Monocrystalline silicon texturing additive and preparation process thereof

By introducing a composite material composed of nano-silica and tetraethoxysilane into the monocrystalline silicon texturing additive, a nanocomposite film is formed to fill the micropores and micro-protrusions of the pyramid structure, which solves the problem of monocrystalline silicon texturing additive. The problem of high reflectivity under large-angle incident light improves the light absorption efficiency of photovoltaic cells.

CN118773748APending Publication Date: 2024-10-15JIANGSU XIANSHUAI TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410809199.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Existing monocrystalline silicon texturing additives increase the reflectivity when light is incident at a larger angle, affecting the performance of photovoltaic cells, and the common pyramid structure weakens the light absorption efficiency when reflected multiple times.

Method used

A monocrystalline silicon texturing additive composed of hypochlorite, surfactant, ethylenediaminetetraacetic acid, hydroxypropyl methylcellulose and siloxane nanocomposite is used to fill the surface of the silicon wafer by forming a nanocomposite film. Nano-silica increases surface roughness and scattering effects.

Benefits of technology

It effectively reduces the light reflectivity, especially when incident at a larger angle, and improves the light absorption efficiency of monocrystalline silicon cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118773748A_ABST
    Figure CN118773748A_ABST
Patent Text Reader

Abstract

The invention discloses a monocrystalline silicon texturing additive which is prepared from the following raw materials in percentage by weight: 0.1%-10% of pypocholoride, 0.01%-1% of a surfactant, 0.1%-1% of ethylenediamine tetraacetic acid, 0.001%-0.1% of hydroxypropyl methyl cellulose, 5.5%-17% of a siloxane nano composite material and the balance of deionized water. According to the monocrystalline silicon texturing additive provided by the invention, the viscosity and the stability of texturing liquid can be improved through the hydroxypropyl methyl cellulose and the siloxane nano composite material, and a layer of nano composite film can be formed on the surface of a silicon wafer through the introduction of the nano silicon dioxide and the tetraethoxysilane; the nano silicon dioxide in the nano composite film can be filled between the micropores and the micro bulges of the pyramid structure, so that the roughness and the scattering effect of the surface are further improved, the surface reflectivity can be more effectively reduced, particularly, the nano composite film has good anti-reflection performance under low-angle incident light, and the surface reflectivity is further reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of photovoltaic additives, and in particular to a single crystal silicon texturing additive and a preparation process thereof. Background Art

[0002] Monocrystalline silicon texturing additive is a chemical mixture specially used to improve the texture structure of monocrystalline silicon surface. Texturing is a key step in processing monocrystalline silicon wafers in the photovoltaic industry. By forming tiny texture structures on the surface of silicon wafers, it can reduce light reflection and improve light absorption efficiency. Texturing additives help form fine texture on the surface of monocrystalline silicon wafers through chemical reactions and physical effects.

[0003] Common monocrystalline silicon texturing additives will generate a delicate and randomly distributed pyramid-shaped structure when applied on the wafer. The reflectivity of the pyramid-shaped structure is generally 15%-20%. However, when light is incident at a larger angle (close to perpendicular to the silicon wafer surface), the multiple reflection effect of the pyramid-shaped structure is weakened, resulting in more direct reflection of light, increasing the reflectivity, and thus affecting the photoelectric conversion efficiency and reducing the performance of photovoltaic cells. Summary of the invention

[0004] The object of the present invention is to provide a single crystal silicon texturing additive and a preparation process thereof to solve the problems raised in the above background technology.

[0005] To achieve the above-mentioned purpose, the present invention provides the following technical scheme: a single crystal silicon texturing additive, composed of the following raw materials in weight percentage: 0.1% hypochlorite, 0.01% surfactant, 0.1% ethylenediaminetetraacetic acid, 0.001% hydroxypropyl methylcellulose, 5.5% silicone nanocomposite material, and the balance is deionized water.

[0006] Preferably, the siloxane nanocomposite material is composed of the following raw materials in weight percentage: 0.5% tetraethoxysilane, 5% nano-silicon dioxide, and the remainder is ethanol.

[0007] Preferably, the surfactant is selected from one of polyethylene glycol octylphenyl ether, polyoxyethylene ether and triethanolamine.

[0008] The present invention also provides a method for preparing a single crystal silicon texturing additive, comprising the following steps:

[0009] S1, taking 0.1%-10% hypochlorite, 0.01%-1% surfactant, 0.1%-1% ethylenediaminetetraacetic acid, 0.001%-0.1% hydroxypropyl methylcellulose and 5.5%-17% silicone nanocomposite material, adding them into the remaining amount of deionized water according to weight percentage, and uniformly mixing to obtain a single crystal silicon texturing additive;

[0010] S2, preparing a 1.0-2.0wt% sodium hydroxide (NaOH) or potassium hydroxide (KOH) aqueous solution to obtain an alkaline solution, and mixing the additive into the alkaline solution in proportion to obtain a first texturing solution;

[0011] S3, taking 0.5%-2% tetraethoxysilane (TEOS) and 5%-15% nano-silicon dioxide, adding them to the remaining ethanol according to weight percentage, and mixing them evenly to obtain a siloxane nano-composite material;

[0012] S4, repeating steps S1-S2 to obtain a second texturing solution, and adding single crystal silicon to the second texturing solution to uniformly mix the siloxane nanocomposite material;

[0013] S5, immersing the manufactured single crystal silicon wafer into the first texturing liquid for texturing, and then transferring the wafer to a water tank for cleaning;

[0014] S6, immersing the cleaned single crystal silicon wafer into the second texturing liquid for texturing, and then transferring it to a water tank for cleaning.

[0015] Preferably, in S3, the temperature during preparation of the siloxane nanocomposite material is 20°C-25°C.

[0016] Preferably, the mass ratio of the single crystal silicon texturing additive to the alkaline solution is 0.3-0.8:100.

[0017] Preferably, the temperature of the first texturing liquid and the second texturing liquid is 70° C.-80° C., and the single crystal silicon wafer is immersed in the first texturing liquid and the second texturing liquid for 15-20 minutes respectively.

[0018] Preferably, the single crystal silicon wafer is cleaned with deionized water.

[0019] Compared with the prior art, the beneficial effects of the present invention are as follows: the single crystal silicon texturing additive provided by the present invention can form a layer of nano-composite film on the surface of the silicon wafer by introducing a composite material composed of nano-silicon dioxide and tetraethoxysilane, and the nano-silicon dioxide in the nano-composite film can fill in the micropores and micro-protrusions of the pyramid structure, further increasing the surface roughness and scattering effect, helping to more effectively reduce the surface reflectivity, especially having good reflectivity under light incident at a larger angle, further improving the light absorption efficiency of the single crystal silicon cell. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a scanning electron microscope image of a single crystal silicon wafer after texturing with a single crystal silicon texturing additive according to Example 1 of the present invention;

[0021] Figure 2 This is a scanning electron microscope image of a single crystal silicon wafer after texturing with the single crystal silicon texturing additive in Example 4 of the present invention. DETAILED DESCRIPTION

[0022] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0023] Embodiment 1

[0024] See also Figure 1-Figure 2 An embodiment of the present invention provides a single crystal silicon texturing additive, which is composed of the following raw materials in weight percentage: 0.1%-10% hypochlorite, 0.01%-1% surfactant, 0.1%-1% ethylenediaminetetraacetic acid, 0.001%-0.1% hydroxypropyl methylcellulose, 5.5%-17% silicone nanocomposite material, and the balance is deionized water, wherein the silicone nanocomposite material is composed of the following raw materials in weight percentage: 0.5%-2% tetraethoxysilane, 5%-15% nano-silicon dioxide, and the balance is ethanol.

[0025] Furthermore, the surfactant is selected from one of polyethylene glycol octylphenyl ether, polyoxyethylene ether, and triethanolamine.

[0026] This embodiment also provides a method for preparing a single crystal silicon texturing additive, comprising the following steps:

[0027] S1, taking 0.1%-10% hypochlorite, 0.01%-1% surfactant, 0.1%-1% ethylenediaminetetraacetic acid, 0.001%-0.1% hydroxypropyl methylcellulose and 5.5%-17% silicone nanocomposite material, adding them into the remaining amount of deionized water according to weight percentage, and uniformly mixing to obtain a single crystal silicon texturing additive;

[0028] S2, preparing a 1.0-2.0wt% sodium hydroxide (NaOH) or potassium hydroxide (KOH) aqueous solution to obtain an alkaline solution, and mixing the additive into the alkaline solution in proportion to obtain a first texturing solution;

[0029] S3, taking 0.5%-2% tetraethoxysilane (TEOS) and 5%-15% nano-silicon dioxide, adding them to the remaining ethanol according to weight percentage, and uniformly mixing to obtain a siloxane nano-composite material, and the temperature during the preparation of the siloxane nano-composite material is 20° C.-25° C.;

[0030] S4, repeating steps S1-S2 to obtain a second texturing solution, and adding single crystal silicon to the second texturing solution to uniformly mix the siloxane nanocomposite material;

[0031] S5, immersing the manufactured single crystal silicon wafer into the first texturing liquid for texturing, and then transferring the wafer to a water tank for cleaning;

[0032] S6. Immerse the cleaned single crystal silicon wafer in a second texturing liquid for texturing, and transfer it to a water tank for cleaning after texturing.

[0033] S7. The temperature of the first texturing liquid and the second texturing liquid is 70° C.-80° C., and the single crystal silicon wafer is immersed in the first texturing liquid and the second texturing liquid for 15-20 minutes respectively.

[0034] In order to ensure the texturing effect and reduce equipment corrosion, the mass ratio of single crystal silicon texturing additive to alkaline solution is 0.3-0.8:100.

[0035] Specifically, deionized water is used to clean the monocrystalline silicon wafers. The alkaline solution and texturing liquid used in the texturing process of the monocrystalline silicon wafers will leave chemical residues on the surface of the silicon wafers. Deionized water can effectively remove the chemical residues.

[0036] Embodiment 2

[0037] See also Figure 1-Figure 2 An embodiment of the present invention provides a single crystal silicon texturing additive, which is composed of the following raw materials in weight percentage: 2% hypochlorite, 0.2% surfactant, 0.3% ethylenediaminetetraacetic acid, 0.02% hydroxypropyl methylcellulose, 9% silicone nanocomposite material, and the balance is deionized water, wherein the silicone nanocomposite material is composed of the following raw materials in weight percentage: 0.85% tetraethoxysilane, 8% nano-silicon dioxide, and the balance is ethanol.

[0038] Furthermore, the surfactant is polyethylene glycol octylphenyl ether.

[0039] Embodiment 3

[0040] See also Figure 1-Figure 2 An embodiment of the present invention provides a single crystal silicon texturing additive, which is composed of the following raw materials in weight percentage: 4% hypochlorite, 0.4% surfactant, 0.5% ethylenediaminetetraacetic acid, 0.05% hydroxypropyl methylcellulose, 9% silicone nanocomposite material, and the balance is deionized water, wherein the silicone nanocomposite material is composed of the following raw materials in weight percentage: 1% tetraethoxysilane, 12% nano-silicon dioxide, and the balance is ethanol.

[0041] Furthermore, the surfactant is polyoxyethylene ether.

[0042] Embodiment 4

[0043] See also Figure 1-Figure 2An embodiment of the present invention provides a single crystal silicon texturing additive, which is composed of the following raw materials in weight percentage: 4% hypochlorite, 0.4% surfactant, 0.5% ethylenediaminetetraacetic acid, 0.05% hydroxypropyl methylcellulose, 11% silicone nanocomposite material, and the balance is deionized water, wherein the silicone nanocomposite material is composed of the following raw materials in weight percentage: 0.5%-2% tetraethoxysilane, 5%-15% nano-silicon dioxide, and the balance is ethanol.

[0044] Embodiment 5

[0045] See also Figure 1-Figure 2 An embodiment of the present invention provides a single crystal silicon texturing additive, which is composed of the following raw materials in weight percentage: 4% hypochlorite, 0.4% surfactant, 0.5% ethylenediaminetetraacetic acid, 0.05% hydroxypropyl methylcellulose, 13% silicone nanocomposite material, and the balance is deionized water, wherein the silicone nanocomposite material is composed of the following raw materials in weight percentage: 0.5%-2% tetraethoxysilane, 5%-15% nano-silicon dioxide, and the balance is ethanol.

[0046] Furthermore, the surfactant is polyethylene glycol octylphenyl ether.

[0047] The single crystal silicon texturing additive raw materials provided in Examples 1 to 5 are selected, and the single crystal silicon texturing additive and the single crystal silicon wafer after texturing are prepared according to the preparation method of the single crystal silicon texturing additive provided in Example 1, and the single crystal silicon wafer after texturing is selected for experimental testing by electron microscope scanning observation.

[0048] Table 1 shows the experimental test results of single crystal silicon wafers after texturing:

[0049]

[0050]

[0051] By comparing the texture structures of Examples 1 to 5 and combining with Table 1, it can be found that the single crystal silicon texture additive prepared in Example 4 of the present application has excellent test results.

[0052] In summary: the single crystal silicon texturing additive provided by the present invention can form a layer of nano-composite film on the surface of the silicon wafer by introducing a composite material composed of nano-silicon dioxide and tetraethoxysilane. The nano-silicon dioxide in the nano-composite film can fill in the micropores and micro-protrusions of the pyramid structure, further increasing the surface roughness and scattering effect, helping to more effectively reduce the surface reflectivity, especially having good reflectivity under light incident at a larger angle, further improving the light absorption efficiency of the single crystal silicon cell.

[0053] Parts not involved in the present invention are the same as the prior art or can be implemented by the prior art. Although the embodiments of the present invention have been shown and described, it is understood by those skilled in the art that various changes, modifications, substitutions and variations can be made to these embodiments without departing from the principles and spirit of the present invention, and the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A single crystal silicon texturing additive, characterized in that: The invention is composed of the following raw materials in percentage by weight: 0.1%-10% of hypochlorite, 0.01%-1% of surfactant, 0.1%-1% of ethylenediaminetetraacetic acid, 0.001%-0.1% of hydroxypropylmethylcellulose, 5.5%-17% of silicone nanocomposite material, and the balance is deionized water.

2. The single crystal silicon texturing additive according to claim 1, characterized in that: The siloxane nano composite material is composed of the following raw materials in weight percentage: 0.5%-2% of tetraethoxysilane, 5%-15% of nano silicon dioxide, and the balance is ethanol.

3. The single crystal silicon texturing additive according to claim 1, characterized in that: The surfactant is selected from one of polyethylene glycol octylphenyl ether, polyoxyethylene ether and triethanolamine.

4. A method for preparing a single crystal silicon texturing additive, characterized in that: The following steps are involved: S1, taking 0.1%-10% hypochlorite, 0.01%-1% surfactant, 0.1%-1% ethylenediaminetetraacetic acid, 0.001%-0.1% hydroxypropyl methylcellulose and 5.5%-17% silicone nanocomposite material, adding them into the remaining amount of deionized water according to weight percentage, and uniformly mixing to obtain a single crystal silicon texturing additive; S2, preparing a 1.0-2.0wt% sodium hydroxide (NaOH) or potassium hydroxide (KOH) aqueous solution to obtain an alkaline solution, and mixing the additive into the alkaline solution in proportion to obtain a first texturing solution; S3, taking 0.5%-2% tetraethoxysilane (TEOS) and 5%-15% nano-silicon dioxide, adding them to the remaining ethanol according to weight percentage, and mixing them evenly to obtain a siloxane nano-composite material; S4, repeating steps S1-S2 to obtain a second texturing solution, and adding single crystal silicon to the second texturing solution to uniformly mix the siloxane nanocomposite material; S5, immersing the manufactured single crystal silicon wafer into the first texturing liquid for texturing, and then transferring the wafer to a water tank for cleaning; S6. Immerse the cleaned single crystal silicon wafer in a second texturing liquid for texturing, and transfer it to a water tank for cleaning after texturing.

5. The method for preparing a single crystal silicon texturing additive according to claim 1, characterized in that: In the step S3, the temperature during preparation of the siloxane nanocomposite material is 20°C-25°C.

6. The method for preparing a single crystal silicon texturing additive according to claim 4, characterized in that: The mass ratio of the single crystal silicon texturing additive to the alkaline solution is 0.3-0.8:

100.

7. The method for preparing a single crystal silicon texturing additive according to claim 6, characterized in that: The temperature of the first texturing liquid and the second texturing liquid is 70° C.-80° C., and the single crystal silicon wafer is immersed in the first texturing liquid and the second texturing liquid for 15-20 minutes respectively.

8. The method for preparing a single crystal silicon texturing additive according to claim 1, characterized in that: The single crystal silicon wafer is cleaned with deionized water.