A rare earth metal-In based self-grown nanocrystalline composite material suitable for hydrogen production by hydrolysis
Through the design and preparation of rare earth metal-In-based self-incubation nanocrystal composite materials, the problems of poor hydrolysis and high cost of hydrogen production at low temperatures are solved, and rapid hydrogen production at below -32 degrees Celsius is achieved, reducing the Cost and improve hydrogen production efficiency, and has environmentally friendly and green and resource-recyclable processes.
Patent Information
- Application Number
- CN202411266289.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-11
AI Technical Summary
The poor activity and high cost of hydrolysis of existing metal-based materials at low temperatures limit their widespread use in industrial applications, especially in water reaction hydrogen production technology below zero degrees.
Through the design and preparation method of rare earth metal-In-based self-incubation nanocrystal composite materials, RE-In nanoparticles are generated in the In matrix by induction heating and arc smelting technology, the reactive activity of RE elements is improved and the reaction activity is at -32 degrees Celsius. The following reacts with water to achieve rapid hydrogen production.
The hydrogen production is achieved by reacting with pure water below -32 degrees Celsius, reducing the reaction temperature of RE and water, reducing costs, and improving the hydrogen production rate and hydrogen production rate. The product produced by the reaction of the material with water is insoluble in water and is corrosion-free , environmentally friendly and resource-recyclable processes.
Smart Images

Figure CN118792562B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a composition design and preparation technology of a metal composite material for producing hydrogen by hydrolysis, in particular, through rare earth metal (RE)-In element composite, wherein the rare earth metal elements include La (lanthanum), Ce (cerium), Pr (praseodymium), Nd (neodymium), Pm (promethium), Sm (samarium), Eu (europium). RE nano-crystals are self-bred in the In matrix, thereby realizing a composite material and a preparation method thereof in which the RE element reacts with water to produce hydrogen in a temperature range as low as -32 degrees Celsius. Background Art
[0002] Hydrogen energy is mainly used in the industrial and transportation fields. Hydrogen energy has broad application prospects in many fields such as transportation, industry, construction and electricity. The development of hydrogen energy is seen as an important path for clean energy transformation and achieving carbon neutrality. However, the rare content and high cost of platinum, a precious metal used in traditional hydrogen production, have limited the widespread application of platinum (Pt) in practical production. In recent years, scientists have been working hard to explore new catalysts to replace Pt. Such as transition metal nitrogen, phosphorus, sulfur and carbide, but their catalytic performance is still lower than that of platinum. Therefore, we need to study a new catalyst with excellent catalytic performance, low price and large storage capacity. As we all know, rare earth metal (RE) catalysts, as environmentally friendly materials, have attracted widespread attention in the catalytic reduction of hydrogen due to their excellent oxygen storage and release capacity and excellent redox performance. However, RE catalysts have the disadvantages of poor low-temperature activity and weak anti-toxicity, which are key issues limiting their widespread application. The composite of In element and RE can well solve the existing problems of transition metal catalysts. Therefore, this study mainly studies RE-In-based composite materials. So far, no matter what kind of research, people are committed to the production of hydrogen by hydrolysis of metal-based materials at room temperature and above, and there are fewer studies on the production of hydrogen by alloys at low temperatures. Hydrolysis of metal-based materials has significant advantages over other hydrogen production methods and applications. There is no need to store and transport hydrogen, two cumbersome industrial chain links, and rapid hydrogen production and utilization can be achieved, that is, hydrogen can be quickly produced and used anytime and anywhere. The key to achieving this advantage is that the temperature range of the hydrogen production reaction temperature needs to be wide, especially at low temperatures. Providing metal-based materials and preparation methods that can react with water (ice) below zero degrees to produce hydrogen is a challenging task. Therefore, choosing the right metal-based material is crucial to achieving this goal.
[0003] So far, the metal-based material proposed for hydrogen production below low temperature is Sc-Sn-based alloy. The Sc-Sn alloy ingot prepared by smelting can react with water when the temperature rises to minus thirty degrees Celsius (a Sc-Sn-based self-inoculated nanocrystalline composite material suitable for hydrolysis hydrogen production, ZL202310087921.5). However, due to the high unit price of Sc, it will greatly increase the cost of industrial use. Therefore, it is considered to replace the Sc-Sn-based alloy material for hydrogen production at low temperature with a lower-priced metal element. Summary of the invention
[0004] The present invention aims to solve the above problems and proposes a rare earth metal-In-based self-inoculated nano-grain composite material suitable for hydrolysis hydrogen production. The material is a composite material of RE-In nanoparticles spontaneously generated in the In matrix by compounding two metals, thereby realizing RE-In composite alloying and improving the reactivity of the RE element. In order to realize the preparation of the RE-In metal composite material, a specific smelting method is adopted to mix and smelt a certain proportion of RE-In metals. By induction heating, it is ensured that the two are uniformly mixed in a molten state. Subsequently, by controlling the solidification rate, RE-In-based nanoparticles are generated in the cooling and solidification process of the material. The In matrix in these nanoparticles is uniformly embedded in the excess RE element under the above conditions. The composite material generated by the present invention exhibits a special property, that is, it can react with water in a temperature range as low as -32 degrees Celsius, thereby producing the effect of hydrolysis hydrogen production.
[0005] The technical solution of the present invention is:
[0006] A rare earth metal-In based self-incubated nanocrystalline composite material suitable for hydrogen production by hydrolysis, the elemental chemical formula of the material is RE 1-x In x , 0.1 ≤X≤0.85; the subscript symbol x in the formula represents the molar ratio of the limiting element among the elements.
[0007] The microstructure consists of matrix In and RE nanoparticles distributed in it;
[0008] The particle size of nanoparticles is 2~100nm, accounting for 10%-80% of the weight of the composite material;
[0009] RE=La, Ce, Pr, Nd, Pm, Sm or Eu.
[0010] The method for preparing the rare earth metal-In based self-inoculated nano-crystalline composite material suitable for producing hydrogen by hydrolysis comprises the following steps:
[0011] (1) Weigh pure RE and pure In according to the material ratio of the chemical formula;
[0012] The purity of the pure RE and pure In is above 90%;
[0013] (2) Place pure RE material and pure In material in a high vacuum non-consumable arc furnace and evacuate the vacuum to a degree of 1.0×10 -3 Pa~1.0×10 -7 Pa, after filling with argon, the pressure is -0.5~0MPa; then repeatedly turn over and melt for 3~6 times; after cooling, take out the obtained smelted ingot; the smelting current range can be adjusted within 30-110A;
[0014] The purity of the argon gas is above 95%;
[0015] (3) Place the melted ingot in a quartz tube and evacuate to 1.0×10 -3 Pa~1.0×10 -6 Pa, a closed quartz tube; subsequently, the ingot is placed in an induction coil and heated until it melts;
[0016] The heating temperature of the induction coil is preferably 600-1800 degrees Celsius;
[0017] (4) After the ingot is completely melted, lower the current intensity of the induction coil to cool the alloy at a rate of 1°C / min to 15°C / min;
[0018] (5) When the molten metal liquid is completely solidified, the power is cut off and it is naturally cooled to room temperature to obtain a composite material.
[0019] The application of the rare earth metal-In based self-inoculated nano-crystalline grain composite material suitable for producing hydrogen by hydrolysis comprises the following steps:
[0020] Adding the composite material into pure water (ice) within the range of -32 to 400°C to generate hydrogen;
[0021] Among them, the molar ratio is, H2O: composite material = 1: 0.0147~3.68;
[0022] The hydrogen production rate of the application is 82%~100%; the average hydrogen production rate is 4.63~15.83 mL / min•g.
[0023] The essential features of the present invention are:
[0024] In current technology, metal-based materials use a simple alloying mechanism to produce hydrogen. The metal elements themselves have poor low-temperature activity and weak anti-toxicity, and the activity of the "reactive metal" cannot be fully improved after alloying, resulting in the inability to react with pure water to produce hydrogen below zero degrees. At the same time, the existing Sc-Sn-based alloy materials that hydrolyze hydrogen at low temperatures can react at minus 30 degrees Celsius, but the alloy cost is high, about 85% higher than the price of RE-In.
[0025] The present invention has two preparation stages: smelting alloy ingots and self-inoculating nanoparticles, and self-inoculating nanocrystals to form a composite material. The self-inoculated nanoparticles and the In matrix form a primary cell reaction, which promotes the hydrolysis hydrogen production reaction process and reduces the temperature of the reaction between RE and water, that is, In plays the role of a catalyst to reduce the temperature of the reaction between RE and water; the material can react with pure water (not a modified solution) to produce hydrogen at -32 degrees Celsius.
[0026] Since bulk In does not react with water, RE reacts with water to generate RE2O3, which can be reused after recycling. In practical applications, the composition ratio of RE and In or different cooling rates are used to control the composition and phase structure of the composite material to meet the needs of different hydrogen production rates.
[0027] The beneficial effects of the present invention are:
[0028] The present invention discloses a composition design and preparation technology for metal composite materials for hydrogen production by hydrolysis. This series of metal-based composite materials can react rapidly with water within a temperature range as low as -32 degrees Celsius, which solves the problem that catalysts lack a wide temperature range in practical applications and the problem that existing low-temperature catalysts are expensive. In addition, the products generated by the reaction of the material with water are insoluble in water, do not form a strong alkaline solution, are non-corrosive, non-polluting, and can be efficiently recycled and reused. The metal-based composite materials of the present invention comply with environmentally friendly green hydrogen production and resource-recyclable processes, and have the potential for widespread promotion and application. The two-stage process of arc melting alloy ingots and self-incubated induction heating nanoparticles in the present invention is a new process for controllable preparation of RE-In composite materials. Its essence is that the composite material phases constitute a primary cell reaction to increase the material's reaction activity with water. The preparation process based on this mechanism has broad promotion value in the field of related composite material preparation. Compared with the Sc-Sn-based alloy with the widest temperature range at present, the reaction temperature of the RE-In composite material of the present invention with pure water is reduced to -2 degrees Celsius (Sn-Sn is above -30 degrees), and the cost is saved by more than 85%. The two most important hydrogen production performance parameters: reaction hydrogen production rate and hydrogen production rate reach 8.47 mL / min·g and 93% respectively, reaching the level of arc melting Sc-Sn alloy ingots. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is a cross-sectional morphology of La3In2 obtained in Example 1 (scanning electron microscope image). Figure 1 (a) is a scanning electron microscope image of the point 1 area; Figure 1 (b) is a scanning electron microscope image of point 2;
[0030] Figure 2 is the XRD pattern of the La-In alloy obtained in Example 1; DETAILED DESCRIPTION
[0031] Example 1: 1) Nominal composition of composite material: La 0.6 In 0.4 ; The subscript numbers are the molar ratios between the elements.
[0032] According to the above chemical formula, the molar ratio of the elements is converted into the mass ratio, and then the mass of each raw material is calculated according to the mass ratio. The purity of the raw materials is 99.9%, which meets the requirements of experimental precision. (The purity of the material can be selected to be above 90%)
[0033] 2) Arc melting to prepare composite material ingot: The raw materials (La 8.334g, In 4.592g) were melted in a high vacuum non-consumable arc furnace. The melting vacuum was 1.0×10 -3 Pa, after filling with argon (purity above 99.9%), the pressure is -0.5MPa. During the smelting process, the metal ingot is turned over three times for smelting. Smelting current: at 85A, the smelting temperature is maintained at 600℃.
[0034] 3) Induction coil temperature control self-incubation of nanoparticles: The ingot obtained by smelting is first placed in a quartz tube. After the quartz tube is vacuum sealed, the sealed quartz tube is placed in an induction coil, and the vacuum degree is maintained at 1.0×10 -3 Pa, induction heating is carried out (the heating temperature of the induction coil is 900 degrees Celsius), and the current intensity of the induction coil is regulated by the infrared temperature measurement / thermocouple temperature measurement feedback system to slowly cool the temperature from the melting point and maintain the cooling rate at 1 degree / minute.
[0035] 4) When the molten metal liquid is completely solidified, quickly cut off the power supply, let it cool naturally to room temperature, and take out the sample.
[0036] The cross-sectional morphology (scanning electron microscope image) of the La3In2 alloy obtained by the present invention is as follows: Figure 1 As shown, it is obvious that there are nanoparticles (30-100 nanoparticles) embedded in the matrix. The energy spectrum analysis of point 1 and point 2 was performed respectively, and the components of the two areas are Figure 1 (a) Point area nanoparticles La:In=5:4, Figure 1(b) Point area nanoparticles La:In=5:3, and X-ray diffraction analysis was carried out on the phase composition of La2In3 alloy. Different phase compositions can be observed in the obtained composite materials, including: La3In2 phase, La5In4 phase, La5In3 phase, and LaIn phase. La3In2 phase, La5In4 phase, La5In3 phase and LaIn nanoparticles are distributed in the matrix In, and the particle range is 30-100nm.
[0037] The data obtained by measuring the hydrogen production rate and the hydrogen production speed at different temperatures are shown in Table 1.
[0038] Measurement method and conditions:
[0039] a. Collect hydrogen by drainage method and measure hydrogen production rate and rate. 1) Place 5g composite material ingot into a three-necked flask, and then place the three-necked flask into crushed ice at -32 degrees Celsius. Place another 50g of crushed ice (at this time, the molar ratio is H2O: composite material = 68:1. Place it into the three-necked flask, connect the catheter, and start collecting gas. Pass the collected gas into the Monte Carlo wash bottle to drain the water in the bottle. Use an electronic balance (accuracy 0.001g) to weigh the weight of the excluded water and calculate the hydrogen production rate and rate. 2) Inject 0.1 liter of pure water as a reaction water source into the three-necked flask, heat it to 50 degrees Celsius in a water bath in the reactor, and put in 5g composite material ingot (at this time, the molar ratio is H2O: composite material = 68:1). Connect the catheter and start collecting gas. The collected gas is introduced into the Monte Carlo wash bottle and drained out. The weight of the excluded water was weighed using an electronic balance (accuracy 0.001g) to calculate the hydrogen production rate and hydrogen production rate.
[0040] b. It is assumed that when the reaction rate between the material and water is less than 0.1 mL / min•g, all the materials have completed the reaction with water. This is used as the time for calculating the hydrogen production rate.
[0041] c. The water-reactive composite material sample used was a smelted composite material ingot (weight 5 g, oval cake shape).
[0042] d. During the reaction with water (ice), the entire ingot is always completely covered by water.
[0043] The mechanism of hydrogen production by hydrolysis of the present invention is: H2O+La ===La2O3+H 2, In plays the role of alloying to increase the electrochemical potential difference between La and In, which is equivalent to the role of a catalyst. In this process, due to the existence of different phases in the composite material, the reaction of La and water can be achieved at a lower temperature through the galvanic cell reaction formed between different phases.
[0044] Example 2: 1) Nominal composition of composite material: Ce 0.35 In0.65 ;
[0045] The mass of each raw material is calculated according to the stoichiometric ratio, and the purity of the raw materials is 96%.
[0046] 2) Arc melting to prepare composite material ingot: The weighed raw materials Ce 4.904g, In 7.462g) were melted in a high vacuum non-consumable arc furnace. The melting vacuum degree was: 1.0×10 -4 Pa, after filling with argon (purity above 99.9%), the pressure is -0.3MPa. During the smelting process, the metal ingot is turned over three times for smelting. Smelting current: at 80A, the smelting temperature is maintained at 900℃.
[0047] 3) Induction coil temperature control self-incubation of nanoparticles: The ingot obtained by smelting is placed in a quartz tube, the quartz tube is vacuum sealed, and then the induction coil is placed, and the vacuum degree is maintained at 1.0×10 -3 Pa, induction heating is carried out (the heating temperature of the induction coil is 1000 degrees Celsius). The infrared temperature measurement / thermocouple temperature measurement feedback system is used to adjust the current intensity of the induction coil and slowly cool the temperature from the melting point at a cooling rate of 4 degrees per minute.
[0048] 4) When the molten metal liquid is completely solidified, quickly cut off the power supply, let it cool naturally to room temperature, and take out the sample.
[0049] Different phase compositions are generated, including: CeIn3 phase, Ce2In phase, Ce3In phase and pure In phase. CeIn3 phase, Ce2In phase, Ce3In phase nanoparticles are distributed in the matrix In, and the particle size range is 30-75nm. The data obtained by measuring the hydrogen production rate and the hydrogen production rate at different temperatures are shown in Table 1. The measurement method and conditions are the same as those in Example 1.
[0050] Example 3: 1) Nominal composition of composite material: Pr 0.5 In 0.5 ;
[0051] The mass of each raw material is calculated according to the stoichiometric ratio, and the purity of the raw materials is 98%.
[0052] 2) Arc melting to prepare composite material ingot: The weighed raw materials (Pr 7.045g, In 5.741g) were melted in a high vacuum non-consumable arc furnace. The melting vacuum was 1.0×10 -5 Pa, fill with argon (purity above 99.9%), pressure is -0.1MPa. During the smelting process, the metal ingot is turned over three times for smelting. Smelting current: at 70A, the smelting temperature can be maintained at 1100℃.
[0053] 3) Induction coil temperature control self-incubation of nanoparticles: The ingot obtained by smelting is placed in a quartz tube, the quartz tube is vacuum sealed, and then the induction coil is placed, and the vacuum degree is maintained at 1.0×10 -3 Pa or above (the heating temperature of the induction coil is 1200 degrees Celsius), and the current intensity of the induction coil is regulated by the infrared temperature measurement / thermocouple temperature measurement feedback system to slowly cool the temperature from the melting point at a cooling rate of 8 degrees per minute.
[0054] 4) When the molten metal liquid is completely solidified, quickly cut off the power supply, let it cool naturally to room temperature, and take out the sample.
[0055] The obtained composite material has different phase compositions, including: PrIn phase, Pr2In phase, Pr3In phase, PrIn3 phase and pure In phase. PrIn phase, Pr2In phase, Pr3In phase, PrIn3 phase nanoparticles are distributed in the matrix In, and the particle range is 10-45nm. The data obtained by measuring the hydrogen production rate and the hydrogen production rate at different temperatures are shown in the table. The measurement method and conditions are the same as those in Example 1.
[0056] Example 4: 1) Nominal composition of composite material: Nd 0.7 In 0.3 ;
[0057] The mass of each raw material is calculated according to the stoichiometric ratio, and the purity of the raw materials is required to be greater than 94%.
[0058] 2) Arc melting to prepare composite material ingot: The weighed raw materials (Nd 10.94g, In 3.445g) were melted in a high vacuum non-consumable arc furnace. The melting vacuum was 1.0×10 -6 Pa, after filling with argon (purity above 99.9%), the pressure is 0MPa. During the smelting process, the metal ingot is turned over three times for smelting. Smelting current: at 85A, the smelting temperature can be maintained at 1200℃.
[0059] 3) Induction coil temperature control self-incubation of nanoparticles: The ingot obtained by smelting is placed in a quartz tube, the quartz tube is vacuum sealed, and then the induction coil is placed, and the vacuum degree is maintained at 1.0×10 -3 Pa or above (the heating temperature of the induction coil is 1400 degrees Celsius), and the induction coil current intensity is regulated by the infrared temperature measurement / thermocouple temperature measurement feedback system to slowly cool the temperature from the melting point at a cooling rate of 12 degrees per minute.
[0060] 4) When the molten metal liquid is completely solidified, quickly cut off the power supply, let it cool naturally to room temperature, and take out the sample.
[0061] The generated products have different phase compositions, including: NdIn phase, NdIn3 phase, Nd2In phase, Nd3In phase nanoparticles distributed in the matrix In, with a particle size range of 20-75nm. The data obtained by measuring the hydrogen production rate and the hydrogen production rate at different temperatures are shown in the table. The measurement method and conditions are the same as those in Example 1.
[0062] Example 5: 1) Nominal composition of composite material: Pm 0.85 In 0.15 ;
[0063] The mass of each raw material is calculated according to the stoichiometric ratio, and the purity of the raw materials is 92%.
[0064] 2) Arc melting to prepare composite material ingot: The weighed raw materials (Pm 12.325g, In 1.722g) were melted in a high vacuum non-consumable arc furnace. The melting vacuum was 1.0×10 -7 Pa, after filling with argon (purity above 99.9%), the pressure is 0MPa. During the smelting process, the metal ingot is turned over three times for smelting. Smelting current: The smelting temperature can be maintained at 1800℃ at 110A.
[0065] 3) Induction coil temperature control self-incubation of nanoparticles: The ingot obtained by smelting is placed in a quartz tube, the quartz tube is vacuum sealed, and then the induction coil is placed, and the vacuum degree is maintained at 1.0×10 -3 Pa or above (the heating temperature of the induction coil is 1800 degrees Celsius), and the current intensity of the induction coil is regulated by the infrared temperature measurement / thermocouple temperature measurement feedback system to slowly cool the temperature from the melting point at a cooling rate of 15 degrees / minute.
[0066] 4) When the molten metal liquid is completely solidified, quickly cut off the power supply, let it cool naturally to room temperature, and take out the sample.
[0067] The generated product has a two-phase composition, including: PmIn3 phase and pure In phase. PmIn3 phase nanoparticles are distributed in the matrix In, and the particle range is 2-45nm. The data obtained by measuring the hydrogen production rate, the hydrogen production rate at different temperatures, evaluating the proportion of nanophase, and the phase composition are shown in the table. The measurement method and conditions are the same as those in Example 1.
[0068] Example 6: 1) Nominal composition of composite material: Sm 0.85 In 0.15 ;
[0069] The mass of each raw material is calculated according to the stoichiometric ratio, and the purity of the raw materials is 92%.
[0070] 2) Arc melting to prepare composite material ingot: The weighed raw materials (Sm 12.784g, In 1.722g) were melted in a high vacuum non-consumable arc furnace. The melting vacuum was 1.0×10 -3 Pa, after filling with argon (purity above 99.9%), the pressure is -0.2MPa. During the smelting process, the metal ingot is turned over three times for smelting. Smelting current: at 95A, the smelting temperature can be maintained at 1400℃.
[0071] 3) Induction coil temperature control self-incubation of nanoparticles: The ingot obtained by smelting is placed in a quartz tube, the quartz tube is vacuum sealed, and then the induction coil is placed, and the vacuum degree is maintained at 1.0×10 -4 Pa, induction heating is carried out (the heating temperature of the induction coil is 1500 degrees Celsius). The infrared temperature measurement / thermocouple temperature measurement feedback system is used to adjust the current intensity of the induction coil and slowly cool the temperature from the melting point at a cooling rate of 15 degrees per minute.
[0072] 4) When the molten metal liquid is completely solidified, quickly cut off the power supply, let it cool naturally to room temperature, and take out the sample.
[0073] The generated product has a two-phase composition, including: SmIn phase, SmIn3 phase, Sm2In phase, Sm3In and pure In phase. SmIn phase, SmIn3 phase, Sm2In phase, Sm3In phase nanoparticles are distributed in the matrix In, and the particle range is 5-35nm. The data obtained by measuring the hydrogen production rate, the hydrogen production rate at different temperatures, evaluating the proportion of nanophase, and the phase composition are shown in the table. The measurement method and conditions are the same as those in Example 1.
[0074] Example 7: 1) Nominal composition of composite material: Eu 0.85 In 0.15 ;
[0075] The mass of each raw material is calculated according to the stoichiometric ratio, and the purity of the raw materials is 92%.
[0076] 2) Arc melting to prepare composite material ingot: The raw materials (Eu 10.625g, In 1.722g) were melted in a high vacuum non-consumable arc furnace. The melting vacuum was 1.0×10 -3 Pa, after filling with argon (purity above 99.9%), the pressure is -0.1MPa. During the smelting process, the metal ingot is turned over three times for smelting. Smelting current: at 90A, the smelting temperature can be maintained at 1500℃.
[0077] 3) Induction coil temperature control self-incubation of nanoparticles: The ingot obtained by smelting is placed in a quartz tube, the quartz tube is vacuum sealed, and then the induction coil is placed, and the vacuum degree is maintained at 1.0×10 -5Pa or above (the heating temperature of the induction coil is 1600 degrees Celsius), and the current intensity of the induction coil is regulated by the infrared temperature measurement / thermocouple temperature measurement feedback system to slowly cool the temperature from the melting point at a cooling rate of 15 degrees / minute.
[0078] 4) When the molten metal liquid is completely solidified, quickly cut off the power supply, let it cool naturally to room temperature, and take out the sample.
[0079] The generated product has a two-phase composition, including: EuIn phase, EuIn2 phase, EuIn3 phase, EuIn4 phase and pure In phase. EuIn phase, EuIn2 phase, EuIn3 phase, EuIn4 phase nanoparticles are distributed in the matrix In, and the particle range is 3-50nm. The hydrogen production rate, hydrogen production rate at different temperatures, evaluation of the proportion of nanophase, and phase composition are obtained. The measurement method and conditions are the same as those in Example 1.
[0080]
[0081] The above examples and data illustrate that the new metal composite material prepared by the preparation method and process technology of the present invention has enhanced the reduction characteristics of RE and greatly broadened the temperature range of the reaction between RE and pure water due to the self-incubation of multiphase nanoparticles on the matrix. The composite material can react with water to quickly produce hydrogen in a temperature range of -32 degrees Celsius, which is 2 degrees Celsius lower than the current best metal-based hydrogen production at low temperatures. The hydrogen production rate of all materials involved in the present invention can be as high as 82% or more, and can reach up to 93%. Its hydrogen production rate is basically equivalent to the Sc-Sn-based alloy that is currently being studied more. Its hydrogen production rate at -32 degrees Celsius reaches more than 4.63 mL / min•g, and can reach up to 15.83 mL / min•g. This result has not been reported so far.
[0082] Matters not covered by the present invention are known technologies.
Claims
1. A rare earth metal-In-based self-incubated nanocrystalline composite material suitable for hydrolysis hydrogen production, characterized in that the elemental chemical formula of the material is RE 1-x In x , 0.1≤X≤0.85; the subscript symbol x in the formula is the molar ratio between the elements; RE=La, Ce, Pr, Nd, Pm, Sm or Eu; The microscopic composition of the composite material is a matrix In and RE nanoparticles distributed therein; the particle size of the nanoparticles is 2-100 nm, accounting for 10%-80% of the weight of the composite material.
2. The method for preparing the rare earth metal-In based self-inoculated nano-crystalline composite material suitable for hydrolysis hydrogen production as claimed in claim 1, characterized in that The following steps are involved: (1) Weigh pure RE and pure In according to the material ratio of the chemical formula; (2) Place pure RE material and pure In material in a high vacuum non-consumable arc furnace and evacuate the vacuum to a degree of 1.0×10 -3 Pa~1.0×10 -7 Pa, fill with argon; then repeatedly turn over and melt for 3 to 6 times; after cooling, take out the obtained smelted ingot; the smelting current range can be adjusted within 30-110A; (3) Place the melted ingot in a quartz tube and evacuate to 1.0×10 -3 Pa~1.0×10 -6 Pa, a closed quartz tube; subsequently, the ingot is placed in an induction coil and heated until it melts; (4) After the ingot is completely melted, lower the current intensity of the induction coil to cool the alloy at a rate of 1°C / min to 15°C / min; (5) When the molten metal liquid is completely solidified, it is naturally cooled to room temperature to obtain a composite material.
3. The method for preparing a rare earth metal-In based self-inoculated nano-crystalline composite material suitable for hydrogen production by hydrolysis as claimed in claim 2, characterized in that the purity of the pure RE and pure In are both above 90%; the purity of the argon is above 95%.
4. The method for preparing a rare earth metal-In based self-inoculated nano-crystalline composite material suitable for producing hydrogen by hydrolysis as claimed in claim 2, characterized in that the heating temperature of the induction coil is 600-1800 degrees Celsius.
5. The use of the rare earth metal-In based self-inoculated nano-crystalline composite material suitable for producing hydrogen by hydrolysis as claimed in claim 1, characterized in that it comprises the following steps: Adding the composite material to pure water / ice in the range of -32 to 400°C to generate hydrogen; in, The molar ratio is, H2O:composite material=1:0.0147~3.68.
Citation Information
Patent Citations
Sc-Sn-based self-inoculation nanocrystal composite material suitable for hydrolysis hydrogen production
CN115852202A
Rare-earth indium alloy
CN103469041A
Catalyst used for preparing low-carbon olefin through low-carbon alkane dehydrogenation and using method thereof
CN105363443A
Sn / Sb / In-based perovskite oxide catalyst and application thereof
CN116145179A