Vanadium extraction sulfur-containing solid waste recycling method
Patent Information
- Application Number
- CN202410878754.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-02
- Publication Date
- 2024-10-15
AI Technical Summary
In the existing technology, the processing cost of solid waste from vanadium extraction is high and the recovery and utilization efficiency of sulfur element is low, resulting in resource waste and environmental pollution.
The steps of crushing, acid leaching, alkali leaching and purification are used to recover sulfur element from vanadium extraction solid waste. Sodium sulfide is generated through the reaction of sulfuric acid and sodium hydroxide. Combined with the use of calcium hydroxide and sodium carbonate, the roasting temperature is reduced and the sulfur content is increased. Element recovery rate.
It reduces the cost of processing solid waste from vanadium extraction, increases the recovery rate of sulfur elements, realizes the effective utilization of solid waste from vanadium extraction, and reduces pollution to land and environment.
Smart Images

Figure BDA0004923891090000111
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of chemical engineering, and in particular to a method for recycling vanadium-extracted sulfur-containing solid waste. Background Art
[0002] Vanadium extraction solid waste refers to the solid waste generated in the process of vanadium extraction. Vanadium extraction is usually a process of extracting vanadium from vanadium-containing ores by wet or dry methods. In this process, various solid wastes are generated, such as acid leaching residue, alkaline leaching residue, water leaching residue, etc. These wastes contain a large amount of sulfur, which makes them difficult to handle and has high processing costs, which leads to the accumulation of solid wastes and causes a series of problems, such as occupying land resources, polluting water sources, etc. The recycling of vanadium extraction solid waste is of great significance in improving resource utilization, improving economic benefits, reducing land occupation, and alleviating environmental pollution.
[0003] At present, the treatment of vanadium-containing solid waste is usually based on high-temperature roasting, with the temperature generally being 1200-1300°C. Most companies have given up on this treatment due to the high cost.
[0004] In the prior art, Chinese patent CN117737462A discloses a method for extracting vanadium from vanadium slag by solidifying calcium, and specifically discloses that vanadium slag is added to a solvent, sulfuric acid is used to adjust the system pH to 2-3.5, and after the reaction, the system is separated into solid and liquid to obtain vanadium slag A and solution A; vanadium slag A is oxidatively roasted to obtain roasted material B; and roasted material B is acid-leached to obtain leachate B, and leachate B is used as a raw material to extract vanadium. The roasting conditions are: oxidative roasting at a temperature of 850-950°C for 30-90 minutes to obtain roasted material B. It is beneficial to reduce the liquid-solid ratio in the acid leaching process and improve the roasting-leaching efficiency of vanadium, but it does not recycle the sulfur element in the vanadium slag, resulting in a waste of elements.
[0005] Chinese patent CN106495104A discloses a method for producing sodium sulfide based on vanadium-extracting solid waste sodium sulfate, and specifically discloses the following steps: A: batching: weighing solid waste sodium sulfate, coke powder and barium sulfide and putting them into a converter; B: roasting: heating the converter described in step A, performing roasting reaction, generating alkaline slag and molten sodium sulfide; C: thermal leaching: transferring the molten sodium sulfide described in step B into hot water for stirring and leaching, obtaining coarse slag and a primary sodium sulfide aqueous solution; D: slag removal and clarification: standing the primary sodium sulfide aqueous solution described in step C, after solid-liquid separation operation, obtaining fine slag and a secondary sodium sulfide aqueous solution; E: evaporation and concentration: evaporating and concentrating the secondary sodium sulfide aqueous solution described in step D, obtaining a concentrated sodium sulfide aqueous solution. It is based on roasting reaction to obtain molten sodium sulfide, the cost of producing sodium sulfide is relatively high, and waste slag containing barium is also generated while producing sodium sulfide, which is difficult to post-process.
[0006] In the prior art, sulfur element is recovered from vanadium-extracting solid waste by high-temperature roasting, which hinders the recycling of elements in the vanadium-extracting solid waste.
[0007] In view of this, it is of great significance to provide a method for recycling vanadium-extracted solid waste, which can reduce the recycling cost of sulfur and improve the efficiency of recovering sulfur from vanadium-extracted solid waste. Summary of the invention
[0008] The present invention provides a method for recycling vanadium-extracting solid waste, which solves the technical problems of accumulation of vanadium-extracting solid waste and effective recycling of sulfur element, realizes the recycling treatment of vanadium-extracting solid waste, reduces the treatment cost of vanadium-extracting solid waste, and improves the extraction efficiency of sulfur element in vanadium-extracting solid waste.
[0009] A method for recycling vanadium-containing sulfur-containing solid waste comprises the following steps:
[0010] 1) Crushing: ball-milling and sieving the vanadium-extracted sulfur-containing solid waste to obtain solid waste powder;
[0011] 2) Acid leaching: adding sulfuric acid solution to the crushed solid waste powder in step 1) for acid leaching, stirring and solid-liquid separation to obtain filter residue A and filtrate A;
[0012] 3) Alkali leaching: adding iron powder and sodium hydroxide solution to the filtrate A of the acid leaching in step 2) to carry out an alkaline leaching reaction to obtain a reaction solution containing sodium sulfide;
[0013] 4) Purification: adding calcium hydroxide solution to the reaction solution of the alkali leaching in step 3) to react, filtering to obtain filter residue B and filtrate B; adding sodium carbonate solution to the filter residue B, mixing, concentrating and crystallizing to obtain sodium sulfide solid;
[0014] 5) Making slag bricks: the filter residue A obtained by acid leaching in step 2) is mixed with lime and illite and heated to form, and then cooled and washed with washing liquid to obtain slag bricks.
[0015] In a specific embodiment of the present invention, in step 1) crushing, the sulfur content of the vanadium-extracted solid waste is 30% to 50wt%; and the mesh number of the filter used for screening is 80 to 120 meshes.
[0016] In a specific embodiment of the present invention, the mesh size of the filter used for sieving is 100 meshes.
[0017] In a specific embodiment of the present invention, in step 2) acid leaching, the mass ratio of the sulfuric acid solution to the solid waste powder is 8 to 12:1, and the concentration of the sulfuric acid solution is 25 to 40 wt %; the acid leaching stirring time is 2 to 3 hours; and the solid-liquid separation adopts a plate and frame filter press.
[0018] In a specific embodiment of the present invention, the solid-liquid separation time is 2 to 3 hours, the acid leaching stirring time is 2 to 3 hours, and the pressure is 0.149 to 0.159 MPa.
[0019] In a specific embodiment of the present invention, the solid-liquid separation time is 3 hours and the pressure is 0.152 MPa.
[0020] In a specific embodiment of the present invention, the concentration of the sulfuric acid solution is 35 wt %.
[0021] In a specific embodiment of the present invention, in step 3) alkaline leaching, the mass ratio of the sodium hydroxide solution to the filtrate A is 1:1.8-2.4, the mass ratio of the iron powder to the sodium hydroxide solution is 1:2-3, and the concentration of the sodium hydroxide solution is 350-500 g / L.
[0022] In a specific embodiment of the present invention, the mass ratio of the sodium hydroxide solution to the filtrate A is 1:2.2, the mass ratio of the iron powder to the sodium hydroxide solution is 1:2, and the concentration of the sodium hydroxide solution is 450 g / L.
[0023] In a specific embodiment of the present invention, in step 3) alkali leaching, the alkali leaching reaction temperature is 75-90° C. and the time is 1-2 hours.
[0024] In a specific embodiment of the present invention, the temperature of the alkali leaching reaction is 85° C. and the time is 1 hour.
[0025] In a specific embodiment of the present invention, in step 4) purification, the mass ratio of the reaction solution to the calcium hydroxide solution is 1:0.5-1.2.
[0026] In a specific embodiment of the present invention, the concentration of the calcium hydroxide solution is 25-35wt%.
[0027] In a specific embodiment of the present invention, the mass ratio of the reaction solution to the calcium hydroxide solution is 1:1.2, and the concentration of the calcium hydroxide solution is 35wt%.
[0028] In a specific embodiment of the present invention, in step 4) purification, the mass ratio of the filter residue B to the sodium carbonate solution is 1:2-3, and the concentration of the sodium carbonate solution is 30-40wt%.
[0029] In a specific embodiment of the present invention, the mass ratio of the filter residue B to the sodium carbonate solution is 1:3, and the concentration of the sodium carbonate solution is 35wt%.
[0030] In a specific embodiment of the present invention, in step 4) purification, the concentration temperature is 50-100°C, and the crystallization temperature is 5-15°C.
[0031] In a specific embodiment of the present invention, the concentration temperature is 60°C and the crystallization temperature is 10°C.
[0032] In a specific embodiment of the present invention, in step 5) slag bricks are made, the mass ratio of the filter residue A to lime and illite is 1:0.15-0.25:0.05-0.1.
[0033] In a specific embodiment of the present invention, the mass ratio of the filter residue A to lime and illite is 1:0.2:0.08.
[0034] In a specific embodiment of the present invention, the heating temperature is 90-110° C.; the washing liquid is distilled water, and the washing times are 5-6 times.
[0035] In a specific embodiment of the present invention, the heating temperature is 100°C.
[0036] In the present invention, during the acid leaching process in step 2), negative divalent sulfur reacts with sulfate ions under acidic conditions to generate elemental sulfur and sulfur dioxide gas, and the chemical reaction equation is shown in the following (1):
[0037]
[0038] Step 3) During the alkaline leaching process, elemental sulfur reacts with iron powder to generate ferrous sulfide, and ferrous sulfide reacts with sodium hydroxide to generate sodium sulfide and ferrous hydroxide. The chemical reaction equations are shown in (2) and (3) below, respectively:
[0039] Fe+S→FeS (2);
[0040] FeS+2NaOH→Na 2 S+Fe(OH) 2 (3);
[0041] During the purification process of step 4), the reaction solution containing sodium sulfide reacts with calcium hydroxide to generate calcium sulfide solid and sodium hydroxide. The chemical reaction equation is shown in the following (4):
[0042] 2Na 2 S+Ca(OH) 2 →CaS↓+2NaOH (4);
[0043] When calcium sulfide solid is mixed with sodium carbonate, it reacts to form calcium carbonate and sodium sulfide. The chemical reaction equation is shown below (5):
[0044] CaS+Na 2 CO 3 →CaCO3↓+Na 2 S (5).
[0045] The beneficial effects of the present invention are as follows: the present invention recovers sulfur from vanadium-containing sulfur-containing solid waste based on crushing, acid leaching, alkali leaching and purification steps, and the product is sodium sulfide solid, which does not require roasting, thereby reducing the treatment cost of vanadium-containing sulfur-containing solid waste, and the recovery rate of sulfur in vanadium-containing sulfur-containing solid waste is high. DETAILED DESCRIPTION
[0046] To make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described in detail below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other implementation methods obtained by ordinary technicians in this field without creative work belong to the scope of protection of the present invention.
[0047] A method for recycling vanadium-containing sulfur-containing solid waste comprises the following steps:
[0048] 1) Crushing: ball-milling and sieving the vanadium-extracted sulfur-containing solid waste to obtain solid waste powder;
[0049] 2) Acid leaching: adding sulfuric acid solution to the crushed solid waste powder in step 1) for acid leaching, stirring and solid-liquid separation to obtain filter residue A and filtrate A;
[0050] 3) Alkali leaching: adding iron powder and sodium hydroxide solution to the filtrate A in step 2) to carry out an alkaline leaching reaction to obtain a reaction solution containing sodium sulfide;
[0051] 4) Purification: adding calcium hydroxide solution to the reaction solution of the alkali leaching in step 3) to react, filtering to obtain filter residue B and filtrate B; adding sodium carbonate solution to the filter residue B, mixing, concentrating and crystallizing to obtain sodium sulfide solid;
[0052] 5) Making slag bricks: the filter residue A obtained by acid leaching in step 2) is mixed with lime and illite and heated to form, and then cooled and washed with washing liquid to obtain slag bricks.
[0053] In some examples, in step 1) crushing, the sulfur content of the vanadium-extracted solid waste is 30% to 50wt%; and the mesh number of the filter used for screening is 80 to 120 meshes.
[0054] In some examples, the sieving uses a filter with a mesh size of 100 meshes.
[0055] In some examples, in step 2) acid leaching, the mass ratio of the sulfuric acid solution to the solid waste powder is 8 to 12:1, and the concentration of the sulfuric acid solution is 25 to 40 wt %; the acid leaching stirring time is 2 to 3 hours; and the solid-liquid separation adopts a plate and frame filter press.
[0056] In some examples, the solid-liquid separation time is 2 to 3 hours, the acid leaching stirring time is 2 to 3 hours, and the pressure is 0.149 to 0.159 MPa;
[0057] In some examples, the solid-liquid separation time is 3 h and the pressure is 0.152 MPa;
[0058] In some examples, the concentration of the sulfuric acid solution is 35 wt %.
[0059] In some examples, in step 3) alkaline leaching, the mass ratio of the sodium hydroxide solution to the filtrate A is 1:1.8-2.4, the mass ratio of the iron powder to the sodium hydroxide solution is 1:2-3, and the concentration of the sodium hydroxide solution is 350-500 g / L.
[0060] It should be noted that after iron powder and sodium hydroxide solution are added to the filtrate A for alkaline leaching reaction, the reaction solution is filtered to remove ferrous hydroxide and obtain a reaction solution containing sodium sulfide.
[0061] In some examples, the mass ratio of the sodium hydroxide solution to the filtrate A is 1:2.2, the mass ratio of the iron powder to the sodium hydroxide solution is 1:2, and the concentration of the sodium hydroxide solution is 450 g / L.
[0062] In some examples, in step 3) alkali leaching, the alkali leaching reaction temperature is 75-90° C. and the time is 1-2 hours.
[0063] In some examples, the alkali leaching reaction is carried out at a temperature of 85° C. and for a time of 1 h.
[0064] In some examples, in step 4) purification, the mass ratio of the reaction solution to the calcium hydroxide solution is 1:0.5-1.2.
[0065] In some examples, the concentration of the calcium hydroxide solution is 25-35 wt %.
[0066] In some examples, the mass ratio of the reaction solution to the calcium hydroxide solution is 1:1.2, and the concentration of the calcium hydroxide solution is 35 wt %.
[0067] In the present invention, after the reaction liquid reacts with the calcium hydroxide solution, a sponge filter is used for filtration, and the pore size of the filter is 20-40 μm.
[0068] In some examples, in step 4) purification, the mass ratio of the filter residue B to the sodium carbonate solution is 1:2-3, and the concentration of the sodium carbonate solution is 30-40 wt%.
[0069] In some examples, the mass ratio of the filter residue B to the sodium carbonate solution is 1:3, and the concentration of the sodium carbonate solution is 35 wt %.
[0070] In some examples, in step 4) purification, the concentration temperature is 50-100°C, and the crystallization temperature is 5-15°C.
[0071] In some examples, the concentration temperature is 60°C and the crystallization temperature is 10°C.
[0072] In some examples, in step 5) for making slag bricks, the mass ratio of the filter residue A to lime and illite is 1:0.15-0.25:0.05-0.1; preferably, the mass ratio of the filter residue A to lime and illite is 1:0.2:0.08.
[0073] In some examples, the heating temperature is 90-110° C.; the washing liquid is distilled water, and the washing times are 5-6 times.
[0074] In some examples, the heating temperature is 100°C.
[0075] In the present invention, the filter residue A is mixed with lime and illite and heated, and then formed in a brick-making machine. After forming, the mixture is cooled and washed with distilled water for 5 to 6 times to obtain a slag brick.
[0076] The technical solution of the present invention is further described below through specific embodiments.
[0077] Example 1
[0078] The element contents of the vanadium-extracting solid waste in this embodiment are: S 33.24wt%, Fe 8.72wt%, Mg 2.88wt%.
[0079] This embodiment provides a method for recycling vanadium-containing sulfur-containing solid waste, comprising the following steps:
[0080] 1. Break the vanadium-extracting sulfur-containing solid waste into pieces, add them into a ball mill with an 80-mesh screen, grind and screen them until all the vanadium-extracting sulfur-containing solid waste is screened off to obtain solid waste powder;
[0081] 2. The solid waste powder was mixed with a 30wt% sulfuric acid solution (with a mass ratio of 9:1:1 to the solid waste powder) for 2 hours, and then the solid-liquid mixture was input into a plate-frame filter press for solid-liquid separation to obtain filter residue A and filtrate A; wherein the solid-liquid separation time in the plate-frame filter press was 2 hours and the pressure was 0.150 MPa;
[0082] 3. Add iron powder (mass ratio to filtrate A is 1:1.2) and 350 g / L sodium hydroxide solution (mass ratio to filtrate is 1:1.8) to filtrate A, stir and react at 75°C for 1 hour, and filter with a top cloth filter to obtain a reaction solution containing sodium sulfide;
[0083] 4. Add 25 wt% calcium hydroxide solution (with a mass ratio of 0.8:1 to the reaction solution) to the reaction solution, stir and react, and filter through a sponge filter to obtain a filter residue B and a filtrate B;
[0084] 5. Add 30 wt% sodium carbonate solution (with a mass ratio of 2:1 to the filter residue B) to dissolve it, concentrate it at 80°C to a 92% sodium sulfide solution, and then crystallize it at 0°C to obtain a crude sodium sulfide product;
[0085] 6. Wash the crude sodium sulfide with low-concentration ethanol and then dry it in a vacuum drying oven, and finally crush it with a blade crusher to obtain a finished sodium sulfide product;
[0086] 7. Mix the filter residue A and lime in a mass ratio of 1:0.15, then add illite in a mass ratio of 0.06:1 to the filter residue A, mix at 90°C and put into a brick-making machine for molding. After cooling, wash with distilled water for 5 to 6 times to obtain brick residue.
[0087] Example 2
[0088] The element contents of the vanadium-extracting solid waste in this embodiment are: S 38.26wt%, Fe 6.74wt%, Mg 1.26wt%.
[0089] This embodiment provides a method for recycling vanadium-containing sulfur-containing solid waste, comprising the following steps:
[0090] 1. Break the vanadium-extracting sulfur-containing solid waste into pieces, add them into a ball mill with a 100-mesh screen, grind and screen them until all the vanadium-extracting sulfur-containing solid waste is screened off to obtain solid waste powder;
[0091] 2. The solid waste powder was mixed with a 35wt% sulfuric acid solution (with a mass ratio of 10:1 to the solid waste powder) and stirred for 3h, and then the solid-liquid mixture was input into a plate-frame filter press for solid-liquid separation to obtain filter residue A and filtrate A; wherein the solid-liquid separation time in the plate-frame filter press was 3h and the pressure was 0.152MPa;
[0092] 3. Add iron powder (mass ratio to filtrate A is 1:2.2) and 450 g / L sodium hydroxide solution (mass ratio to filtrate is 1:2) to filtrate A, mix, stir and react at 85° C. for 1 h, filter with a top cloth filter to obtain a reaction solution containing sodium sulfide;
[0093] 4. Add 35 wt% calcium hydroxide solution (with a mass ratio of 1.2:1 to the reaction solution) to the reaction solution, stir and react, and filter through a sponge filter to obtain a filter residue B and a filtrate B;
[0094] 5. Add 30 wt% sodium carbonate solution (with a mass ratio of 3:1 to the filter residue B) to dissolve it, concentrate it at 60°C to a 97% sodium sulfide solution, and then crystallize it at 10°C to obtain a crude sodium sulfide product;
[0095] 6. Wash the crude sodium sulfide with low-concentration ethanol and then dry it in a vacuum drying oven, and finally crush it with a blade crusher to obtain a finished sodium sulfide product;
[0096] 7. Mix the filter residue A and lime in a mass ratio of 1:0.2, then add illite in a mass ratio of 0.08:1 to the filter residue A, mix at 100°C and put into a brick-making machine for molding. After cooling, wash with distilled water for 5 to 6 times to obtain brick residue.
[0097] Example 3
[0098] The element contents of the vanadium-extracting solid waste in this embodiment are: S 45wt%, Fe 9.2wt%, and Mg 0.95wt%.
[0099] This embodiment provides a method for recycling vanadium-containing sulfur-containing solid waste, comprising the following steps:
[0100] 1. Break the vanadium-extracting sulfur-containing solid waste into pieces, add them into a ball mill with a 120-mesh screen, grind and screen them until all the vanadium-extracting sulfur-containing solid waste is screened off to obtain solid waste powder;
[0101] 2. The solid waste powder was mixed with a 40wt% sulfuric acid solution (with a mass ratio of 11:1 to the solid waste powder) and stirred for 2h, and then the solid-liquid mixture was input into a plate-frame filter press for solid-liquid separation to obtain filter residue A and filtrate A; wherein the solid-liquid separation time in the plate-frame filter press was 3h and the pressure was 0.156MPa;
[0102] 3. Add iron powder (mass ratio to filtrate A is 1:3) and 500 g / L sodium hydroxide solution (mass ratio to filtrate is 1:2.4) to filtrate A, stir and react at 90° C. for 1.5 h, and filter with a top cloth filter to obtain a reaction solution containing sodium sulfide;
[0103] 4. Add 35 wt% calcium hydroxide solution (with a mass ratio of 1:1 to the reaction solution) to the reaction solution, stir and react, and filter through a sponge filter to obtain a filter residue B and a filtrate B;
[0104] 5. Add 40 wt% sodium carbonate solution (with a mass ratio of 2.5:1 to the filter residue B) to dissolve it, concentrate it at 50°C to a sodium sulfide solution with a concentration of 80%, and then crystallize it at 20°C to obtain a crude sodium sulfide product;
[0105] 6. Wash the crude sodium sulfide with low-concentration ethanol and then dry it in a vacuum drying oven, and finally crush it with a blade crusher to obtain a finished sodium sulfide product;
[0106] 7. Mix the filter residue A and lime in a mass ratio of 1:0.25, then add illite in a mass ratio of 0.05:1 to the filter residue A, mix at 110°C and put into a brick-making machine for molding. After cooling, wash with distilled water for 5 to 6 times to obtain brick residue.
[0107] Comparative Example 1
[0108] This comparative example is different from Example 2 in that the same molar amount of barium hydroxide is used to replace calcium hydroxide.
[0109] Comparative Example 2
[0110] This comparative example is compared with Example 2, except that sodium bicarbonate is used instead of sodium carbonate with the same molar amount.
[0111] Comparative Example 3
[0112] The difference between this comparative example and Example 2 is that the same molar amount of hydrochloric acid is used instead of sulfuric acid.
[0113] The sulfur content in the sodium sulfide products obtained in Examples 1-3 and Comparative Examples 1-3 was detected, and the extraction rate of sulfur element was calculated, and the statistics are shown in Table 1.
[0114] The slag bricks obtained in Examples 1-3 and Comparative Examples 1-3 were tested for compressive strength, and the results are shown in Table 1.
[0115] Table 1
[0116]
[0117] Note: “-” indicates no result or the same result as Example 2.
Claims
1. A method for recycling vanadium-containing sulfur-containing solid waste, characterized in that: The following steps are involved: 1) Crushing: ball-milling and sieving the vanadium-extracted sulfur-containing solid waste to obtain solid waste powder; 2) Acid leaching: adding sulfuric acid solution to the crushed solid waste powder in step 1) for acid leaching, stirring and solid-liquid separation to obtain filter residue A and filtrate A; 3) Alkali leaching: adding iron powder and sodium hydroxide solution to the filtrate A of the acid leaching in step 2) to carry out an alkaline leaching reaction to obtain a reaction solution containing sodium sulfide; 4) Purification: adding calcium hydroxide solution to the reaction solution of the alkali leaching in step 3) to react, filtering to obtain filter residue B and filtrate B; adding sodium carbonate solution to the filter residue B, mixing, concentrating and crystallizing to obtain sodium sulfide solid; 5) Making slag bricks: the filter residue A obtained by acid leaching in step 2) is mixed with lime and illite and heated to form, and then cooled and washed with washing liquid to obtain slag bricks.
2. The method for recycling vanadium-containing sulfur-containing solid waste according to claim 1, characterized in that: Step 1) crushing, the sulfur content of the vanadium-extracting solid waste is 30% to 50wt%; the mesh number of the filter used for screening is 80 to 120 meshes; Preferably, the mesh size of the filter used for sieving is 100 meshes.
3. The method for recycling vanadium-containing sulfur-containing solid waste according to claim 1, characterized in that: Step 2) acid leaching, the mass ratio of the sulfuric acid solution to the solid waste powder is 8-12:1, the concentration of the sulfuric acid solution is 25-40wt%; the acid leaching stirring time is 2-3h; the solid-liquid separation adopts a plate and frame filter press; Preferably, the mass ratio of the sulfuric acid solution to the solid waste powder is 10:1; Preferably, the solid-liquid separation time is 2 to 3 hours, and the acid leaching stirring time is 2 to 3 hours. The pressure is 0.149~0.159MPa; More preferably, the solid-liquid separation time is 3 hours, and the acid leaching stirring time is 2.5 hours. The pressure is 0.152MPa; Preferably, the concentration of the sulfuric acid solution is 35wt%.
4. The method for recycling vanadium-containing sulfur-containing solid waste according to claim 1, characterized in that: Step 3) alkaline leaching, the mass ratio of the sodium hydroxide solution to the filtrate A is 1:1.8-2.4, the mass ratio of the iron powder to the sodium hydroxide solution is 1:2-3, and the concentration of the sodium hydroxide solution is 350-500 g / L; preferably, the mass ratio of the sodium hydroxide solution to the filtrate A is 1:2.2, the mass ratio of the iron powder to the sodium hydroxide solution is 1:2, and the concentration of the sodium hydroxide solution is 450 g / L.
5. The method for recycling vanadium-containing sulfur-containing solid waste according to claim 1, characterized in that: Step 3) alkali leaching, wherein the alkali leaching reaction temperature is 75-90° C. and the time is 1-2 hours; Preferably, the alkali leaching reaction is carried out at a temperature of 85° C. and for a time of 1 h.
6. The method for recycling vanadium-containing sulfur-containing solid waste according to claim 1, characterized in that: Step 4) purification, the mass ratio of the reaction solution to the calcium hydroxide solution is 1:0.5-1.2; Preferably, the concentration of the calcium hydroxide solution is 25-35wt%; More preferably, the mass ratio of the reaction solution to the calcium hydroxide solution is 1:1.2, and the concentration of the calcium hydroxide solution is 35wt%.
7. The method for recycling vanadium-containing sulfur-containing solid waste according to claim 1, characterized in that: Step 4) purification, the mass ratio of the filter residue B to the sodium carbonate solution is 1:2-3, and the concentration of the sodium carbonate solution is 30-40wt%; preferably, the mass ratio of the filter residue B to the sodium carbonate solution is 1:3, and the concentration of the sodium carbonate solution is 35wt%.
8. The method for recycling vanadium-containing sulfur-containing solid waste according to claim 1, characterized in that: Step 4) purification, the concentration temperature is 50-80°C, and the crystallization temperature is 5-15°C; preferably, the concentration temperature is 60°C, and the crystallization temperature is 10°C.
9. The method for recycling vanadium-containing sulfur-containing solid waste according to claim 1, characterized in that: Step 5) making slag bricks, the mass ratio of the filter residue A to lime and illite is 1:0.15-0.25:0.05-0.1; preferably, the mass ratio of the filter residue A to lime and illite is 1:0.2:0.
08.
10. The method for recycling vanadium-containing sulfur-containing solid waste according to claim 1, characterized in that: The heating temperature is 90-110°C; the washing liquid is distilled water, and the washing times are 5-6 times; Preferably, the heating temperature is 100°C.