflect the heat resistance. The results are shown in Table 1.

[0078] Table 1

[0079]

[0080] As can be seen from Table 1, the finished sealant product prepared by the present invention has excellent heat resistance. This is because the present invention uses modified hollow glass microspheres, fumed silica and aluminosilicate as sealant fillers, which synergistically make the prepared sealant have excellent heat resistance; on this basis, hexamethyldisilazane is added to effectively inhibit the reaction of thermal rearrangement and degradation of the main chain of the system at excessively high temperatures, thereby improving the thermal stability of the system, that is, further strengthening the heat resistance of the finished sealant product.

[0081] Comparative Example 5

[0082] Compared with Example 3, the difference is that in step S2 of Comparative Example 5, hexadecyl phosphate is not added, and the other operating steps and parameters remain unchanged.

[0083] Comparative Example 6

[0084] Compared with Example 3, the difference is that in step S2 of Comparative Example 6, lauric acid is not added, and the other operating steps and parameters remain unchanged.

[0085] Test Example 2

[0086] The sealants prepared in Examples 1-3 and Comparative Examples 5-6 were coated respectively, and after being completely cured, the static contact angle and the rolling contact angle were tested. The test liquid was deionized water, so as to judge the waterproof performance of the finished sealant.

[0087] Table 2

[0088] Static contact angle / ° Rolling contact angle / ° Example 1 156 9 Example 2 157 8 Example 3 157 8 Comparative Example 5 129 18 Comparative Example 6 131 25

[0089] As can be seen from Table 2, the finished sealant prepared by the present invention has excellent waterproof performance. This is because the present invention adds hexadecyl phosphate and lauric acid to modify the nano calcium carbonate, which effectively increases its hydrophobicity. The modified nano calcium carbonate is applied to the preparation of the sealant, which can greatly increase the waterproof performance of the finished sealant.

[0090] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0091] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A method for preparing a silicone structural sealant, characterized in that: The preparation method specifically comprises the following steps: S1, pretreatment A: pretreating the hollow glass microspheres to obtain pretreated hollow glass microspheres; S2, pretreatment B: pretreating the nano calcium carbonate to obtain pretreated nano calcium carbonate; S3, preparing a base glue: kneading α, ω-dihydroxy polydimethylsiloxane, polydimethylsiloxane, pretreated hollow glass microspheres, fumed silica and aluminosilicate uniformly at room temperature, adding pretreated nano-calcium carbonate, kneading and stirring under controlled temperature, and dehydrating and drying under controlled temperature to obtain a base glue; S4. Prepare the finished sealant product: stir the base glue, hexamethyldisilazane and the cross-linking agent evenly, then add the catalyst and stir in vacuum to remove bubbles to obtain the finished sealant product.

2. The method for preparing the silicone structural sealant according to claim 1, characterized in that: Step S1 is specifically as follows: The hollow glass microspheres and the sodium hydroxide solution are mixed evenly and stirred under controlled temperature, washed once, filtered, and the hollow glass microspheres are dried under controlled temperature to obtain dried hollow glass microspheres. The dried hollow glass microspheres and ethyl acetate are ultrasonically dispersed, dodecyltrimethoxysilane is added, mixed evenly, and heated to reflux under controlled temperature. After the reflux is completed, the product is washed twice, filtered, and dried under controlled temperature in a vacuum to obtain pretreated hollow glass microspheres.

3. The method for preparing the silicone structural sealant according to claim 2, characterized in that: The usage ratio of the hollow glass microspheres and the sodium hydroxide solution is 1-1.2 g: 30-35 mL; the usage ratio of the dried hollow glass microspheres, ethyl acetate and dodecyltrimethoxysilane is 1-1.3 g: 100-135 mL: 0.15-0.2 g.

4. The method for preparing the silicone structural sealant according to claim 1, characterized in that: Step S2 is specifically as follows: Nano calcium carbonate and deionized water are mixed evenly to obtain mixture A; hexadecyl phosphate and anhydrous ethanol are mixed evenly to obtain mixture B; lauric acid and anhydrous ethanol are mixed evenly to obtain mixture C; mixture A and mixture B are mixed evenly and stirred under controlled temperature, after stirring, mixture C is added and stirred under controlled temperature, cooled, filtered, washed, filtered, and dried under controlled temperature to obtain pretreated nano calcium carbonate.

5. The method for preparing the silicone structural sealant according to claim 4, characterized in that: The dosage ratio of the nano-calcium carbonate and deionized water is 1-1.2g:12.5-15mL; the mass ratio of the hexadecyl phosphate and anhydrous ethanol is 0.04-0.05:10-12; the molar ratio of the lauric acid and anhydrous ethanol is 1:8-8.5; the mass ratio of the mixture A, the mixture B and the mixture C is 1:0.03-0.04:0.04-0.

05.

6. The method for preparing the silicone structural sealant according to claim 1, characterized in that: In step S3, the mass ratio of α,ω-dihydroxypolydimethylsiloxane, polydimethylsiloxane, pretreated hollow glass microspheres, fumed silica, aluminosilicate and pretreated nano-calcium carbonate is 100-110:5-10:8-10:3-5:7-11:20-30.

7. The method for preparing the silicone structural sealant according to claim 1, characterized in that: The viscosity of the α,ω-dihydroxypolydimethylsiloxane in step S3 is 20-25 Pa·s; the viscosity of the polydimethylsiloxane is 0.5 Pa·s.

8. The method for preparing the silicone structural sealant according to claim 1, characterized in that: The mass ratio of the base glue, hexamethyldisilazane, cross-linking agent and catalyst in step S4 is 100:0.3-0.35:6-8:1.5-2.

9. The method for preparing the silicone structural sealant according to claim 1, characterized in that: In step S4, the cross-linking agent is methyltrimethoxysilane; and the catalyst is dibutyltin dilaurate.

10. A silicone structural sealant prepared by the method for preparing a silicone structural sealant according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Heat-resistant auxiliary agent for silicone rubber and preparation method of heat-resistant auxiliary agent

    CN114149689A

  • High-elongation light flame-retardant silicone sealant and preparation method thereof

    CN117025165A

  • Ceramic silicone rubber composite material and preparation method thereof

    CN118222100A

  • Room temperature curable polyoranopolysloxane silicone sealant composition, the silicone sealant and method for preparing thereof

    US20190194508A1

Cited By

  • Two-component silicone structural adhesive and preparation method thereof

    CN120924225A