Preparation method of super-hydrophilic polycaprolactone composite fiber

By preparing polycaprolactone and water-soluble polymers through emulsion electrospinning technology, the problem of poor wettability of polycaprolactone fibers in aqueous media has been solved, the preparation of super-hydrophilic fibers has been achieved, and its application fields have been expanded. and reduces production costs and environmental impact.

CN118773772APending Publication Date: 2024-10-15CHINA UNIV OF MINING & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410956469.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Polycaprolactone fiber prepared by traditional technology has poor wettability in aqueous media, which limits its application in biomedicine, food packaging, catalysis and other fields.

Method used

Emulsion electrospinning technology is used to mix polycaprolactone and water-soluble polymers, use ethyl acetate as the oil phase solvent, form a water-in-oil emulsion through stirring and emulsification, and use electrospinning technology to prepare super hydrophilic Polycaprolactone composite fiber.

Benefits of technology

The prepared fiber has super hydrophilicity, continuous shape, and uniform size distribution, which expands its application in biomedicine, food packaging, catalysis and other fields. The preparation process is gentle and environmentally friendly, and the operation is simple. It is suitable for mass production and avoids surface damage. Active agent residues and environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118773772A_ABST
    Figure CN118773772A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of super-hydrophilic polycaprolactone composite fibers, and belongs to the field of fiber preparation. Polycaprolactone and a water-soluble polymer are used as main raw materials, low-toxicity ethyl acetate is used as an oil-phase solvent, and the super-hydrophilic polycaprolactone composite fiber is prepared through an emulsion electrospinning technology. The method comprises the following steps: firstly, dissolving a water-soluble polymer in water to form a water phase; ethyl acetate is selected as an oil phase and is mixed with the water phase according to a certain proportion; adding polycaprolactone, stirring and emulsifying to obtain a water-in-oil emulsion; the polycaprolactone-water-soluble polymer composite fiber with regular morphology is prepared by adopting an electrostatic spinning technology. The method has the advantages of simple equipment and process, no need of adding any surfactant in the preparation process, good repeatability, low energy consumption and cost, and easy industrial production. The obtained composite fiber can be used in the fields of medicine transportation, tissue repair, food packaging, catalysis, adsorption and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a functional fiber and a preparation method thereof, in particular to a preparation method of a super-hydrophilic polycaprolactone composite fiber applicable to the technical field of fiber preparation. Background Art

[0002] Electrospinning is an important method for preparing fiber materials. It splits polymer solutions or melts into jets under the action of high-voltage electric field forces. These jets solidify due to the volatilization of solvents during flight, and eventually form fibers with diameters ranging from nanometers to micrometers. Fiber materials prepared by electrospinning technology have the advantages of large specific surface area, high porosity, controllable composition and structure, etc., so they are widely used in filtration, catalysis, biomedicine, and sensor protection. Research results in recent years have shown that composite fiber materials prepared by electrospinning technology not only overcome the performance defects of single materials, but also have a series of new and unique functions, so they have the potential to be applied in a wider range of fields.

[0003] Polycaprolactone (PCL) is a synthetic polymer material with good biocompatibility and biodegradability. It has been widely used in biomedicine, food packaging, environmental protection and other fields. However, since the PCL molecular chain is mainly composed of non-polar ester groups and methylene groups, the entire polymer chain exhibits strong hydrophobic properties, which limits its application in many applications. At present, there are several main ways to prepare hydrophilic PCL fibers: (1) Surface modification, that is, modifying the surface of PCL fibers by physical or chemical methods such as plasma treatment, ultraviolet light-induced graft polymerization, and chemical vapor deposition to introduce hydrophilic groups or polymer segments to improve their hydrophilicity. (2) Co-spinning, that is, co-spinning PCL with other hydrophilic polymer materials (such as polyvinyl alcohol, polyacrylic acid, etc.) to prepare hydrophilic composite fibers. (3) Forming nanocomposite materials, that is, compounding hydrophilic inorganic nanomaterials such as nano-silicon oxide and nano-aluminum oxide with PCL to prepare hydrophilic PCL composite fibers. However, the above method can usually only improve the hydrophilicity of PCL fibers to a certain extent, but it is difficult to achieve super-hydrophilicity. The present invention uses low-toxic ethyl acetate as an organic solvent, mixes and emulsifies PCL with a specific water-soluble polymer, and then uses emulsion electrospinning technology to obtain a super-hydrophilic PCL composite fiber. The content of the present invention is expected to greatly improve the application effect of PCL materials in the fields of biomedicine, environmental protection, food packaging, catalysis, adsorption, etc., and promote its application in more fields. Summary of the invention

[0004] Technical problem: The purpose of the present invention is to address the problem of poor wettability of polycaprolactone fibers prepared by traditional technology in aqueous media. By compounding with hydrophilic polymers, a method for preparing super hydrophilic polycaprolactone composite fibers using emulsion electrospinning technology is provided to solve the problems of strong hydrophobicity of polycaprolactone fibers and limited application areas.

[0005] Technical solution: A method for preparing a super-hydrophilic polycaprolactone composite fiber of the present invention uses polycaprolactone (PCL) and a water-soluble polymer as main raw materials and ethyl acetate as an oil phase solvent; dissolving the water-soluble polymer in water to form an aqueous phase; mixing the aqueous phase with the ethyl acetate oil phase in proportion; then adding PCL and stirring and emulsifying to obtain an oil-in-water emulsion; preparing a super-hydrophilic PCL-water-soluble polymer composite fiber by electrospinning technology; the specific steps are as follows:

[0006] (1) dissolving a water-soluble polymer in water to obtain an aqueous phase solution of the water-soluble polymer;

[0007] (2) mixing the aqueous phase solution with the ethyl acetate oil phase in proportion;

[0008] (3) adding PCL to step (2) at a certain temperature and stirring and emulsifying to obtain a water-in-oil emulsion;

[0009] (4) The water-in-oil emulsion obtained in step (3) is prepared into PCL-water-soluble polymer composite fibers by electrospinning technology.

[0010] In step (1), the water-soluble polymer is one or more of bovine serum albumin, Pluronic F127, and Pluronic F68.

[0011] In step (1), the water-soluble polymer is dissolved in water at a mass concentration of 1% to 30%.

[0012] In step (2), the volume ratio of the ethyl acetate oil phase and the aqueous phase solution is 3:1 to 20:1.

[0013] In step (3), the certain temperature is room temperature to 60°C.

[0014] In step (3), after adding PCL, the mass concentration of PCL in the water-in-oil emulsion obtained is 8% to 30%.

[0015] In step (3), the emulsification time is 1 min to 24 h, the emulsification speed is 500 to 20000 rpm, and no surfactant is required to be added during the emulsification process.

[0016] In step (4), a single needle is used in the electrospinning technology, and the needle model is 15-25G; the static voltage is 8-30kV, the injection speed of the obtained oil-in-water emulsion is 0.1-5mL / h, and the receiving distance of the fiber is 10-20cm.

[0017] In step (4), the diameter of the prepared PCL-soluble polymer composite fiber is in the range of 0.1 to 1.5 μm; the obtained composite fiber has a regular morphology, high dispersibility, and super hydrophilicity.

[0018] Beneficial effects: Due to the adoption of the above technical solution, the present invention overcomes the problems of strong hydrophobicity and limited application fields of PCL fibers of a single component or structure prepared by traditional technology, and provides a method for preparing super-hydrophilic polycaprolactone composite fibers by forming an emulsion with PCL and a water-soluble polymer using emulsion electrospinning technology. The PCL composite fibers prepared by the present invention have continuous morphology, uniform size distribution, and super-hydrophilicity, and can be used in the fields of drug transportation, tissue repair, food packaging, catalysis, adsorption, etc. The entire preparation process is gentle and environmentally friendly, simple to operate, has good repeatability, low energy consumption, and is suitable for mass production. Compared with the prior art, it has the following unique advantages:

[0019] (1) The present invention does not require the addition of additional surfactants, and a stable emulsion system can be formed solely by the surface activity of the water-soluble polymer itself. Therefore, compared with the traditional emulsion system containing surfactants such as Span 80, the present invention can avoid the negative effects caused by the residual surfactant, while saving costs and reducing environmental pollution.

[0020] (2) The present invention uses ethyl acetate as an organic solvent to prepare PCL composite fibers. Compared with the commonly used solvents such as dichloromethane, chloroform, trifluoroethanol, and hexafluoroisopropanol in the traditional method, ethyl acetate is cheap and easy to obtain, has low toxicity, and has little harm to the environment and human body. Moreover, ethyl acetate as an oil phase solvent can form a stable emulsion system with the water phase.

[0021] (3) The present invention obtains PCL composite fibers with super-hydrophilicity by compounding PCL with a hydrophilic polymer, which can effectively solve the problem of poor wettability of PCL materials in aqueous media, thereby expanding its application in the fields of biomedicine, food packaging, catalysis, adsorption, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a scanning electron microscope photograph of the super hydrophilic PCL composite fiber prepared in Example 1 of the present invention.

[0023] Figure 2 This is a transmission electron microscope photograph of the super hydrophilic PCL composite fiber prepared in Example 1 of the present invention.

[0024] Figure 3 This is a curve showing the change of the water contact angle of the super hydrophilic PCL composite fiber prepared in Example 1 of the present invention over time. DETAILED DESCRIPTION

[0025] The invention discloses a method for preparing a super-hydrophilic polycaprolactone composite fiber, comprising using polycaprolactone (PCL) and a water-soluble polymer as main raw materials and ethyl acetate as an oil phase solvent; dissolving the water-soluble polymer in water to form an aqueous phase; mixing the aqueous phase with an ethyl acetate oil phase in proportion; adding PCL thereto and stirring and emulsifying to obtain an oil-in-water emulsion; and preparing a super-hydrophilic PCL-water-soluble polymer composite fiber by using an electrostatic spinning technology. The specific steps are as follows:

[0026] (1) Dissolving a water-soluble polymer in water to obtain an aqueous phase solution of the water-soluble polymer; the water-soluble polymer is one or more of bovine serum albumin, Pluronic F127, and Pluronic F68; and the mass concentration of the water-soluble polymer is 1% to 30%.

[0027] (2) The aqueous phase solution is mixed with the ethyl acetate oil phase in proportion; the volume ratio of the oil phase and the aqueous phase solution is 3:1 to 20:1.

[0028] (3) At a certain temperature, adding PCL to step (2) and stirring and emulsifying to obtain an oil-in-water emulsion; the temperature is room temperature to 60° C.; the mass concentration of PCL in the oil-in-water emulsion obtained after adding PCL is 8% to 30%; the emulsification time is 1 min to 24 h; the emulsification speed is 500 to 20,000 rpm; and the emulsification process does not require the addition of any surfactant.

[0029] (4) The water-in-oil emulsion obtained in step (3) is made into PCL-water-soluble polymer composite fibers by electrospinning technology; a single needle is used in the electrospinning technology, and the needle model is 15-25G; the static voltage is 8-30kV, the injection speed of the obtained water-in-oil emulsion is 0.1-5mL / h, and the receiving distance of the fiber is 10-20cm. The diameter range of the PCL-water-soluble polymer composite fiber is 0.1-1.5μm; the obtained composite fiber has a regular morphology, high dispersibility, and super hydrophilicity.

[0030] The present invention will be further described below with reference to the embodiments in the accompanying drawings:

[0031] Example 1: Dissolve bovine serum albumin particles in water to prepare an aqueous solution, in which the mass concentration of BSA is 10%; mix ethyl acetate and the BSA aqueous solution in a volume ratio of 8:2; dissolve PCL particles in the above mixed solution at 37°C, and emulsify for 0.5h under stirring conditions of 1000rpm to form an oil-in-water emulsion, in which the mass concentration of PCL is 18%; transfer the spinning solution to a syringe with a 21G stainless steel needle, set the electrostatic field voltage to 15kV, the flow rate to 2mL / h, and the distance from the needle tip to the receiving plate to 15cm, and perform electrostatic spinning to obtain PCL-BSA composite fibers.

[0032] Experimental results: Figure 1 As shown, the PCL-BSA composite fibers obtained in Example 1 have a continuous and regular morphology, and no structural defects such as droplets and beads are observed in the product; the average diameter of the fiber is about 0.55 μm, and the diameter distribution range of the fiber is relatively narrow, mostly concentrated in the range of 0.2 to 0.8 μm. Figure 2 The transmission electron micrographs shown in the figure show that some of the composite fibers have a more obvious core-shell structure. In addition, the PCL-BSA composite fibers obtained in Example 1 exhibit strong superhydrophilicity. Figure 3 As shown in Figure 3, the initial contact angle of the fiber is 112°, which then decreases rapidly and is completely wetted by water at 5 s, with the contact angle becoming 0.

[0033] Example 2: Pluronic F127 particles were dissolved in water to prepare an aqueous solution, wherein the mass concentration of Pluronic F127 was 20%; ethyl acetate and the Pluronic F127 aqueous solution were mixed at a volume ratio of 15:1; PCL particles were dissolved in the above-mentioned mixed solution at 50°C, and emulsified at 2000rpm for 1h to form an oil-in-water emulsion, wherein the mass concentration of PCL was 12%; the spinning solution was transferred to a syringe with a 25G stainless steel needle, the electrostatic field voltage was set to 25kV, the flow rate was 4mL / h, and the distance from the needle tip to the receiving plate was 20cm, and electrospinning was performed to obtain PCL-Pluronic F127 composite fibers.

[0034] Example 3: Pluronic F68 particles were dissolved in water to prepare an aqueous solution, in which the mass concentration of Pluronic F68 was 30%; ethyl acetate and the Pluronic F68 aqueous solution were mixed at a volume ratio of 3:1; PCL particles were dissolved in the above mixed solution at room temperature, and emulsified for 2 minutes under stirring conditions of 18000 rpm to form an oil-in-water emulsion, in which the mass concentration of PCL was 25%; the spinning solution was transferred to a syringe with an 18G stainless steel needle, the electrostatic field voltage was set to 25 kV, the flow rate was 0.5 mL / h, and the distance from the needle tip to the receiving plate was 10 cm, and electrospinning was performed to obtain PCL-Pluronic F68 composite fibers.

Claims

1. A method for preparing a super-hydrophilic polycaprolactone composite fiber, characterized in that: Polycaprolactone (PCL) and a water-soluble polymer are used as main raw materials, and ethyl acetate is used as an oil phase solvent; the water-soluble polymer is dissolved in water to form an aqueous phase; the aqueous phase is mixed with the ethyl acetate oil phase in proportion; PCL is then added and stirred and emulsified to obtain an oil-in-water emulsion; and super-hydrophilic PCL-water-soluble polymer composite fibers are prepared by electrospinning technology; the specific steps are as follows: (1) dissolving a water-soluble polymer in water to obtain an aqueous phase solution of the water-soluble polymer; (2) mixing the aqueous phase solution with the ethyl acetate oil phase in proportion; (3) adding PCL to step (2) at a certain temperature and stirring and emulsifying to obtain a water-in-oil emulsion; (4) The water-in-oil emulsion obtained in step (3) is prepared into PCL-water-soluble polymer composite fibers by electrospinning technology.

2. The method for preparing a super-hydrophilic polycaprolactone composite fiber according to claim 1, characterized in that: In step (1), the water-soluble polymer is one or more of bovine serum albumin, Pluronic F127, and Pluronic F68.

3. The method for preparing a super-hydrophilic polycaprolactone composite fiber according to claim 1 or 2, characterized in that: In step (1), the water-soluble polymer is dissolved in water at a mass concentration of 1% to 30%.

4. The method for preparing a super-hydrophilic polycaprolactone composite fiber according to claim 1, characterized in that: In step (2), the volume ratio of the ethyl acetate oil phase and the aqueous phase solution is 3:1 to 20:

1.

5. The method for preparing a super-hydrophilic polycaprolactone composite fiber according to claim 1, characterized in that: In step (3), the certain temperature is room temperature to 60°C.

6. The method for preparing a super-hydrophilic polycaprolactone composite fiber according to claim 1, characterized in that: In step (3), after adding PCL, the mass concentration of PCL in the water-in-oil emulsion obtained is 8% to 30%.

7. The method for preparing a super-hydrophilic polycaprolactone composite fiber according to claim 1, characterized in that: In step (3), the emulsification time is 1 min to 24 h, the emulsification speed is 500 to 20000 rpm, and no surfactant is required to be added during the emulsification process.

8. The method for preparing a super-hydrophilic polycaprolactone composite fiber according to claim 1, characterized in that: In step (4), a single needle is used in the electrospinning technology, and the needle model is 15-25G; the static voltage is 8-30kV, the injection speed of the obtained oil-in-water emulsion is 0.1-5mL / h, and the receiving distance of the fiber is 10-20cm.

9. The method for preparing a super-hydrophilic polycaprolactone composite fiber according to claim 1, characterized in that: In step (4), the diameter of the prepared PCL-soluble polymer composite fiber is in the range of 0.1 to 1.5 μm; the obtained composite fiber has a regular morphology, high dispersibility, and super hydrophilicity.