High-temperature sodium ion electrolyte and high-safety sodium ion battery
By using propylene carbonate and additives such as fluorinated ethylene carbonate, hexamethylene diisocyanate and vinyl sulfate in high-temperature sodium-ion batteries to form a stable main solvation structure, the failure and failure of existing batteries in harsh environments are solved. Safety issues, improved high-temperature cycle and storage performance and high safety.
Patent Information
- Application Number
- CN202410957108.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-10-15
AI Technical Summary
The electrolyte of existing high-temperature sodium-ion batteries is prone to failure, fire or explosion in harsh environments, and has poor cycle performance. In addition, existing technologies mostly refer to lithium-ion battery systems, using compound organic solvents and using propylene carbonate alone as the electrolyte. Electrolytes are less technical.
Propylene carbonate is used as the non-aqueous organic solvent, combined with additives such as fluoroethylene carbonate, hexamethylene diisocyanate and vinyl sulfate, to form a stable main solvation structure of Na+-PC-DTD-FEC-HMDI-anion. Form a strong cathode electrolyte membrane and solid electrolyte membrane to improve the thermodynamic and electrochemical stability of sodium-ion batteries.
It improves the thermal stability and cycle performance of sodium-ion batteries, avoids the peeling phenomenon of the negative electrode layer caused by solvent co-intercalation decomposition, enhances high-temperature cycle and storage performance, and verifies its high safety through hot plate and thermal shock tests.
Smart Images

Figure BDA0004949176590000091 
Figure BDA0004949176590000092 
Figure BDA0004949176590000101
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sodium ion batteries, and more specifically, to a high-temperature sodium ion electrolyte and a high-safety sodium ion battery. Background Art
[0002] Sodium-ion batteries have similar physical and chemical properties to lithium batteries. Given the abundance of sodium resources and low cost, they are considered to be the most promising for large-scale energy storage, and high temperature, high safety, and long cycle performance have attracted widespread attention. In the sodium-ion battery system, the electrolyte plays a vital role as an intermediate bridge connecting the positive and negative electrode material systems. Ethylene carbonate (EC) is an organic solvent with excellent performance. As a non-protonic polar organic solvent, it has a high dielectric constant and can dissolve a variety of organic substances and inorganic salts. It is a widely used electrolyte solvent. However, its melting point is high (35-38°C), the liquid range is relatively narrow, and it is a crystalline solid at room temperature (25°C), which requires heating and melting before use. More importantly, ethylene carbonate is easily reduced, and its electrochemical stability is not high. The battery is prone to gasification when used in harsh environments, resulting in battery failure, fire, and even explosion. Propylene carbonate (PC), as a solvent similar to ethylene carbonate, has a high dielectric constant and strong dissolving ability. It also has the characteristics of low melting point, high boiling point, wide liquid temperature range, wide electrochemical window and good chemical stability. Using it as a solvent can improve the operating temperature range and safety of the battery, and has great application advantages in sodium-ion batteries.
[0003] However, most of the existing technologies refer to the lithium-ion battery system and use compound organic solvents as the electrolyte of high-temperature sodium-ion batteries, and very few technologies use propylene carbonate as a single solvent as the electrolyte. In addition, the existing technologies often need to add homemade special additives to the electrolyte in order to achieve better high-temperature cycle performance. Summary of the invention
[0004] In order to solve the above-mentioned defects of the prior art, the primary purpose of the present invention is to provide a high-temperature sodium ion electrolyte, which uses only propylene carbonate as a non-aqueous organic solvent, and forms a stable Na by reacting propylene carbonate with sodium ions and three commonly used additives in the art, FEC, HMDI, and DTD. + -PC-DTD-FEC-HMDI-FSI - The main solvation structure of the anion forms a strong and stable cathode electrolyte membrane (CEI) and solid electrolyte membrane (SEI) on the electrode surface. The main solvation structure forms a high-conductivity ion interface membrane component, which significantly improves the performance of sodium-ion batteries in terms of thermodynamics and electrochemical stability.
[0005] Another object of the present invention is to provide an application of the high-temperature sodium ion electrolyte in the preparation of a high-safety sodium ion battery.
[0006] Another object of the present invention is to provide a highly safe sodium ion battery.
[0007] The above-mentioned object of the present invention is achieved by the following technical solutions:
[0008] The present invention protects a high-temperature sodium ion electrolyte, characterized in that it includes a sodium salt, a non-aqueous organic solvent and an additive a;
[0009] The non-aqueous organic solvent is propylene carbonate;
[0010] The additive a is fluoroethylene carbonate (FEC), hexamethylene diisocyanate (HMDI) and diethylene sulfate (DTD).
[0011] The present invention uses only propylene carbonate as a non-aqueous organic solvent, and forms a stable Na by reacting propylene carbonate with sodium ions and three additives: FEC, HMDI and DTD. + -PC-DTD-FEC-HMDI - The main solvation structure of the anion makes the sodium ion battery highly thermally stable, forming a strong and stable cathode electrolyte membrane (CEI) and solid electrolyte membrane (SEI) on the electrode surface. Adjusting the structure and composition of the interface membrane significantly improves the overall performance of the sodium ion battery in terms of thermodynamics and electrochemical stability. Moreover, the pure propylene carbonate-based electrolyte and the soft carbon and hard carbon negative electrodes will not undergo solvent co-intercalation decomposition and cause the negative electrode layer to peel off, and the cycle performance is also guaranteed.
[0012] Preferably, the amount of the additive a is greater than 0.1 wt% and less than 30 wt%. More preferably, the amount of the additive a is greater than 2.0 wt% and less than 10 wt%. Further preferably, the amount of the additive a is greater than 2.0 wt% and less than 7 wt%.
[0013] Preferably, the mass ratio of fluoroethylene carbonate, hexamethylene diisocyanate and vinyl sulfate in the additive a is 1-15:0.2-3:0.3-5, more preferably 2-5:0.3-1:0.6-2.
[0014] Preferably, the total amount of the non-aqueous organic solvent and the additive a added is ≥40wt% and ≤97wt%. More preferably, the total amount of the non-aqueous organic solvent and the additive a added is ≥50wt% and ≤90wt%.
[0015] Preferably, the added amount of the sodium salt is 8-42 wt%.
[0016] Preferably, the sodium salt is selected from one or both of an inorganic sodium salt or an organic sodium salt. More preferably, the sodium salt is selected from sodium hexafluorophosphate (NaPF6), sodium perchlorate (NaClO4), sodium tetrafluoroborate (NaBF4), sodium hexafluoroarsenate (NaAsF6), sodium bis(trifluoromethylsulfonyl)imide (NaFSI), sodium fluoromalonate borate (NaBFMB), sodium bis(trifluoromethylsulfonyl)imide (NaTFSI), sodium bis(oxalatoborate) (NaBOB), sodium difluorooxalatoborate (NaODFB), sodium difluorophosphate (NaPO2F2) or one or more of the above sodium salt halogenated derivatives.
[0017] More preferably, the sodium salt is selected from one or two of sodium hexafluorophosphate, sodium bis(trifluoromethylsulfonyl)imide, sodium difluorophosphate and sodium bis(trifluoromethylsulfonyl)imide.
[0018] More preferably, the sodium salt is sodium hexafluorophosphate and sodium bis(fluorosulfonyl)imide. Specifically, the mass ratio of sodium hexafluorophosphate to sodium bis(fluorosulfonyl)imide is 4-9:3-7.
[0019] Preferably, the concentration of the sodium salt is 1M to 4M. More preferably, the concentration of the sodium salt is 1.2M to 3M.
[0020] Preferably, the high temperature sodium ion electrolyte further comprises an additive b.
[0021] Preferably, the auxiliary additive b is selected from one or more of vinylene carbonate, vinyl ethylene carbonate, tris(trimethylsilyl) phosphate, tris(trimethylsilyl) borate, 1,3-propane sultone, propenyl-1,3-propane sultone, pentafluoro(phenoxy)cyclotriphosphazene, tetrafluoroethyl tetrafluoropropyl ether, pyridine, ethylene glycol dibutyl ether, propylene sulfite, 4-methylethylene sulfate, succinonitrile, and adiponitrile.
[0022] More preferably, the co-additive b is selected from one of 1,3-propane sultone, pentafluoro(phenoxy)cyclotriphosphazene, tris(trimethylsilyl)borate, adiponitrile or a combination of vinylene carbonate and 1,3-propane sultone.
[0023] In the electrolyte system of the present invention, the auxiliary additive b can play a synergistic role with the additive a to improve the cycle performance and the residual recovery value of the sodium ion battery after high-temperature storage.
[0024] Preferably, the total amount of the additive a and the co-additive b added is >0.1wt% and ≤40wt%. More preferably, the total amount of the additive a and the co-additive b added is ≥2.0wt% and ≤10wt%.
[0025] Preferably, the total amount of the non-aqueous organic solvent, additive a and co-additive b added is ≥40wt% and ≤97wt%. More preferably, the total amount of the non-aqueous organic solvent, additive a and co-additive b added is ≥50wt% and ≤90wt%.
[0026] The present invention also protects the use of the above-mentioned high-temperature sodium ion battery in the preparation of high-safety sodium ion batteries.
[0027] The present invention also protects a high-safety sodium ion battery, comprising a positive electrode sheet, a negative electrode sheet, a diaphragm and the high-temperature sodium ion electrolyte.
[0028] Furthermore, the positive electrode plate includes a positive electrode active material, a conductive agent, and a binder.
[0029] Preferably, the positive electrode active material of the positive electrode plate is selected from one or more of layered oxide type, polyanion type, Prussian blue type and Prussian white type.
[0030] Preferably, the conductive agent of the positive electrode plate is selected from one or more of conductive graphite, carbon black, carbon fiber, carbon nanotubes, and graphene.
[0031] Preferably, the binder of the positive electrode plate is selected from one or more of polyvinylidene fluoride, polyacrylic acid, polyacrylonitrile, polyimide and polytetrafluoroethylene.
[0032] Furthermore, the negative electrode plate includes a negative electrode material, a conductive agent, and a binder.
[0033] Preferably, the negative electrode active material of the negative electrode plate is hard carbon or soft carbon.
[0034] Preferably, the conductive agent of the negative electrode plate is selected from one or more of conductive graphite, carbon black, carbon fiber, carbon nanotube and graphene.
[0035] Preferably, the binder of the negative electrode plate is selected from one or more of polyacrylic acid, polyacrylonitrile, sodium carboxymethyl cellulose, styrene-butadiene rubber, polyvinylidene fluoride and polytetrafluoroethylene.
[0036] Preferably, the diaphragm is selected from one of PP, PE, PP and PE multilayer composite diaphragm, ceramic layer modified diaphragm, PMMA coated diaphragm, aramid modified diaphragm, and oxide solid electrolyte coated diaphragm.
[0037] Compared with the prior art, the present invention has the following beneficial effects:
[0038] 1. The high-temperature sodium ion electrolyte provided by the present invention uses only propylene carbonate as a non-aqueous organic solvent. The electrolyte has the characteristics of high boiling point, wide liquid range and good stability. By compounding propylene carbonate with three additives FEC, HMDI and DTD, the overall performance of the sodium ion battery in terms of thermodynamics and electrochemical stability is improved.
[0039] 2. The high-temperature sodium ion electrolyte provided by the present invention and the commonly used sodium ion battery negative electrode (soft carbon, hard carbon) will not undergo solvent co-intercalation decomposition to cause the negative electrode layer to peel off, and the cycle performance is also guaranteed.
[0040] 3. The high-safety sodium ion battery prepared using the high-temperature sodium ion electrolyte prepared by the present invention has excellent high-temperature cycle and storage performance, and can withstand ultra-high temperature hot plate testing and thermal shock safety testing. DETAILED DESCRIPTION
[0041] In order to more clearly and completely describe the technical solution of the present invention, the present invention is further described in detail through specific embodiments below. It should be understood that the specific embodiments described herein are only used to explain the present invention, and are not used to limit the present invention. Various changes can be made within the scope of the rights of the present invention.
[0042] Example 1
[0043] A high-temperature sodium ion electrolyte comprises: a sodium salt of NaPF6, a sodium salt concentration of 1.2M, a non-aqueous organic solvent of propylene carbonate, an additive a of FEC, HMDI, and DTD, an auxiliary additive b of 1,3-propane sultone, the addition amounts of the sodium salt, the non-aqueous organic solvent, the additive a, and the auxiliary additive b are 16.8wt%, 74.88wt%, 6.656wt%, and 1.664wt% of the total mass of the high-temperature sodium ion electrolyte, and the mass ratio of fluoroethylene carbonate, hexamethylene diisocyanate, and vinyl sulfate in the additive a is 4.1:0.556:2.
[0044] Example 2
[0045] A high-temperature sodium ion electrolyte comprises: a sodium salt of NaFSI, a sodium salt concentration of 3M, a non-aqueous organic solvent of propylene carbonate, an additive a of FEC, HMDI, and DTD, an auxiliary additive b of pentafluoro(phenoxy)cyclotriphosphazene, the addition amounts of the sodium salt, the non-aqueous organic solvent, the additive a, and the auxiliary additive b are 42wt%, 54.23wt%, 2.9wt%, and 0.87wt% of the total mass of the high-temperature sodium ion electrolyte, and the mass ratio of fluoroethylene carbonate, hexamethylene diisocyanate, and vinyl sulfate in the additive a is 2:0.3:0.6.
[0046] Example 3
[0047] A high-temperature sodium ion electrolyte comprises: sodium salts of NaPF6 and NaFSI, the sodium salt concentration is 1.4M, the mass ratio of NaPF6 to NaFSI is 7:4, the non-aqueous organic solvent is propylene carbonate, the additive a is FEC, HMDI, DTD, the auxiliary additive b is tris(trimethylsilane) phosphate, the addition amounts of the sodium salt, the non-aqueous organic solvent, the additive a, and the auxiliary additive b are 19.6wt%, 73.968wt%, 5.628wt%, and 0.804wt% of the total mass of the high-temperature sodium ion electrolyte, and the mass ratio of fluoroethylene carbonate, hexamethylene diisocyanate, and vinyl sulfate in the additive a is 3:0.628:2.
[0048] Example 4
[0049] A high-temperature sodium ion electrolyte comprises: sodium salts of NaPO2F2 and NaFSI, the sodium salt concentration is 1.4M, the mass ratio of NaPO2F2 to NaFSI is 1:13, the non-aqueous organic solvent is propylene carbonate, the additive a is FEC, HMDI, and DTD, the auxiliary additive b is vinylene carbonate and 1,3-propane sultone, the addition amounts of the sodium salt, the non-aqueous organic solvent, the additive a, and the auxiliary additive b are 19.6wt%, 74.37wt%, 4.824wt%, and 1.206wt% of the total mass of the high-temperature sodium ion electrolyte, the mass ratio of fluoroethylene carbonate, hexamethylene diisocyanate, and vinyl sulfate in the additive a is 2:0.824:2, and the mass ratio of vinylene carbonate to 1,3-propane sultone in the auxiliary additive b is 0.206:1.
[0050] Example 5
[0051] A high-temperature sodium ion electrolyte comprises: sodium salts of NaFSI and NaTFSI, a sodium salt concentration of 1.2M, a mass ratio of NaFSI to NaTFSI of 2:1, a non-aqueous organic solvent of propylene carbonate, an additive a of FEC, HMDI, and DTD, an auxiliary additive b of adiponitrile, the addition amounts of the sodium salt, the non-aqueous organic solvent, the additive a, and the auxiliary additive b of the high-temperature sodium ion electrolyte are 16.8wt%, 78.208wt%, 4.576wt%, and 0.416wt% respectively of the total mass of the high-temperature sodium ion electrolyte, and the mass ratio of fluoroethylene carbonate, hexamethylene diisocyanate, and vinyl sulfate in the additive a is 2.5:0.576:1.5.
[0052] Example 6
[0053] A high-temperature sodium ion electrolyte comprises: a sodium salt of NaPF6, a sodium salt concentration of 1.2M, a non-aqueous organic solvent of propylene carbonate, an additive a of FEC, HMDI, and DTD, wherein the sodium salt, the non-aqueous organic solvent, and the additive a account for 16.8wt%, 76.544wt%, and 6.656wt% of the total mass of the high-temperature sodium ion electrolyte, respectively; and the mass ratio of fluoroethylene carbonate, hexamethylene diisocyanate, and vinyl sulfate in the additive a is 4.1:0.556:2.
[0054] Comparative Example 1
[0055] A sodium ion electrolyte comprises: a sodium salt of NaPF6, a sodium salt concentration of 1M, a non-aqueous organic solvent of propylene carbonate / dimethyl carbonate / propyl acetate, a mass ratio of propylene carbonate / dimethyl carbonate / propyl acetate of 20:30:50, an additive a of FEC, HMDI, and DTD, an auxiliary additive b of 1,3-propane sultone, and the addition amounts of the sodium salt, the non-aqueous organic solvent, the additive a, and the auxiliary additive b are 14wt%, 80.41wt%, 4.73wt%, and 0.86wt% of the total mass of the high-temperature sodium ion electrolyte, respectively; and the mass ratio of fluoroethylene carbonate, hexamethylene diisocyanate, and vinyl sulfate in the additive a is 3:0.53:1.2.
[0056] Comparative Example 2
[0057] A high-temperature sodium ion electrolyte comprises: a sodium salt of NaPF6, a sodium salt concentration of 1.2M, a non-aqueous organic solvent of propylene carbonate, an additive a of FEC, an auxiliary additive b of 1,3-propane sultone, and the addition amounts of the sodium salt, the non-aqueous organic solvent, the additive a, and the auxiliary additive b are 16.8wt%, 77.436wt%, 4.1wt%, and 1.664wt% of the total mass of the high-temperature sodium ion electrolyte.
[0058] Comparative Example 3
[0059] A high-temperature sodium ion electrolyte comprises: a sodium salt of NaPF6, a sodium salt concentration of 1.2M, a non-aqueous organic solvent of propylene carbonate, an additive a of DTD, an auxiliary additive b of 1,3-propane sultone, and the addition amounts of the sodium salt, the non-aqueous organic solvent, the additive a, and the auxiliary additive b are 16.8wt%, 79.536wt%, 2wt%, and 1.664wt% of the total mass of the high-temperature sodium ion electrolyte.
[0060] Comparative Example 4
[0061] A high-temperature sodium ion electrolyte comprises: a sodium salt of NaPF6, a sodium salt concentration of 1.2M, a non-aqueous organic solvent of propylene carbonate, an additive a of HMDI, an auxiliary additive b of 1,3-propane sultone, and the addition amounts of the sodium salt, the non-aqueous organic solvent, the additive a, and the auxiliary additive b are 16.8wt%, 80.98wt%, 0.556wt%, and 1.664wt% of the total mass of the high-temperature sodium ion electrolyte.
[0062] Comparative Example 5
[0063] A high-temperature sodium ion electrolyte comprises: a sodium salt of NaPF6, a sodium salt concentration of 1.2M, a non-aqueous organic solvent of propylene carbonate, an additive a of FEC and HMDI, an auxiliary additive b of 1,3-propane sultone, the addition amounts of the sodium salt, the non-aqueous organic solvent, the additive a, and the auxiliary additive b are 16.8wt%, 74.88wt%, 6.656wt%, and 1.664wt% of the total mass of the high-temperature sodium ion electrolyte, and the mass ratio of fluoroethylene carbonate to hexamethylene diisocyanate in the additive a is 4.1:0.556.
[0064] Comparative Example 6
[0065] A high-temperature sodium ion electrolyte comprises: a sodium salt of NaPF6, a sodium salt concentration of 1.2M, a non-aqueous organic solvent of propylene carbonate, an additive a of HMDI and DTD, an auxiliary additive b of 1,3-propane sultone, the addition amounts of the sodium salt, the non-aqueous organic solvent, the additive a, and the auxiliary additive b are 16.8wt%, 74.88wt%, 6.656wt%, and 1.664wt% of the total mass of the high-temperature sodium ion electrolyte, and the mass ratio of hexamethylene diisocyanate to vinyl sulfate in the additive a is 0.556:2.
[0066] Comparative Example 7
[0067] A high-temperature sodium ion electrolyte comprises: a sodium salt of NaPF6, a sodium salt concentration of 1.2M, a non-aqueous organic solvent of propylene carbonate, an additive a of FEC and DTD, an auxiliary additive b of 1,3-propane sultone, the addition amounts of the sodium salt, the non-aqueous organic solvent, the additive a, and the auxiliary additive b are 16.8wt%, 74.88wt%, 6.656wt%, and 1.664wt% of the total mass of the high-temperature sodium ion electrolyte, and the mass ratio of fluoroethylene carbonate to vinyl sulfate in the additive a is 4.1:2.
[0068] Performance Testing
[0069] 1. Prepare a high temperature sodium ion electrolyte, comprising the following steps:
[0070] In a glove box filled with argon, H2O<0.1ppm, O2<0.1ppm, add sodium salt to propylene carbonate as the non-aqueous organic solvent, stir evenly (if adding two sodium salts, add one sodium salt first, stir evenly, then add the other sodium salt, and stir evenly). After the sodium salt is completely dissolved, add additive a and co-additive b, stir evenly, and use The high temperature electrolyte is obtained after the molecular sieve is dried and filtered.
[0071] 2. Preparation of high-safety sodium-ion batteries
[0072] (1) Preparation of positive electrode sheets: The positive electrode active material (sodium ferric phosphate pyrophosphate), conductive agent (SP and CNT mass ratio is 1:1), binder (PVDF) and sodium ion conductive agent are weighed and mixed in a mass ratio of 93:2:3:2, and then added to N-methylpyrrolidone (NMP). The mixture is stirred evenly with a planetary mixer to obtain a positive electrode slurry. The positive electrode slurry is evenly coated on both sides of an aluminum foil with a coating machine. The positive electrode sheets are obtained after baking, rolling and slitting. Finally, the mixture is vacuum dried and set aside for use.
[0073] (2) Preparation of negative electrode sheets: negative electrode active material (hard carbon), conductive agent (SP), binder (CMC and SBR in a mass ratio of 1:1), and sodium ion conductive agent are weighed and mixed in a mass ratio of 92:3:3:2 and added into deionized water. The mixture is stirred evenly with a planetary mixer to obtain negative electrode slurry. The negative electrode slurry is evenly coated on both sides of an aluminum foil with a coating machine. The negative electrode sheets are obtained after baking, rolling, and slitting. The negative electrode sheets are then vacuum dried and set aside for use.
[0074] (3) High-safety sodium-ion battery assembly: The positive electrode sheet, separator and negative electrode sheet are wound to obtain a bare cell, which is then packaged to obtain a dry cell; a high-temperature sodium-ion electrolyte is injected into the dry cell, and a high-safety sodium-ion battery is obtained through formation and capacity separation.
[0075] 3. High temperature cycle test:
[0076] After the battery was placed in a constant temperature oven at 45℃ / 60℃ for 3h, it was charged to 3.45V at 1C constant current, then charged to 0.05C at constant voltage, and then discharged to 1.5V at 1C constant current, and the cycle was repeated. The initial capacity of the battery and the discharge capacity of the last cycle (800th cycle) were recorded. Capacity retention rate = discharge capacity of the last cycle (800th cycle) / initial capacity × 100%.
[0077] 4.85℃ high temperature storage test:
[0078] Standard charge: Charge the battery at 25°C at a constant current of 0.5C to 3.45V, cut off at 0.02C, and then discharge at a constant current of 0.2C to 1.5V. Record the initial thickness, initial capacity and internal resistance R1 of the battery cell.
[0079] Charge to 3.45V with standard method, place in an oven at a constant temperature of 85℃ for 28 days, wait for the battery to cool to room temperature, and measure the cell thickness and internal resistance R2 after 28 days. The capacity discharged to 1.5V at 0.2C current is recorded as the remaining capacity. Charge the stored cell to 3.45V at 0.5C constant current, cut off at 0.02C, and then discharge to 1.5V at 0.2C constant current, which is recorded as the recovered capacity.
[0080] Residual value = remaining capacity / initial capacity × 100%,
[0081] Recovery value = recovery capacity / initial capacity × 100%,
[0082] Thickness expansion rate = (thickness after storage - thickness before storage) / thickness before storage × 100%,
[0083] Internal resistance growth rate=(internal resistance after storage-internal resistance before storage) / internal resistance before storage×100%.
[0084] 5. Hot plate safety test:
[0085] At 25°C, charge the battery cell at 1C to 3.45V and cut off at 0.02C. Then place the battery cell on the graphene heating plate and heat it until the temperature at the bottom of the battery cell reaches about 300°C. Keep it above 300°C for 30 to 40 minutes, observe the voltage changes and whether the battery cell expands or fails.
[0086] 6. Thermal shock safety test:
[0087] At 25℃, charge the battery cell at 1C to 3.45V and cut off at 0.02C. Then place the fully charged battery cell in an air circulation heating furnace with an initial temperature of 25±3℃, and heat it to 180±2℃ at a heating rate of 5±2℃ / min and maintain it for 30min. It passes the test if there is no fire or explosion.
[0088] Table 1 High temperature cycle and storage performance
[0089]
[0090] Table 2 Hot plate, thermal shock safety test
[0091]
[0092]
[0093] It can be seen from the data in Table 1 that the embodiments all show better high-temperature cycle and high-temperature storage performance, while the thickness of the comparative example expands greatly and produces gas; it can be seen from the test results in Table 2 that after the high-temperature hot plate and thermal shock tests, the voltage of the embodiments is still stable at 3.39V and above, and the battery cell has not failed, while the voltage of the comparative example has dropped to 0V and the battery cell has expanded and smoked, and the internal short circuit of the battery cell has caused complete failure, which shows that the pure PC-based electrolyte has excellent thermal stability, and the Na formed in the electrolyte + -PC-DTD-FEC-HMDI - The main solvation structure of the anion makes the sodium-ion battery have high thermal stability and good cycle performance.
[0094] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A high-temperature sodium ion electrolyte comprising a sodium salt, a non-aqueous organic solvent and an additive a, characterized in that: The non-aqueous organic solvent is propylene carbonate; The additive a is fluoroethylene carbonate, hexamethylene diisocyanate and vinyl sulfate.
2. The high temperature sodium ion electrolyte according to claim 1, characterized in that: The amount of the additive a added is >0.1wt% and ≤30wt%.
3. The high temperature sodium ion electrolyte according to claim 1, characterized in that: The mass ratio of the fluoroethylene carbonate, hexamethylene diisocyanate and vinyl sulfate in the additive a is 0.1-29:0.1-5:0.1-8.
4. The high temperature sodium ion electrolyte according to claim 1, characterized in that: The addition amount of the sodium salt is 8-42 wt%.
5. The high temperature sodium ion electrolyte according to claim 1, characterized in that: The high temperature sodium ion electrolyte further includes an additive b.
6. The high temperature sodium ion electrolyte according to claim 5, characterized in that: The auxiliary additive b is selected from one or more of vinylene carbonate, vinyl ethylene carbonate, tris(trimethylsilyl) phosphate, tris(trimethylsilyl) borate, 1,3-propane sultone, propenyl-1,3-propane sultone, pentafluoro(phenoxy)cyclotriphosphazene, tetrafluoroethyl tetrafluoropropyl ether, pyridine, ethylene glycol dibutyl ether, propylene sulfite, 4-methylethylene sulfate, succinonitrile, and adiponitrile.
7. The high temperature sodium ion electrolyte according to claim 5, characterized in that: The total addition amount of the additive a and the co-additive b is greater than 0.1 wt % and less than 40 wt %.
8. The high temperature sodium ion electrolyte according to claim 5, characterized in that: The total addition amount of the non-aqueous organic solvent, additive a and co-additive b is ≥40% and ≤97%.
9. Use of the high-temperature sodium ion electrolyte according to any one of claims 1 to 8 in the preparation of a high-safety sodium ion battery.
10. A high-safety sodium ion battery, characterized in that: The invention comprises a positive electrode sheet, a negative electrode sheet, a separator and the high-temperature sodium ion electrolyte according to any one of claims 1 to 8.
Citation Information
Cited By
Sodium ion battery and electric device
CN119674184A
High-temperature-resistant stable-circulation sodium metal battery electrolyte
CN122781981A
High-temperature sodium ion electrolyte and high-safety sodium ion battery
WO2026016605A1
Sodium-ion battery electrolyte and sodium-ion battery prepared therefrom
WO2026097814A1