Method for synergistically extracting lithium from ammonium fluoride, gypsum and lithium ore

Through the collaborative roasting method of ammonium fluoride and gypsum, the problems of high cost and low resource utilization in the lithium extraction process from lithium ore are solved, and efficient lithium recovery and environmental improvement are achieved, with the lithium extraction rate reaching 92.4%-97.1%.

CN118773452APending Publication Date: 2024-10-15CENT SOUTH UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410742800.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-11
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

The existing lithium extraction process from lithium ores has the problems of high cost, environmental pollution and low resource utilization. In particular, waste gypsum is difficult to effectively utilize, and the lithium extraction efficiency of lithium clay ores is low.

Method used

Using the ammonium fluoride and gypsum collaborative roasting method, lithium ore is mixed with ammonium fluoride and gypsum and then roasted at high temperature to generate a high-concentration lithium-containing leachate. Fluoride ions are used to improve the extraction efficiency of lithium sulfate and reduce production costs.

Benefits of technology

It achieves efficient recovery of lithium and reuse of resources, reduces the risk of environmental pollution, is low-cost, and is suitable for large-scale production. The lithium extraction rate reaches 92.4%-97.1%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118773452A_ABST
    Figure CN118773452A_ABST
Patent Text Reader

Abstract

The invention discloses a method for synergistically extracting lithium from ammonium fluoride, gypsum and lithium ore, which comprises the following steps: firstly, crushing the lithium ore to be extracted; secondly, uniformly mixing the crushed lithium ore with ammonium fluoride and gypsum, and granulating; then, putting the granulated pellets into a muffle furnace for high-temperature roasting; finally, leaching the calcined product with water to obtain a filtrate which is a lithium-containing mother solution; according to the method, the problems of gypsum treatment and lithium ore resource development are effectively solved, the recovery rate of lithium is creatively high by utilizing ammonium fluoride and gypsum, the cost is low and the process is simple in the lithium extraction process, and the method plays an important role in waste resource utilization and efficient development and utilization of lithium resources and has a wide application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of lithium extraction from lithium ore, and in particular to a method for extracting lithium from lithium ore in a coordinated manner using ammonium fluoride, gypsum and lithium ore. Background Art

[0002] Lithium ore is mined primarily from three types of deposits: pegmatite, brine, and sedimentary. Lithium in pegmatites is often found in ores such as spodumene and lepidolite. Brine-type lithium deposits can be divided into underground brine and salt lake brine types. Sedimentary-type deposits primarily refer to lithium ores found in sedimentary rocks with lower lithium grades. Currently, pegmatite and brine-type lithium deposits are the most mined worldwide. my country has abundant reserves of lepidolite, and the development of efficient lithium extraction processes is crucial for their comprehensive utilization. Sulfate roasting is the mainstream extraction process for lepidolite due to its low energy consumption and short roasting and leaching times. However, processes that utilize gypsum as a sulfate source and co-smelt lepidolite are less common. With the widespread use of lithium batteries, the demand for lithium is increasing. Sedimentary-type lithium deposits have not yet been developed on a large scale due to their low lithium grade, the varying occurrence of lithium in different types of deposits, and their relatively recent discovery. With the vigorous development of the new energy industry, lithium clay ores are expected to become a research focus in the future to alleviate the shortage of lithium resources. Currently, direct leaching and additive roasting are the main methods for extracting lithium from clay ores. However, research on the synergistic smelting of lithium clay ores using waste gypsum has been limited.

[0003] As China's urbanization accelerates, urban waste generation is increasing. The current mainstream waste treatment process is high-temperature incineration. During incineration, the presence of sulfur in domestic waste oxidizes to sulfur dioxide at high temperatures, requiring prompt absorption and treatment to prevent serious environmental problems. Companies often use lime-limestone to recover sulfur dioxide from flue gas. The byproduct is waste gypsum. Due to low gypsum demand, long transportation distances, and high raw material costs, waste gypsum is difficult to effectively utilize. Long-term storage occupies large tracts of land and can cause secondary pollution of soil and water sources. Waste gypsum utilization in my country is primarily concentrated in the mid- and low-end cement and gypsum building materials industries, followed by the production of gypsum-based building materials. A small amount is also used in agriculture to improve saline-alkali soils. Scaled-up and industrialized application in other sectors has yet to be achieved.

[0004] Therefore, considering that my country has a large output of industrial byproduct gypsum and a low resource utilization rate. Adhering to the idea of ​​green resource utilization, the above-mentioned byproduct gypsum can be used to react with large reserves of lithium clay ore and lithium mica to obtain a high-concentration lithium-containing leachate, thereby achieving resource recycling and environmental improvement. Patent CN201410098348.9 proposes a modified roasting-heap leaching method, adding calcium fluoride during the roasting process. However, calcium fluoride is expensive, and later fluoride removal is difficult. If not handled properly, it will pollute the environment. In addition, fluoride ions will corrode equipment, resulting in high costs. Patent CN202210353260.1 involves a method of mixing lithium clay ore with soda ash and sodium sulfate for roasting and then leaching. This method is prone to equipment corrosion and high costs. Patent CN110697740A involves a method for extracting lithium by smelting lithium porcelain stone and gypsum. The gypsum includes industrial gypsum or flue gas desulfurization gypsum, but the patent does not involve the lithium extraction efficiency of the reaction between lithium porcelain stone and desulfurization gypsum. CN115821060A proposes mixing lepidolite, calcium carbonate, sodium sulfate, and potassium sulfate and then calcining them at high temperature. This process involves a complex variety of additives and the high price of potassium sulfate, resulting in high costs and prohibitive industrial use. Furthermore, potassium ions are introduced, making them difficult to separate from lithium during subsequent purification. Patent CN116219204A proposes producing lithium carbonate by reacting lepidolite with gypsum and calcium oxide. The gypsum can be solid waste gypsum from the lime process for producing lithium hydroxide or from hydrofluoric acid smelters. However, the solid waste gypsum content cannot exceed 50% of the total gypsum, resulting in a low waste treatment capacity. Summary of the Invention

[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for synergistically extracting lithium using ammonium fluoride, gypsum and lithium ore. The method comprises the following steps: first, crushing the lithium ore to be extracted; second, uniformly mixing the lithium ore obtained by the crushing with ammonium fluoride and gypsum, and granulating; then, placing the granulated pellets in a muffle furnace for high-temperature roasting; finally, leaching the calcined product with water, and the filtrate is a lithium-containing mother liquor. The method effectively solves the problems of gypsum treatment and lithium ore resource development, utilizes ammonium fluoride and gypsum, creatively achieves a high lithium recovery rate, low costs in the lithium extraction process, and a simple process, plays an important role in waste resource utilization and efficient development and utilization of lithium resources, and has broad application prospects.

[0006] In order to achieve the above technical effects, the following technical solutions are adopted:

[0007] A method for extracting lithium by synergistically using ammonium fluoride, gypsum and lithium ore, comprising the following steps:

[0008] Step S1: crushing the lithium ore to be extracted;

[0009] Step S2: uniformly mixing the crushed lithium ore obtained in step S1 with ammonium fluoride and gypsum, and granulating the mixture;

[0010] Step S3: calcining the pellets prepared in step S2 at high temperature to obtain a calcined product;

[0011] Step S4: leaching the calcined product obtained in step S3 with a leaching agent, wherein the filtrate is a lithium-containing mother liquor and the leached residue is a filler.

[0012] The key to this invention lies in the synergistic roasting reaction of difficult-to-treat waste gypsum and ammonium fluoride with lithium ore, achieving resource utilization of the gypsum and efficient extraction of lithium resources. This method utilizes waste gypsum, a common waste resource, achieving resource utilization and reducing environmental pollution. Through the reaction with lithium ore, efficient lithium extraction is achieved, meeting the demand for lithium resources. Furthermore, this method features simple steps, low cost, easy operation, and suitability for large-scale production.

[0013] The principle of extracting lithium by reacting lithium ore and gypsum is: under high temperature conditions, gypsum solidifies the free silicon dioxide in the lithium ore and produces sulfur dioxide at the same time. The sulfur dioxide reacts with the lithium in the lithium ore to form soluble lithium sulfate.

[0014]

[0015] In the above reaction, although calcium sulfate fixes a portion of the free silica in the lithium ore in the first step, in the second step, free silica is produced at the same time as lithium sulfate. Due to the production of free silica, the reaction may lead to the reverse reaction of the second step (refer to the reaction mechanism of the first step), that is, lithium sulfate reacts with free silica to produce lithium ore products.

[0016] On the other hand, according to the above reaction mechanism, in the second step of the reaction, since lithium sulfate and free silica are generated at the same time, the free silica will wrap or adhere to the generated lithium sulfate, causing the lithium sulfate to enter the surface or interior of the free silica, hindering the dissolution of lithium sulfate in the subsequent leaching agent, so that the lithium extraction efficiency of the calcium sulfate auxiliary agent (gypsum) alone is not high. It is recorded in relevant literature that calcium sulfate itself participates in the lithium extraction reaction as an auxiliary agent. It is roasted with lithium clay ore at 800°C, 900°C, 1000°C and 1050°C for 4h, and the roasted samples are water-leached with water. The lithium leaching rates are 6%, 41%, 72% and 68% respectively.

[0017] However, the additive of the present invention contains not only gypsum, i.e., calcium sulfate, but also ammonium fluoride. At high temperatures, ammonium fluoride can decompose in the reaction system to produce hydrogen fluoride. Due to the presence of free water in the system, free fluoride ions are generated. The reaction equation is as follows:

[0018] NH4F→NH3↑+HF↑+N2↑

[0019] Fluoride ions react with the free silica product of the second step reaction at high temperature, and the silica in the second step product is converted into fluorosilicate ions for removal (fluoride ions and silica undergo an ion exchange reaction, fluoride ions replace a portion of oxygen ions in silica to form fluorosilicate ions, an exothermic reaction, and the reaction rate increases with increasing temperature). The advantages are: first, the reduction of free silica is conducive to the forward progress of the second step reaction, thereby increasing the yield of lithium sulfate and reducing the reverse reaction, thereby reducing the loss of lithium sulfate; second, the reduction of free silica in the second step reaction reduces the free silica generated at the same time from encapsulating or adhering to the generated lithium sulfate, reducing the leaching barrier of silica to lithium sulfate, and is more conducive to the dissolution of lithium sulfate in the subsequent leaching agent, thereby further increasing the extraction efficiency of lithium sulfate; therefore, the present invention can generate free fluoride ions at high temperature through gypsum calcium sulfate and ammonium fluoride, and the fluoride ions can greatly improve the lithium extraction efficiency of calcium sulfate as an auxiliary agent, thereby achieving a better lithium extraction effect than the prior art.

[0020] On the other hand, the negative monovalent F obtained by high temperature decomposition of ammonium fluoride - During high temperature roasting, it can replace the negative divalent O in the aluminosilicate structure in lithium ore. 2- , which causes the Al-O and Si-O bonds in the mineral structure to be destroyed. In order to maintain the electrical neutrality of the mineral, the excess positive one-valence Li + It will be "pushed out" of the lattice structure, making it susceptible to leaching.

[0021] Furthermore, the lithium ore includes one or more of lepidolite and lithium clay ore.

[0022] Furthermore, the lithium ore is crushed and ground to 200 mesh, accounting for 70% by mass.

[0023] Furthermore, the lithium ore, ammonium fluoride, and gypsum are mixed in a mass ratio of 0.5-2:0.05-0.1:1, and the calcium sulfate content of the gypsum is 75-85%. If the gypsum dosage is too low, the reaction cannot be complete, making it difficult to achieve efficient lithium extraction; if the gypsum dosage is too high, the amount of lithium extraction tailings will be too large, resulting in high processing costs.

[0024] Furthermore, polyacrylamide is used as a granulating agent in the granulation process, and the amount of the granulating agent is 1-2 wt% of the lithium ore. The viscosity of polyacrylamide can ensure uniform mixing of materials, and it volatilizes during high-temperature roasting, generating no or small amounts of impurities.

[0025] Furthermore, the particle size of the granulation balls is 5-10 mm.

[0026] Furthermore, the calcination temperature is 800-1100° C., and the calcination time is 1-4 hours.

[0027] When the temperature is too low or the roasting time is too short, the reaction is incomplete. As the temperature rises, the reaction between the lithium ore and gypsum becomes more complete, and the lithium leaching rate increases. When the roasting temperature is too high, the clinker partially sinters, and the sintered parts are difficult to break up, making it difficult to release the lithium during the leaching process, resulting in a lower lithium leaching rate.

[0028] Furthermore, the granulated pellets are calcined in a muffle furnace, and the mesh size of the calcined product is less than 100 meshes. Controlling the particle size of the calcined product within a reasonable range is beneficial to improving the leaching efficiency.

[0029] Furthermore, the leaching agent is water, and the volume ratio of the calcined product to the leaching agent is 1:2-4.

[0030] Furthermore, the leaching temperature is 30-90° C., the leaching time is 30-60 min, and a lithium-containing leaching solution is obtained. The leached residue is used as a cement admixture or a concrete admixture.

[0031] Controlling the liquid-to-solid ratio, leaching temperature, and leaching time during the leaching process can effectively improve leaching efficiency. A low liquid-to-solid ratio, low leaching temperature, or short leaching time will reduce leaching efficiency. A high liquid-to-solid ratio, high leaching temperature, or long leaching time will increase leaching process costs.

[0032] The leached residue is used as cement admixture or concrete admixture.

[0033] The beneficial effects of the present invention are:

[0034] (1) Waste gypsum is an industrial by-product. Using it to extract lithium resources realizes the recycling of waste, conforms to the principle of sustainable development, and promotes the development of the green economy.

[0035] (2) The comprehensive utilization of waste gypsum and lithium ore can reduce the discharge and storage of waste, reduce the risk of pollution to soil, water sources and atmosphere, and is beneficial to the environment;

[0036] (3) The use of waste gypsum, ammonium fluoride and lithium ore to extract lithium in a coordinated manner can reduce the purchase of sulfate raw materials. Through the special effects of gypsum and ammonium fluoride, free fluoride ions can be generated at high temperatures. Fluoride ions can greatly improve the efficiency of lithium extraction using calcium sulfate as an auxiliary agent, thereby achieving a better lithium extraction effect than the existing technology; reducing production costs and improving economic benefits; the method is mature, low-cost and has strong system adaptability. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. The drawings described below are merely embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying any creative work.

[0038] Figure 1 This is a schematic diagram of the process of collaborative lithium extraction using ammonium fluoride, gypsum and lithium ore provided in an embodiment of the present invention. DETAILED DESCRIPTION

[0039] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0040] It should be noted that the following detailed descriptions are exemplary and intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which the present invention belongs.

[0041] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit the exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is intended to include the plural form. In addition, it should be understood that when the terms "comprise" and / or "include" are used in this specification, they indicate the presence of features, steps, operations and / or combinations thereof.

[0042] Example 1:

[0043] according to Figure 1 As shown, lithium extraction operation of lithium ore is carried out:

[0044] 100g of lithium clay ore was crushed and ground to a 200-mesh size, accounting for 70% by weight. The main components of the lithium clay ore are 0.58% Li2O, 40.48% SiO2, 20.36% Al2O3, and 20.52% CaO. 50g of waste gypsum and 2.5g of ammonium fluoride were added and mixed thoroughly. Polyacrylamide was used as a granulating agent to prepare a spherical material with a particle size of 10mm. The material was calcined in a muffle furnace at 800°C for 1 hour. After calcination, the calcined material was cooled to 100°C and ball-milled to a size of less than 100 mesh. The ball-milled material was then placed in a 1L aqueous solution (calcined material: leaching agent ratio of 1:4 by volume) at 30°C and stirred at a constant speed for 30 minutes. The leaching solution is then obtained by filtration. The leaching residue is calcium aluminosilicate, which can be used as a cement admixture. After testing and analysis, the lithium extraction rate of Example 1 is 92.4%.

[0045] This technical solution demonstrates the synergistic lithium extraction using waste gypsum, ammonium fluoride, and lithium clay ore. The waste gypsum reacts with the lithium clay ore, solidifying the free silica in the clay ore sample and releasing sulfur dioxide. The sulfur dioxide then reacts with the lithium in the lithium-containing silicate to form soluble lithium sulfate. The free fluoride ions generated by the ammonium fluoride at high temperatures further increase the lithium extraction efficiency, resulting in a lithium ore extraction rate of 92.4%. The chemical composition of the waste gypsum used is shown in Table 1.

[0046] Table 1 Chemical composition of waste gypsum

[0047]

[0048] Example 2:

[0049] according to Figure 1 As shown, lithium extraction operation of lithium ore is carried out:

[0050] 100g of lithium clay ore was crushed and ground to a 200-mesh size of 70% by weight. The main components of the lithium clay ore are 0.58% Li2O, 40.48% SiO2, 20.36% Al2O3, and 20.52% CaO. 200g of waste gypsum and 20g of ammonium fluoride were added and mixed thoroughly. Polyacrylamide was used as a granulating agent to prepare a 5mm spherical material. The material was calcined in a muffle furnace at 1100°C for 4 hours. After calcination, the calcined material was cooled to 100°C and ball-milled to a size of less than 100 mesh. The ball-milled material was then placed in a 1.2L aqueous solution (calcined material: leaching agent ratio of 1:2 by volume) at 90°C and stirred at a constant speed for 60 minutes. The leaching solution is then obtained by filtration. The leaching residue is calcium aluminosilicate, which can be used as a cement admixture. After testing and analysis, the lithium extraction rate of Example 2 is 97.1%.

[0051] This technical solution demonstrates the synergistic use of waste gypsum and lithium clay ore for lithium extraction. The gypsum reacts with the lithium clay ore, solidifying the free silicon dioxide in the clay ore sample and releasing sulfur dioxide. The sulfur dioxide then reacts with the lithium in the lithium-containing silicate to form soluble lithium sulfate. The free fluoride ions generated by ammonium fluoride at high temperatures further increase the lithium extraction efficiency, resulting in a lithium ore extraction rate of 97.1%. The chemical composition of the gypsum used is shown in Table 2.

[0052] Table 2 Chemical composition of waste gypsum

[0053]

[0054] Comparative Example 1:

[0055] As a comparison benchmark with Example 1, ammonium fluoride was removed.

[0056] Take 100g of lithium clay ore, crush it and grind it to 200 mesh, accounting for 70% by mass. Add 50g of waste gypsum and mix evenly. Use polyacrylamide as the granulating agent to prepare a spherical material with a particle size of 10mm. The material is placed in a muffle furnace for high-temperature roasting, the roasting temperature is set to 800℃, and the roasting time is 4h. After roasting, the roasted material is cooled to 100℃ and ball-milled to less than 100 mesh. Then all the ball-milled fines are placed in a 1L volume, 30℃ temperature aqueous solution and stirred at a constant speed for 30min. Then, the leachate is obtained by filtration. After testing and analysis, the lithium extraction rate of Comparative Example 1 is 22.3%.

[0057] Comparative Example 2:

[0058] As a comparison benchmark with Example 2, ammonium fluoride was removed.

[0059] 100g of lithium clay ore was crushed and ground to 200 mesh, accounting for 70% by mass. 200g of waste gypsum was added and mixed evenly. Polyacrylamide was used as a granulating agent, and the mixture was prepared into a spherical material with a particle size of 5mm. The material was placed in a muffle furnace for high-temperature roasting at 1100°C for 4 hours. After roasting, the roasted material was cooled to 100°C and ball-milled to less than 100 mesh. Then, all the ball-milled fines were placed in a 1.2L aqueous solution at 90°C and stirred at a constant speed for 30 minutes. The leachate was then filtered to obtain a leachate. After testing and analysis, the lithium extraction rate of Comparative Example 2 was 67.4%.

[0060] Comparative Example 3:

[0061] As a comparison benchmark with Example 1, the waste gypsum was replaced with calcium sulfate and the ammonium fluoride was removed.

[0062] Take 100g of lithium clay ore, crush it and grind it to 200 mesh, accounting for 70% by mass. Add 50g of calcium sulfate and mix well. Use polyacrylamide as a granulating agent to prepare a spherical material with a particle size of 10mm. The material is placed in a muffle furnace for high-temperature roasting, the roasting temperature is set to 800℃, and the roasting time is 4h. After roasting, the roasted material is cooled to 100℃ and ball-milled to less than 100 mesh. Then all the ball-milled fines are placed in a 1L aqueous solution at a temperature of 30℃ and stirred at a constant speed for 30min. Then, the leachate is obtained by filtration. After testing and analysis, the lithium extraction rate of Comparative Example 3 is 23.7%.

[0063] Comparative Example 4:

[0064] As a comparison benchmark with Example 2, the waste gypsum was replaced with calcium sulfate and the ammonium fluoride was removed.

[0065] Take 100g of lithium clay ore and crush it to 200 mesh, accounting for 70% by mass. Add 200g of calcium sulfate and mix well. Use polyacrylamide as a granulating agent to prepare a spherical material with a particle size of 5mm. The material is placed in a muffle furnace for high-temperature roasting, the roasting temperature is set to 1100℃, and the roasting time is 4h. After roasting, the roasted material is cooled to 100℃ and ball-milled to less than 100 mesh. Then all the ball-milled fines are placed in a 1L aqueous solution at a temperature of 90℃ and stirred at a constant speed for 30min. The leachate is then filtered to obtain a leachate. After testing and analysis, the lithium extraction rate of Comparative Example 4 is 67.4%.

[0066] Comparative Example 5:

[0067] As a comparison benchmark with Example 1, the waste gypsum was replaced with calcium sulfate and the ammonium fluoride was removed.

[0068] Take 100g of lithium clay ore, crush it and grind it to 200 mesh, accounting for 70% by mass. Add 50g of calcium sulfate and mix well. Use polyacrylamide as the granulating agent to prepare a spherical material with a particle size of 10mm. The material is placed in a muffle furnace for high-temperature roasting. The roasting temperature is set to 1100℃ and the roasting time is 4h. After roasting, the roasted material is cooled to 100℃ and ball-milled to less than 100 mesh. Then all the ball-milled fine materials are placed in a 1L aqueous solution at a temperature of 30℃ and stirred at a constant speed for 30min. Then, the leachate is obtained by filtration. After testing and analysis, the lithium extraction rate of Comparative Example 5 is 55.9%.

[0069] In summary, the present invention discloses a method for collaboratively extracting lithium using ammonium fluoride, gypsum and lithium ore, the method comprising the following steps: first, crushing the lithium ore to be extracted; second, uniformly mixing the lithium ore obtained by the crushing with ammonium fluoride and gypsum, and granulating; then, placing the granulated balls in a muffle furnace for high-temperature roasting; finally, leaching the calcined product with water, and obtaining a lithium-containing mother liquor as the filtrate; the method effectively solves the problems of gypsum treatment and lithium ore resource development, utilizes ammonium fluoride and gypsum, creatively achieves a high lithium recovery rate, low costs in the lithium extraction process, and a simple process, plays an important role in waste resource utilization and efficient development and utilization of lithium resources, and has broad application prospects.

[0070] At this point, those skilled in the art will recognize that, although the embodiments of the present invention have been shown and described in detail herein, many other variations or modifications consistent with the principles of the present invention may be directly determined or derived from the disclosure of the present invention without departing from the spirit and scope of the present invention. Therefore, the scope of the present invention should be understood and deemed to cover all such other variations or modifications.

Claims

1. A method for extracting lithium by synergistic use of ammonium fluoride, gypsum and lithium ore, characterized in that: The lithium extraction method comprises the following steps: Step S1: crushing the lithium ore to be extracted; Step S2: uniformly mixing the crushed lithium ore obtained in step S1 with ammonium fluoride and gypsum, and granulating the mixture; Step S3: calcining the granulated pellets in step S2 at high temperature to obtain a calcined product; Step S4: The calcined product obtained in step S3 is leached with a leaching agent, the filtrate is a lithium-containing mother liquor, and the leached residue is a filler.

2. A method for extracting lithium by synergistic use of ammonium fluoride, gypsum and lithium ore as claimed in claim 1, characterized in that: The lithium ore includes one or more of lithium mica and lithium clay ore.

3. A method for extracting lithium by synergistic use of ammonium fluoride, gypsum and lithium ore as claimed in claim 1, characterized in that: The lithium ore is crushed and ground to 200 meshes, accounting for 70% by weight.

4. A method for extracting lithium by synergistic use of ammonium fluoride, gypsum and lithium ore as claimed in claim 1, characterized in that: The mixing mass ratio of the lithium ore, ammonium fluoride and gypsum is 0.5-2:0.05-0.1:1, and the calcium sulfate content in the gypsum is 75-85%.

5. The method for extracting lithium by synergistic use of ammonium fluoride, gypsum and lithium ore as claimed in claim 1, characterized in that: The granulation adopts polyacrylamide as a granulating agent, and the dosage of the granulating agent is 1-2wt% of the lithium ore.

6. A method for extracting lithium by synergistic use of ammonium fluoride, gypsum and lithium ore as claimed in claim 1, characterized in that: The particle size of the granulated balls is 5-10 mm.

7. A method for extracting lithium by synergistic use of ammonium fluoride, gypsum and lithium ore as claimed in claim 1, characterized in that: The calcination temperature is 800-1100° C., and the calcination time is 1-4 hours.

8. A method for extracting lithium by synergistic use of ammonium fluoride, gypsum and lithium ore as claimed in claim 1, characterized in that: The granulated balls are calcined in a muffle furnace, and the mesh number of the calcined product is less than 100 meshes.

9. A method for extracting lithium by synergistic use of ammonium fluoride, gypsum and lithium ore as claimed in claim 1, characterized in that: The leaching agent is water, and the volume ratio of the calcined product to the leaching agent is 1:2-4.

10. A method for extracting lithium by synergistic use of ammonium fluoride, gypsum and lithium ore as claimed in claim 1, characterized in that: The leaching temperature is 30-90° C., the leaching time is 30-60 min, and a lithium-containing leaching solution is obtained. The leached residue is used as a cement admixture or a concrete admixture.

Citation Information

Cited By

  • Method for extracting lithium, rubidium and cesium from lepidolite by using acidic fluorgypsum

    CN121450955A