A preparation system for functional gradient materials
Through the preparation system, the mixture of metal particles and ceramic powders of different particle sizes is prepared, and hot pressing and sintering is carried out to form functional gradient materials, which solves the problems of taking into account both hardness and toughness in the prior art, and achieves high hardness and high toughness materials in the aerospace field need.
Patent Information
- Application Number
- CN202411275637.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-09-12
AI Technical Summary
In the prior art, increasing hardness of the material will lead to a decrease in toughness, and vice versa, making it difficult to take into account the high hardness and high toughness requirements of the material in the aerospace field.
Through the preparation system, metal particles of different particle sizes are prepared using plasma guns and drive devices, mixed with ceramic powder, and hot-pressed sintering to form a multi-layer sintered body and superimposed along the thickness direction, obtain functional gradient materials and achieve hardness and toughness. Gradient variation.
It has achieved functional gradient materials with different ceramic contents, different crystal sizes, and high hardness and high toughness along the thickness direction, meeting the diversified needs of the aerospace field.
Smart Images

Figure CN118788971B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of functional gradient materials, and in particular to a preparation system of functional gradient materials. Background Art
[0002] With the improvement of science and technology, people's demands on material properties are becoming increasingly diversified.
[0003] In the prior art, as the hardness of a material increases, its toughness decreases, and vice versa. However, in the aerospace field, there is a high demand for both toughness and hardness of materials.
[0004] Therefore, a system is needed to prepare functionally gradient materials that have both hardness and toughness. Summary of the invention
[0005] The embodiment of the present invention provides a system for preparing a functional gradient material, which can provide a functional gradient material having both hardness and toughness.
[0006] The embodiment of the present invention provides a system for preparing a functional gradient material, including a powder making device, a mixing device and a hot pressing device;
[0007] The powder making device comprises a plasma gun, a powder making bin and a driving device, wherein the plasma release end of the plasma gun is arranged in the powder making bin, the driving device penetrates into the powder making bin and is opposite to the plasma gun, one end of the driving device penetrates into the powder making bin and is used to place metal rods to be melted and powdered, the driving device is used to drive the metal rods to rotate circumferentially and advance and retreat axially, the metal rods and the plasma gun are both arranged in a vertical direction, a plurality of cylindrical plates are arranged in the powder making bin with the axial direction of the metal rods as the center, the plurality of cylindrical plates divide the powder making bin into a plurality of collecting bins, and metal particles of different sizes are obtained in different collecting bins by adjusting the current of the plasma gun and the rotation speed and feed speed of the driving device;
[0008] The mixing device is used to evenly mix the metal particles of different particle sizes prepared by the powder making device with ceramic powders of different proportions to obtain mixed particles;
[0009] The hot pressing device is used to perform hot pressing and sintering treatment on metal-ceramic mixed particles containing different proportions of ceramic powder to obtain multiple layered sintered bodies, and then hot pressing and sintering treatment is performed on multiple layered sintered bodies stacked together in order of ceramic content to obtain functional gradient materials.
[0010] In a possible design, the driving device is connected to the flour making bin in a rotating dynamic seal.
[0011] In a possible design, the bottom of the powder making bin is inclined from the center to the surroundings, wherein the center is high and the surroundings are low, and an openable and closable inlet and outlet are provided at the lowest point of each collecting bin, and the inlet and outlet are used to collect the prepared metal particles.
[0012] In a possible design, the inlet and outlet are connected to a collection pipe to collect the metal particles, and the inlet and outlet are provided with a valve to control the opening and closing of the inlet and outlet.
[0013] In a possible design, a vacuum pumping device is also included, and the vacuum pumping device is used to vacuum the flour making bin.
[0014] In one possible design, the mixing device comprises a ball milling device.
[0015] In a possible design, when the metal particles and the ceramic powder are mixed by the mixing device, the finer the particle size of the metal particles, the higher the proportion of the ceramic powder.
[0016] In a possible design, the metal particles include titanium alloy, and the ceramic powder includes ceramic powder containing boron, carbon and / or nitrogen elements.
[0017] In a possible design, when each group of the mixed particles is subjected to the first hot pressing sintering, the higher the proportion of metal particles in the mixed particles, the higher the temperature of the first hot pressing sintering.
[0018] In a possible design, when the stacked layered sintered bodies are hot-pressed, a heat insulating layer is provided on one side of the layered sintered bodies with the lowest ceramic content, and then hot-pressed sintering is performed again to obtain the functional gradient material.
[0019] Compared with the prior art, the present invention has at least the following beneficial effects:
[0020] In the present invention, the rotation speed of the metal rod is first controlled by a driving device to prepare metal particles with different particle sizes. The faster the rotation speed, the smaller the particle size of the metal particles, the faster the cooling rate, and the smaller the size of the crystal. Conversely, the slower the rotation speed, the larger the particle size of the metal particles, the slower the cooling rate, and the larger the size of the crystal. The smaller the size of the crystal, the higher the hardness, the larger the size of the crystal, and the better the toughness. In summary, by controlling the rotation speed of the metal rod, small metal particles with small particle size and small crystal size and large metal particles with large particle size and large crystal size can be obtained. Metal particles of different particle sizes and ceramic powders of different volumes are mixed in a mixing device. The smaller the particle size of the metal particles, the higher the proportion of the mixed ceramic powder, and multiple groups of mixed particles are obtained. In multiple groups of mixed particles, the smaller the particle size of the metal particles, the higher the proportion of the ceramic powder in the mixed particles. The addition of ceramic powder can improve the ablation resistance of the material. At the same time, it can react at the boundary of the metal grains during sintering. The generated ceramic body fills and distributes at the boundary of the metal grains, increasing the hardness of the material itself. The higher the proportion of ceramic powder, the more obvious the hardness improvement. Conversely, the smaller the proportion of ceramic powder, the higher the toughness. Each group of mixed particles is first hot-pressed and sintered to obtain multiple layered sintered bodies. Then, the multiple layered sintered bodies are stacked along the thickness direction in order of the ceramic content, and hot-pressed and sintered again to obtain a functional gradient material. The obtained material has different ceramic content and crystal size along the thickness direction. One side has a small crystal size, a high ceramic content, and high hardness. The other side has a large crystal size, a small ceramic content, or even no ceramic, and good toughness. The hardness and toughness gradient in the middle part change. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0022] Figure 1 It is a structural schematic diagram of a powder making device provided in an embodiment of the present invention.
[0023] In the figure:
[0024] 1- Plasma gun;
[0025] 2- flour making silo;
[0026] 3- driving device;
[0027] 4-Metal bars;
[0028] 5-cylindrical plate;
[0029] 6- Collection bin. DETAILED DESCRIPTION
[0030] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0031] In the description of the embodiments of the present invention, unless otherwise clearly specified and limited, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance; unless otherwise specified or explained, the term "multiple" refers to two or more; the terms "connected" and "fixed" should be understood in a broad sense, for example, "connected" can be a fixed connection, a detachable connection, an integral connection, or an electrical connection; it can be directly connected or indirectly connected through an intermediate medium. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0032] In the description of this specification, it should be understood that the directional words such as "upper" and "lower" described in the embodiments of the present invention are described at the angles shown in the drawings and should not be understood as limiting the embodiments of the present invention. In addition, in the context, it should also be understood that when it is mentioned that an element is connected to another element "upper" or "lower", it can not only be directly connected to another element "upper" or "lower", but also indirectly connected to another element "upper" or "lower" through an intermediate element.
[0033] Please refer to Figure 1 , a preparation system of a functional gradient material, comprising a powder making device, a mixing device and a hot pressing device;
[0034] The powder making device comprises a plasma gun 1, a powder making bin 2 and a driving device 3, wherein the plasma release end of the plasma gun 1 is arranged in the powder making bin 2, the driving device 3 penetrates into the powder making bin 2, and is opposite to the plasma gun 1, and one end of the driving device 3 penetrates into the powder making bin 2 for placing a metal rod 4 to be melted and powdered, and the driving device 3 is used to drive the metal rod 4 to rotate circumferentially and advance and retreat axially, the metal rod 4 and the plasma gun 1 are both arranged in a vertical direction, and a plurality of cylindrical plates 5 are arranged in the powder making bin 2 with the axial direction of the metal rod 4 as the center, and the plurality of cylindrical plates 5 divide the powder making bin 2 into a plurality of collecting bins 6, and metal particles of different sizes are obtained in different collecting bins 6 by adjusting the current of the plasma gun 1 and the rotation speed and feed speed of the driving device 3;
[0035] The mixing device is used to evenly mix the metal particles of different particle sizes prepared by the powder making device with ceramic powders of different proportions to obtain mixed particles;
[0036] The hot pressing device is used to perform hot pressing and sintering treatment on metal-ceramic mixed particles containing different proportions of ceramic powder to obtain multiple layered sintered bodies, and then hot pressing and sintering treatment is performed on multiple layered sintered bodies stacked together in order of ceramic content to obtain functional gradient materials.
[0037] In the present invention, the rotation speed of the metal rod 4 is first controlled by the driving device 3 to prepare metal particles with different particle sizes. The faster the rotation speed, the smaller the particle size of the metal particles, the faster the cooling rate, and the smaller the size of the crystal. Conversely, the slower the rotation speed, the larger the particle size of the metal particles, the slower the cooling rate, and the larger the size of the crystal. The smaller the size of the crystal, the higher the hardness, the larger the size of the crystal, and the better the toughness. In summary, by controlling the rotation speed of the metal rod 4, small metal particles with small particle size and small crystal size and large metal particles with large particle size and large crystal size can be obtained. Metal particles of different particle sizes and ceramic powders of different volumes are mixed in a mixing device. The smaller the particle size of the metal particles, the higher the proportion of the mixed ceramic powder, and multiple groups of mixed particles are obtained. In multiple groups of mixed particles, the smaller the particle size of the metal particles, the higher the proportion of the ceramic powder in the mixed particles. The addition of ceramic powder can improve the ablation resistance of the material. At the same time, it can react at the boundary of the metal grains during sintering. The generated ceramic body fills and distributes at the boundary of the metal grains, increasing the hardness of the material itself. The higher the proportion of ceramic powder, the more obvious the hardness improvement. Conversely, the smaller the proportion of ceramic powder, the higher the toughness. Each group of mixed particles is first hot-pressed and sintered to obtain multiple layered sintered bodies. Then, the multiple layered sintered bodies are stacked along the thickness direction in order of the ceramic content, and hot-pressed and sintered again to obtain a functional gradient material. The obtained material has different ceramic content and crystal size along the thickness direction. One side has a small crystal size, a high ceramic content, and high hardness. The other side has a large crystal size, a small ceramic content, or even no ceramic, and good toughness. The hardness and toughness gradient in the middle part change.
[0038] It should be noted that the large-size metal particles may be mixed with a small amount of ceramic powder or may not be mixed with the ceramic powder. The above-mentioned different amounts of ceramic powder include 0-content ceramic powder.
[0039] In some embodiments of the present invention, the driving device 3 is connected to the flour making bin 2 in a rotating dynamic seal.
[0040] In some embodiments of the present invention, the bottom of the powder making bin 2 is inclined from the center to the surroundings, wherein the center is high and the surroundings are low, and an openable and closable inlet and outlet are provided at the lowest point of each collecting bin 6, and the inlet and outlet are used to collect the prepared metal particles.
[0041] In some embodiments of the present invention, the inlet and outlet are connected to a collection pipe to collect the metal particles, and the inlet and outlet are provided with a valve to control the opening and closing of the inlet and outlet.
[0042] In some embodiments of the present invention, a vacuum pumping device is further included, and the vacuum pumping device is used to vacuum the flour making bin 2.
[0043] In some embodiments of the present invention, the mixing device comprises a ball milling device.
[0044] In some embodiments of the present invention, when the metal particles and the ceramic powder are mixed by the mixing device, the finer the particle size of the metal particles, the higher the proportion of the ceramic powder.
[0045] In some embodiments of the present invention, the metal particles include a titanium alloy.
[0046] In this embodiment, the titanium alloy has the characteristics of high temperature resistance, excellent mechanical properties and light weight, and is suitable for the aerospace field.
[0047] In some embodiments of the present invention, the ceramic powder includes ceramic powder containing boron, carbon and / or nitrogen elements.
[0048] In this embodiment, the ceramic powder containing boron, carbon and / or nitrogen elements can react with titanium to obtain a ceramic body with increased hardness.
[0049] In some embodiments of the present invention, the particle size of the ceramic powder is 5-10 μm.
[0050] In this embodiment, the particle size of the ceramic powder is in the range of 5 to 10 μm, which can be well mixed and wrapped with the metal particles, increase the contact surface between the metal particles and the ceramic powder, and increase the efficiency of the combination or reaction.
[0051] In some embodiments of the present invention, different particle size ranges of metal particles are determined according to needs, and the rotation speed of the rotating electrode in the plasma rotating electrode process is allocated between 8000 and 35000 rpm according to the particle size range; according to the rotation speed of the rotating electrode, the current value in the plasma rotating electrode process is controlled within the range of 600 to 1200 A to obtain micron-sized metal particles of different particle sizes of 5 to 20 μm; wherein the current and the rotation speed are in inverse proportion.
[0052] In this embodiment, the rotation speed can be controlled to be 8000~10000rpm, 18000~20000rpm, and 30000~35000rpm, respectively, and the three rotation speeds correspond to 1000~1200A, 800~1000A, and 600~800A, respectively. The higher the current, the higher the temperature of the electrode, the higher the melting degree of the metal material, the higher the melting degree, the larger the particles thrown out, and in addition, the slower the rotation speed, the larger the particles thrown out by the centrifugal force. Therefore, low rotation speed combined with high current can obtain metal particles with large particle size, and high rotation speed combined with low current can obtain metal particles with small particle size.
[0053] Of course, you can also set more different speeds between 8000~35000rpm according to your needs to obtain metal particles of more different particle sizes. The current can also be adaptively adjusted according to different speeds.
[0054] In some embodiments of the present invention, when each group of mixed particles is subjected to the first hot pressing sintering, the higher the proportion of metal particles in the mixed particles, the higher the temperature of the first hot pressing sintering.
[0055] In the present application, the temperature of the first hot pressing sintering affects the degree of recrystallization of the metal. The higher the temperature, the better the degree of recrystallization and the larger the resulting grains. When the temperature is low, the degree of metal recrystallization is low or no recrystallization occurs. Therefore, by controlling the temperature of the first hot pressing sintering at a higher temperature, the mixed particles of large metal grains can be sintered and the grains can be further enlarged; by controlling the first sintering temperature at a lower temperature, the mixed particles are only combined and compacted with each other, and no or little recrystallization occurs, so that after the mixed particles of small metal grains are sintered, the grains remain at a smaller degree.
[0056] In some embodiments of the present invention, when the stacked layered sintered bodies are hot-pressed, a heat insulating layer is provided on one side of the layered sintered bodies having the lowest ceramic content, and then hot-pressed sintering is performed again to obtain the functional gradient material.
[0057] In this embodiment, after a heat-insulating layer is provided on one side of the layered sintered body with the lowest ceramic content, the heating rate is slow during the second hot-pressing sintering, but with the passage of time, it can still reach a temperature (900°C) that can transform the titanium crystal from a close-packed hexagonal closest packing structure to a body-centered cubic structure. With the end of the second hot-pressing sintering, the temperature begins to gradually decrease. However, due to the presence of the heat-insulating layer, the cooling rate of the part with a low ceramic content is slow. The cooling rate is related to the content of body-centered cubic structure crystals. The slower the cooling rate, the lower the content of body-centered cubic structure crystals, and the stronger the toughness of the material. The faster the cooling rate, the higher the content of body-centered cubic structure crystals, and the stronger the hardness of the material.
[0058] It should be noted that although hot pressing and sintering again will also cause recrystallization, the size relationship between the larger crystals and the smaller crystals remains unchanged after both are recrystallized. In addition, ceramic phases are distributed at the boundaries of small crystals inside the layered sintered body of smaller crystals, which limits the degree of recrystallization. Therefore, only part of the crystals inside the layered sintered body of smaller crystals are recrystallized, which has little effect on the change of the overall crystal particles.
[0059] In some embodiments of the present invention, the temperature of the first hot pressing sintering is 800-1200° C., and the pressure of the first hot pressing sintering is 80-120 MPa.
[0060] In some embodiments of the present invention, the temperature of the hot pressing sintering again is 950-1100° C., and the pressure is 100-150 MPa.
[0061] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A system for preparing a functional gradient material, characterized in that: It includes a powder making device, a mixing device and a hot pressing device; The powder making device comprises a plasma gun (1), a powder making bin (2) and a driving device (3); the plasma release end of the plasma gun (1) is arranged in the powder making bin (2); the driving device (3) penetrates into the powder making bin (2) and is opposite to the plasma gun (1); one end of the driving device (3) penetrates into the powder making bin (2) and is used to place a metal rod (4) to be melted and powdered; the driving device (3) is used to drive the metal rod (4) to rotate circumferentially and advance and retreat axially; the metal rod (4) and the plasma gun (1) are both arranged in a vertical direction; a plurality of cylindrical plates (5) are arranged in the powder making bin (2) with the axial direction of the metal rod (4) as the center; the plurality of cylindrical plates (5) divide the powder making bin (2) into a plurality of collecting bins (6); and metal particles of different sizes are obtained in different collecting bins (6) by adjusting the current of the plasma gun (1) and the rotation speed and feed speed of the driving device (3); When the metal particles and the ceramic powder are mixed by the mixing device, the finer the particle size of the metal particles, the higher the proportion of the ceramic powder; The metal particles include titanium alloy, and the ceramic powder includes ceramic powder containing boron, carbon and / or nitrogen elements; The mixing device is used to evenly mix the metal particles of different particle sizes prepared by the powder making device with ceramic powders of different proportions to obtain mixed particles; The hot pressing device is used to perform hot pressing and sintering treatment on metal-ceramic mixed particles containing ceramic powders in different proportions to obtain a plurality of layered sintered bodies, and then hot pressing and sintering treatment is performed on a plurality of layered sintered bodies stacked together in order of ceramic content to obtain a functional gradient material; When each group of the mixed particles is subjected to the first hot pressing sintering treatment, the higher the proportion of metal particles in the mixed particles, the higher the temperature of the first hot pressing sintering; When hot pressing and sintering the stacked layered sintered bodies, a heat insulating layer is arranged on one side of the layered sintered bodies with the lowest ceramic content, and then hot pressing and sintering are performed again to obtain the functional gradient material; The temperature of the first hot pressing sintering includes 800~1200℃, and the pressure of the first hot pressing sintering includes 80~120MPa; The temperature of the hot pressing sintering again includes 950~1100°C, and the pressure includes 100~150MPa.
2. The preparation system according to claim 1, characterized in that: The driving device (3) is connected to the flour making bin (2) in a rotating dynamic seal.
3. The preparation system according to claim 1, characterized in that: The bottom of the powder making bin (2) is inclined from the center to the surroundings, wherein the center is high and the surroundings are low. An openable and closable inlet and outlet are provided at the lowest point of each collecting bin (6), and the inlet and outlet are used to collect the produced metal particles.
4. The preparation system according to claim 3, characterized in that: The inlet and outlet are connected with a collecting pipe to collect the metal particles, and the inlet and outlet are provided with a valve to control the opening and closing of the inlet and outlet.
5. The preparation system according to claim 1, characterized in that: It also comprises a vacuum extraction device, which is used to extract a vacuum inside the flour making bin (2).
6. The preparation system according to claim 1, characterized in that: The mixing device includes a ball mill.
Citation Information
Patent Citations
Cu-Ti2 AlC functionally gradient material and preparation method thereof
CN103085395A
Gradient distribution hard alloy and preparation method thereof
CN106282718A
Vertical powder production equipment of plasma rotating electrode and powder production process
CN107008913A