Epitaxial wafer defect reason determination method and device
By rotating the base of the reaction chamber of the epitaxial furnace and adjusting the process conditions, the cause of pin-print defects of epitaxial wafers can be accurately determined, solving the problems of misjudgment and missed determination in the existing technology, and improving product quality and production efficiency.
Patent Information
- Application Number
- CN202410843960.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-18
AI Technical Summary
In the epitaxial wafer manufacturing process, it is difficult to accurately determine the cause of pin-print defects with existing technology, resulting in frequent misjudgments and missed determinations, affecting product quality and production efficiency.
By determining whether pin-print defects of epitaxial wafers occur continuously and rotating the base of the epitaxial furnace reaction chamber at a preset angle when they occur, the process conditions are adjusted to determine the cause of the defects, including checking the wear of the ejector pins and the damage of the epitaxial furnace reaction chamber. process conditions.
Accurately determine the causes of pin-print defects, reduce misjudgments and missed judgments, improve the process flow, and improve the flatness and quality of epitaxial wafers.
Smart Images

Figure CN118800686A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor manufacturing technology, and in particular to a method and device for determining the cause of an epitaxial wafer defect. Background Art
[0002] Epitaxial growth refers to the process of growing a single crystal thin film (with the crystal orientation consistent with that of the substrate) on a single crystal silicon substrate through epitaxy technology. The entire production process of epitaxial wafers includes five major processes: crystal growth (pulling silicon crystal rods from polysilicon materials) → molding (slicing and grinding) → polishing (double-sided polishing) → cleaning (removing surface particles, metal ions and organic matter) → epitaxy (vapor deposition). Epitaxy is the last important process, which can improve the crystal properties, native defects, resistivity and flatness of the polished wafer.
[0003] As chip manufacturing processes continue to shrink, the requirements for wafer flatness are becoming increasingly higher. For example, for a lithography machine that can achieve nanometer-level imaging resolution, it is usually necessary to increase the numerical aperture (NA) of the lens in the lens, which will result in a corresponding decrease in the depth of focus (depth of focus). In order to ensure the clarity of the lithography image, the ups and downs of the wafer surface must be within the depth of focus. Therefore, if the wafer surface is not flat enough and the thickness is uneven, it will cause problems with the lithography at the ups and downs of the wafer. Therefore, in order to manufacture high-quality wafers that can be used for smaller chip processes, the flatness of the wafer must be strictly monitored.
[0004] Normally, pin-mark (Pin Nano) defects have a significant impact on the flatness and appearance of wafers. During the epitaxial growth process, epitaxial wafers will have pin-mark defects due to various factors. If the cause of the defect cannot be determined in time, it will not only cause a large number of products to be scrapped, but also affect product production. At present, there is no standard for determining the cause of pin-mark defects. The time to determine the cause of pin-mark defects is slow, inefficient, and prone to misjudgment and missed judgments. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a method and device for determining the cause of epitaxial wafer defects, which can determine the cause of pin mark defects.
[0006] In order to achieve the above object, the technical solution adopted by the embodiment of the present invention is:
[0007] A method for determining the cause of an epitaxial wafer defect, comprising:
[0008] Determine whether the pin mark defects of the epitaxial wafer occur continuously;
[0009] When the pin-mark defects of the epitaxial wafer occur continuously, rotating the base of the epitaxial furnace reaction chamber by a preset angle;
[0010] After the base of the reaction chamber of the epitaxial furnace is rotated by a preset angle, determining whether the position of the pin mark defect of the epitaxial wafer changes;
[0011] When the position of the pin mark defect of the epitaxial wafer changes, it is determined that the cause of the pin mark defect is the wear of the demolding pin; when the position of the pin mark defect of the epitaxial wafer does not change, the process conditions of the reaction chamber of the epitaxial furnace are adjusted to determine whether the pin mark defect of the epitaxial wafer continues to occur;
[0012] When the pin mark defect of the epitaxial wafer no longer occurs, it is judged that the cause of the pin mark defect is the process conditions of the epitaxial furnace reaction chamber; after adjusting the process conditions of the epitaxial furnace reaction chamber, if the pin mark defect of the epitaxial wafer continues to occur, it is judged that the cause of the pin mark defect is the problem of polishing the wafer.
[0013] In some embodiments, rotating the base of the epitaxial furnace reaction chamber by a preset angle includes:
[0014] The base of the epitaxial furnace reaction chamber is rotated 120° clockwise; or, the base of the epitaxial furnace reaction chamber is rotated 240° clockwise; or, the base of the epitaxial furnace reaction chamber is rotated 120° counterclockwise; or, the base of the epitaxial furnace reaction chamber is rotated 240° counterclockwise.
[0015] In some embodiments, adjusting the process conditions of the epitaxial furnace reaction chamber includes:
[0016] Adjust the power proportion of the bottom heating module of the epitaxial furnace reaction chamber, where the power proportion is the ratio of the power of the bottom heating module to the total heating power, and the total heating power is the sum of the power of the bottom heating module and the power of the top heating module of the epitaxial furnace reaction chamber.
[0017] In some embodiments, adjusting the power ratio of the bottom heating module of the epitaxial furnace reaction chamber includes:
[0018] Adjusting the value of the power ratio, preparing an epitaxial wafer, and determining whether the prepared epitaxial wafer has a pin mark defect;
[0019] If the prepared epitaxial wafer still has pin mark defects, return to the previous step and continue to adjust the value of the power ratio; if the prepared epitaxial wafer no longer has pin mark defects or the number of times the power ratio is adjusted reaches a preset number, end the adjustment of the power ratio.
[0020] In some embodiments, determining whether the pin mark defects of the epitaxial wafer occur continuously includes:
[0021] When more than N epitaxial wafers among M epitaxial wafers produced continuously have pin mark defects, it is determined that the pin mark defects of the epitaxial wafers occur continuously, wherein N and M are integers greater than 1 and N is less than M.
[0022] The embodiment of the present invention further provides a device for determining the cause of epitaxial wafer defects, comprising:
[0023] The first judgment module is used to judge whether the pin mark defects of the epitaxial wafer occur continuously;
[0024] A rotating module, used for rotating the base of the reaction chamber of the epitaxial furnace by a preset angle when pin-marking defects of the epitaxial wafer occur continuously;
[0025] A second judgment module is used to judge whether the position of the pin mark defect of the epitaxial wafer changes after the base of the reaction chamber of the epitaxial furnace rotates by a preset angle;
[0026] The third judgment module is used to judge that the cause of the pin mark defect is the wear of the demolding pin when the position of the pin mark defect of the epitaxial wafer changes;
[0027] An adjustment module, used for adjusting the process conditions of the reaction chamber of the epitaxial furnace when the position of the pin-mark defect of the epitaxial wafer does not change, and determining whether the pin-mark defect of the epitaxial wafer continues to occur;
[0028] The fourth judgment module is used to judge that the cause of the pin mark defect is the process conditions of the epitaxial furnace reaction chamber when the pin mark defect of the epitaxial wafer no longer occurs; after adjusting the process conditions of the epitaxial furnace reaction chamber, if the pin mark defect of the epitaxial wafer continues to occur, it is judged that the cause of the pin mark defect is a problem with the polishing wafer.
[0029] In some embodiments, the rotation module is specifically used to rotate the base of the epitaxial furnace reaction chamber 120° clockwise; or, to rotate the base of the epitaxial furnace reaction chamber 240° clockwise; or, to rotate the base of the epitaxial furnace reaction chamber 120° counterclockwise; or, to rotate the base of the epitaxial furnace reaction chamber 240° counterclockwise.
[0030] In some embodiments, the adjustment module is specifically used to adjust the power ratio of the bottom heating module of the epitaxial furnace reaction chamber, where the power ratio is the ratio of the power of the bottom heating module to the total heating power, and the total heating power is the sum of the power of the bottom heating module and the power of the top heating module of the epitaxial furnace reaction chamber.
[0031] In some embodiments, the adjustment module is specifically used to adjust the value of the power ratio, and prepare an epitaxial wafer to determine whether the prepared epitaxial wafer has a pin mark defect; if the prepared epitaxial wafer still has a pin mark defect, return to the previous step and continue to adjust the value of the power ratio; if the prepared epitaxial wafer no longer has a pin mark defect or the number of times the power ratio is adjusted reaches a preset number, end the adjustment of the power ratio.
[0032] In some embodiments, the first judgment module is specifically used to judge that the pin mark defects of the epitaxial wafers occur continuously when more than N epitaxial wafers have pin mark defects among M epitaxial wafers produced continuously, wherein N and M are integers greater than 1 and N is less than M.
[0033] The beneficial effects of the present invention are:
[0034] In this embodiment, when a pin mark defect occurs in an epitaxial wafer, it is first determined whether the pin mark defect occurs continuously. If it occurs continuously, the epitaxial furnace reaction chamber base is rotated. If the position of the pin mark defect also changes accordingly, it is determined that the pin mark defect is caused by the wear of the demolding pin; if the position of the pin mark defect does not change, the process conditions of the epitaxial furnace reaction chamber are adjusted. If the pin mark defect no longer occurs, it is determined that the pin mark defect is caused by the process conditions of the epitaxial furnace reaction chamber. The technical solution of the present invention can accurately determine the cause of the pin mark defect, reduce the occurrence of misjudgment and missed judgment, and then improve the process flow according to the cause of the pin mark defect, avoid the subsequent occurrence of pin mark defects, and improve the quality of epitaxial wafers. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 A schematic diagram showing the structure of the epitaxial furnace reaction chamber;
[0036] Figure 2 A schematic diagram showing the structure of an epitaxial growth device;
[0037] Figure 3 A schematic diagram showing a flow chart of a method for determining causes of epitaxial wafer defects according to an embodiment of the present invention;
[0038] Figure 4 and Figure 5 Schematic diagram showing pin-mark defects on an epitaxial wafer;
[0039] Figure 6 and Figure 7 A schematic diagram showing pin mark defect parameters of epitaxial wafers under different process conditions;
[0040] Figure 8 A schematic diagram showing the structure of an apparatus for determining causes of epitaxial wafer defects according to an embodiment of the present invention. DETAILED DESCRIPTION
[0041] In order to make the purpose, technical solution and advantages of the embodiment of the present invention clearer, the technical solution of the embodiment of the present invention will be clearly and completely described below in conjunction with the drawings of the embodiment of the present invention. Obviously, the described embodiment is a part of the embodiment of the present invention, not all of the embodiments. Based on the described embodiment of the present invention, all other embodiments obtained by ordinary technicians in this field belong to the scope of protection of the present invention.
[0042] Figure 1 The schematic diagram of the structure of the epitaxial furnace reaction chamber is shown in FIG. Figure 1 As shown, the epitaxial furnace reaction chamber includes an upper quartz bell jar 1, a lower quartz bell jar 2, a halogen lamp 3, a mounting component 4, a base 6, a base support rod 7, etc., wherein 5 is the gas flow direction, and 8 is a silicon wafer. After the silicon wafer 8 is input into the epitaxial furnace reaction chamber, the base 6 carries the silicon wafer 8, and the halogen lamp 3 arranged on the upper side of the base 6 and the halogen lamp 3 arranged on the lower side of the base 6 heat the silicon wafer 8, and the raw material gas is supplied to the main surface of the silicon wafer 8, thereby performing vapor phase growth, and after the vapor phase growth, the epitaxial wafer obtained by the vapor phase growth is output to the outside of the epitaxial furnace reaction chamber. During the growth process, the base support rod 7 plays the role of fixing the base 6 and driving the base 6 to rotate, so that the epitaxial growth can be carried out evenly on the substrate.
[0043] Figure 2 The schematic diagram of the structure of the epitaxial growth equipment shows that during epitaxial growth, the transfer blade in the front-end module ② transfers the silicon wafer from the loading port ① to the load lock unit ③, and the load lock unit ③ is evacuated and backfilled with nitrogen. The transfer robot located in the transfer unit ④ transfers the silicon wafer in the load lock unit ③ through the transfer unit to the process reaction chamber ⑤ for epitaxial growth. After the growth is completed, the silicon wafer returns along the original route.
[0044] There are three main sources of pin mark defects in epitaxial wafers:
[0045] (1) It is related to the quality of the substrate (i.e., polished wafer) and the surface condition of the substrate;
[0046] (2) It is closely related to the epitaxial growth process itself. The uniformity of the temperature distribution in the epitaxial furnace reaction chamber will greatly affect the generation of lift pin contamination marks. Under the existing process conditions, the silicon wafer is at ambient temperature before being loaded into the epitaxial furnace reaction chamber, and the temperature of the epitaxial furnace reaction chamber is always maintained at 850°C in the idle state. This leads to a difference between the surface temperature of the base and the temperature of the silicon wafer during film growth, resulting in the generation of lift pin contamination marks on the back of the silicon wafer during epitaxial growth.
[0047] (3) It is related to the wear of the ejection needle hardware in the reaction chamber of the epitaxial furnace. The ejection needle is in contact with the back of the silicon wafer for a long time, causing the material on the top of the ejection needle to wear out. During the epitaxial film extension process at high temperature, the needle marks are produced when it contacts the surface of the silicon wafer.
[0048] The present invention provides a method and device for determining the cause of epitaxial wafer defects, which can determine the cause of pin mark defects.
[0049] The embodiment of the present invention provides a method for determining the cause of an epitaxial wafer defect, such as Figure 3 As shown, including:
[0050] Step 101: determining whether pin mark defects of the epitaxial wafer occur continuously;
[0051] Specifically, when more than N epitaxial wafers have pin mark defects among M epitaxial wafers produced continuously, it is judged that the pin mark defects of the epitaxial wafers occur continuously, wherein N and M are integers greater than 1, and N is less than M. In some embodiments, M may be 25 and N may be 19. For example, if 20 epitaxial wafers have pin mark defects among a box of 25 epitaxial wafers produced, it is judged that the pin mark defects of the epitaxial wafers occur continuously; of course, the values of M and N may be adjusted according to actual production needs.
[0052] Step 102: When the pin mark defects of the epitaxial wafer occur continuously, rotating the base of the reaction chamber of the epitaxial furnace by a preset angle;
[0053] In this embodiment, the base of the epitaxial furnace reaction chamber can be rotated 120° clockwise; or, the base of the epitaxial furnace reaction chamber can be rotated 240° clockwise; or, the base of the epitaxial furnace reaction chamber can be rotated 120° counterclockwise; or, the base of the epitaxial furnace reaction chamber can be rotated 240° counterclockwise.
[0054] Step 103: after the base of the reaction chamber of the epitaxial furnace rotates by a preset angle, determining whether the position of the pin mark defect of the epitaxial wafer changes;
[0055] In this embodiment, the location of the pin mark defect can be determined according to the location of the area with a higher Delta Nano value. The Delta Nano value is equal to the difference between the Nano value of the epitaxial wafer and the Nano value of the polished wafer. If the DeltaNano value is higher, it means that a pin mark defect occurs in the corresponding area.
[0056] Step 104: when the position of the pin mark defect of the epitaxial wafer changes, determining that the cause of the pin mark defect is wear of the demolding pin; when the position of the pin mark defect of the epitaxial wafer does not change, adjusting the process conditions of the reaction chamber of the epitaxial furnace to determine whether the pin mark defect of the epitaxial wafer continues to occur;
[0057] If the base of the epitaxial furnace reaction chamber rotates 120 degrees clockwise, and the area with a higher Delta Nano value also rotates with the silicon wafer, it indicates that the pin mark defect is caused by the wear of the ejection pin. At this time, the operator needs to be reminded to replace the ejection pin. Figure 4 The figure shows the pin mark defect of epitaxial wafer. Figure 5 This is a schematic diagram of the pin-mark defect on the epitaxial wafer after the susceptor rotates 120° clockwise. It can be seen that the pin-mark defect on the surface of the epitaxial wafer also rotates synchronously with the rotation of the susceptor, indicating that the pin-mark defect is caused by the wear of the ejection pin of the epitaxial furnace.
[0058] If the pin mark defect on the surface of the epitaxial wafer does not rotate synchronously with the rotation of the base, it means that the pin mark defect is not caused by the wear of the epitaxial furnace ejection pin. The process conditions of the epitaxial furnace reaction chamber can be adjusted, such as adjusting the power ratio of the bottom heating module of the epitaxial furnace reaction chamber, to determine whether the pin mark defect continues to occur after adjusting the process conditions. The power ratio is the ratio of the power of the bottom heating module to the total heating power, and the total heating power is the sum of the power of the bottom heating module and the power of the top heating module of the epitaxial furnace reaction chamber.
[0059] Specifically, the value of the power ratio can be adjusted, and an epitaxial wafer can be prepared to determine whether the prepared epitaxial wafer has a pin mark defect; if the prepared epitaxial wafer still has a pin mark defect, return to the previous step and continue to adjust the value of the power ratio; if the prepared epitaxial wafer no longer has a pin mark defect or the number of times the power ratio is adjusted reaches a preset number, end the adjustment of the power ratio.
[0060] For example, the power ratio of the bottom heating module of the epitaxial furnace reaction chamber is adjusted to 60% to determine whether the prepared epitaxial wafer has pin mark defects; but if the prepared epitaxial wafer still has pin mark defects, the power ratio of the bottom heating module of the epitaxial furnace reaction chamber is further adjusted to 58% to determine whether the prepared epitaxial wafer has pin mark defects; but if the prepared epitaxial wafer still has pin mark defects, the power ratio of the bottom heating module of the epitaxial furnace reaction chamber is further adjusted to 54%. If the prepared epitaxial wafer no longer has pin mark defects, the adjustment of the power ratio of the bottom heating module of the epitaxial furnace reaction chamber can be terminated.
[0061] Step 105: When the pin mark defect of the epitaxial wafer no longer occurs, it is determined that the cause of the pin mark defect is the process conditions of the epitaxial furnace reaction chamber; after adjusting the process conditions of the epitaxial furnace reaction chamber, if the pin mark defect of the epitaxial wafer continues to occur, it is determined that the cause of the pin mark defect is a problem with the polishing wafer.
[0062] Figure 6The schematic diagram of the pin mark defect parameters of the epitaxial wafer when the power ratio is 54%, 56%, 58% and 60%, wherein in the schematic diagram of the distribution of Nano values of the epitaxial wafer, green indicates the smallest Nano value, red indicates the largest Nano value, and yellow indicates the second largest Nano value, wherein the red area also indicates the possible location of the pin mark defect. In the X-Profile curve, the greater the fluctuation of the curve, the greater the probability of the pin mark defect; the smaller the fluctuation of the curve, the smaller the probability of the pin mark defect.
[0063] Figure 7 Delta Nano value of epitaxial wafer under different power ratios, Figure 7 The Delta Nano values of the epitaxial wafer when the power ratio is 54%, 56%, 58% and 60% are shown respectively, wherein the blue curve is the result of dividing the epitaxial wafer into multiple 10*10mm areas, calculating the Delta Nano value of each area and taking the average value; the orange curve is the result of dividing the epitaxial wafer into multiple 2*2mm areas, calculating the Delta Nano value of each area and taking the average value.
[0064] Depend on Figure 6 and Figure 7 It can be seen that when the process conditions of the bottom heating module power ratio being 58% and 60% are adopted, pin mark defects will appear on the surface of the epitaxial wafer. However, when the process conditions of the bottom heating module power ratio being 54% and 56% are adopted, no pin mark defects will appear on the surface of the epitaxial wafer. Figure 7 As shown, when the power of the bottom heating module accounts for 56% of the process condition, the Delta Nano value of the epitaxial wafer is the smallest, indicating that this condition is the optimal process condition.
[0065] If Delta Nano does not occur continuously after adjusting the power ratio of the bottom heating module of the epitaxial furnace reaction chamber, it means that the power ratio of the bottom heating module of the epitaxial furnace reaction chamber is set unreasonably and the power ratio of the bottom heating module of the epitaxial furnace reaction chamber needs to be adjusted.
[0066] After adjusting the process conditions of the epitaxial furnace reaction chamber, if the pin mark defects of the epitaxial wafer continue to occur, it is judged that the cause of the pin mark defects is a problem with the polished wafer. If the pin mark defects of the epitaxial wafer continue to occur after using different power ratios of the bottom heating module of the epitaxial furnace reaction chamber, and the pin mark defects caused by wear of the demolding needle are also ruled out, it means that the pin mark defects come from the polished wafer. It is necessary to notify the upstream operators to improve the process of polishing the wafer.
[0067] In this embodiment, when a pin mark defect occurs in an epitaxial wafer, it is first determined whether the pin mark defect occurs continuously. If it occurs continuously, the epitaxial furnace reaction chamber base is rotated. If the position of the pin mark defect also changes accordingly, it is determined that the pin mark defect is caused by the wear of the demolding pin; if the position of the pin mark defect does not change, the process conditions of the epitaxial furnace reaction chamber are adjusted. If the pin mark defect no longer occurs, it is determined that the pin mark defect is caused by the process conditions of the epitaxial furnace reaction chamber. The technical solution of the present invention can accurately determine the cause of the pin mark defect, reduce the occurrence of misjudgment and missed judgment, and then improve the process flow according to the cause of the pin mark defect, avoid the subsequent occurrence of pin mark defects, and improve the quality of epitaxial wafers.
[0068] The embodiment of the present invention also provides a device for determining the cause of epitaxial wafer defects, such as Figure 8 As shown, including:
[0069] The first judgment module 21 is used to judge whether the pin mark defect of the epitaxial wafer occurs continuously; specifically, when more than N epitaxial wafers have pin mark defects among the M epitaxial wafers produced continuously, it is judged that the pin mark defects of the epitaxial wafer occur continuously, wherein N and M are integers greater than 1, and N is less than M. In some embodiments, M may be 25 and N may be 19. For example, if 20 epitaxial wafers have pin mark defects among a box of 25 epitaxial wafers produced, it is judged that the pin mark defects of the epitaxial wafer occur continuously; of course, the values of M and N may be adjusted according to actual production needs.
[0070] The rotation module 22 is used to rotate the base of the epitaxial furnace reaction chamber by a preset angle when the pin-mark defects of the epitaxial wafer occur continuously; in this embodiment, the base of the epitaxial furnace reaction chamber can be rotated 120° clockwise; or, the base of the epitaxial furnace reaction chamber can be rotated 240° clockwise; or, the base of the epitaxial furnace reaction chamber can be rotated 120° counterclockwise; or, the base of the epitaxial furnace reaction chamber can be rotated 240° counterclockwise.
[0071] The second judgment module 23 is used to judge whether the position of the pin-mark defect of the epitaxial wafer changes after the base of the reaction chamber of the epitaxial furnace rotates by a preset angle; the position of the pin-mark defect can be determined according to the position of the area with a higher Delta Nano value, and the Delta Nano value is equal to the difference between the Nano value of the epitaxial wafer and the Nano value of the polished wafer. If the Delta Nano value is higher, it means that a pin-mark defect occurs in the corresponding area.
[0072] The third judgment module 24 is used to judge that the cause of the pin mark defect is the wear of the ejection pin when the position of the pin mark defect of the epitaxial wafer changes; if the base of the epitaxial furnace reaction chamber rotates a certain angle, and the area with a higher Delta Nano value also rotates with the silicon wafer, it indicates that the pin mark defect is caused by the wear of the ejection pin, and the operator needs to be reminded to replace the ejection pin.
[0073] The adjustment module 25 is used to adjust the process conditions of the reaction chamber of the epitaxial furnace when the position of the pin-mark defect of the epitaxial wafer does not change.
[0074] The fourth judgment module 26 is used to judge whether the pin mark defect of the epitaxial wafer continues to occur; when the pin mark defect of the epitaxial wafer no longer occurs, it is judged that the cause of the pin mark defect is the process conditions of the epitaxial furnace reaction chamber; after adjusting the process conditions of the epitaxial furnace reaction chamber, if the pin mark defect of the epitaxial wafer continues to occur, it is judged that the cause of the pin mark defect is a problem with the polishing wafer.
[0075] If the pin mark defect on the surface of the epitaxial wafer does not rotate synchronously with the rotation of the base, it means that the pin mark defect is not caused by the wear of the ejection pin of the epitaxial furnace. The process conditions of the epitaxial furnace reaction chamber can be adjusted, such as adjusting the power ratio of the bottom heating module of the epitaxial furnace reaction chamber, to determine whether the pin mark defect continues to occur after adjusting the process conditions; when the pin mark defect of the epitaxial wafer no longer occurs, it is determined that the cause of the pin mark defect is the process conditions of the epitaxial furnace reaction chamber. If DeltaNano does not occur continuously after adjusting the power ratio of the bottom heating module of the epitaxial furnace reaction chamber, it means that the power ratio of the bottom heating module of the epitaxial furnace reaction chamber is set unreasonably, and it is necessary to adjust the power ratio of the bottom heating module of the epitaxial furnace reaction chamber. If the pin mark defect of the epitaxial wafer continues to occur after adopting different power ratios of the bottom heating module of the epitaxial furnace reaction chamber, and the pin mark defect caused by the wear of the ejection pin is also excluded, it means that the pin mark defect comes from the polished wafer. It is necessary to notify the upstream operators to improve the process of polishing wafers.
[0076] In this embodiment, when a pin mark defect occurs in an epitaxial wafer, it is first determined whether the pin mark defect occurs continuously. If it occurs continuously, the epitaxial furnace reaction chamber base is rotated. If the position of the pin mark defect also changes accordingly, it is determined that the pin mark defect is caused by the wear of the demolding pin; if the position of the pin mark defect does not change, the process conditions of the epitaxial furnace reaction chamber are adjusted. If the pin mark defect no longer occurs, it is determined that the pin mark defect is caused by the process conditions of the epitaxial furnace reaction chamber. The technical solution of the present invention can accurately determine the cause of the pin mark defect, reduce the occurrence of misjudgment and missed judgment, and then improve the process flow according to the cause of the pin mark defect, avoid the subsequent occurrence of pin mark defects, and improve the quality of epitaxial wafers.
[0077] In some embodiments, the adjustment module 25 is specifically used to adjust the power ratio of the bottom heating module of the epitaxial furnace reaction chamber, where the power ratio is the ratio of the power of the bottom heating module to the total heating power, and the total heating power is the sum of the power of the bottom heating module and the power of the top heating module of the epitaxial furnace reaction chamber.
[0078] In some embodiments, the adjustment module 25 is specifically used to adjust the value of the power ratio, and prepare an epitaxial wafer to determine whether the prepared epitaxial wafer has a pin mark defect; if the prepared epitaxial wafer still has a pin mark defect, return to the previous step and continue to adjust the value of the power ratio; if the prepared epitaxial wafer no longer has a pin mark defect or the number of times the power ratio is adjusted reaches a preset number, end the adjustment of the power ratio.
[0079] For example, the power ratio of the bottom heating module of the epitaxial furnace reaction chamber is adjusted to 60% to determine whether the prepared epitaxial wafer has pin mark defects; but if the prepared epitaxial wafer still has pin mark defects, the power ratio of the bottom heating module of the epitaxial furnace reaction chamber is further adjusted to 58% to determine whether the prepared epitaxial wafer has pin mark defects; but if the prepared epitaxial wafer still has pin mark defects, the power ratio of the bottom heating module of the epitaxial furnace reaction chamber is further adjusted to 54%. If the prepared epitaxial wafer no longer has pin mark defects, the adjustment of the power ratio of the bottom heating module of the epitaxial furnace reaction chamber can be terminated.
[0080] It should be noted that each embodiment in this specification is described in a progressive manner, and the same or similar parts between the embodiments can be referred to each other, and each embodiment focuses on the differences from other embodiments. In particular, for the embodiments, since they are basically similar to the product embodiments, the description is relatively simple, and the relevant parts can be referred to the partial description of the product embodiments.
[0081] Unless otherwise defined, the technical terms or scientific terms used in the present disclosure should be understood by people with ordinary skills in the field to which the present disclosure belongs. The "first", "second" and similar words used in the present disclosure do not indicate any order, quantity or importance, but are only used to distinguish different components. "Include" or "comprise" and similar words mean that the elements or objects appearing before the word cover the elements or objects listed after the word and their equivalents, without excluding other elements or objects. "Connect" or "connected" and similar words are not limited to physical or mechanical connections, but can include electrical connections, whether direct or indirect. "Up", "down", "left", "right" and the like are only used to indicate relative positional relationships. When the absolute position of the described object changes, the relative positional relationship may also change accordingly.
[0082] It will be understood that when an element such as a layer, film, region, or substrate is referred to as being “on” or “under” another element, it can be “directly on” or “under” the other element or intervening elements may be present.
[0083] In the description of the above embodiments, specific features, structures, materials or characteristics may be combined in a suitable manner in any one or more embodiments or examples.
[0084] The above is only a specific embodiment of the present disclosure, but the protection scope of the present disclosure is not limited thereto. Any person skilled in the art who is familiar with the technical field can easily think of changes or substitutions within the technical scope disclosed in the present disclosure, which should be included in the protection scope of the present disclosure. Therefore, the protection scope of the present disclosure should be based on the protection scope of the claims.
Claims
1. A method for determining the cause of epitaxial wafer defects, characterized in that: include: Determine whether the pin mark defects of the epitaxial wafer occur continuously; When the pin-mark defects of the epitaxial wafer occur continuously, rotating the base of the epitaxial furnace reaction chamber by a preset angle; After the base of the reaction chamber of the epitaxial furnace is rotated by a preset angle, determining whether the position of the pin mark defect of the epitaxial wafer changes; When the position of the pin mark defect of the epitaxial wafer changes, it is determined that the cause of the pin mark defect is the wear of the demolding pin; when the position of the pin mark defect of the epitaxial wafer does not change, the process conditions of the reaction chamber of the epitaxial furnace are adjusted to determine whether the pin mark defect of the epitaxial wafer continues to occur; When the pin mark defect of the epitaxial wafer no longer occurs, it is judged that the cause of the pin mark defect is the process conditions of the epitaxial furnace reaction chamber; after adjusting the process conditions of the epitaxial furnace reaction chamber, if the pin mark defect of the epitaxial wafer continues to occur, it is judged that the cause of the pin mark defect is the problem of polishing the wafer.
2. The method according to claim 1, characterized in that: Rotating the susceptor of the epitaxial furnace reaction chamber to a preset angle includes: The base of the epitaxial furnace reaction chamber is rotated 120° clockwise; or, the base of the epitaxial furnace reaction chamber is rotated 240° clockwise; or, the base of the epitaxial furnace reaction chamber is rotated 120° counterclockwise; or, the base of the epitaxial furnace reaction chamber is rotated 240° counterclockwise.
3. The method according to claim 1, characterized in that The process conditions of adjusting the reaction chamber of the epitaxial furnace include: Adjust the power proportion of the bottom heating module of the epitaxial furnace reaction chamber, where the power proportion is the ratio of the power of the bottom heating module to the total heating power, and the total heating power is the sum of the power of the bottom heating module and the power of the top heating module of the epitaxial furnace reaction chamber.
4. The method according to claim 3, characterized in that The adjusting the power proportion of the bottom heating module of the epitaxial furnace reaction chamber includes: Adjusting the value of the power ratio, preparing an epitaxial wafer, and determining whether the prepared epitaxial wafer has a pin mark defect; If the prepared epitaxial wafer still has pin mark defects, return to the previous step and continue to adjust the value of the power ratio; if the prepared epitaxial wafer no longer has pin mark defects or the number of times the power ratio is adjusted reaches a preset number, end the adjustment of the power ratio.
5. The method according to claim 1, characterized in that The step of judging whether the pin mark defects of the epitaxial wafer occur continuously comprises: When more than N epitaxial wafers have pin mark defects among M epitaxial wafers produced continuously, it is determined that the pin mark defects of the epitaxial wafers occur continuously, wherein N and M are integers greater than 1 and N is less than M.
6. An epitaxial wafer defect cause determination device, characterized in that: include: The first judgment module is used to judge whether the pin mark defects of the epitaxial wafer occur continuously; A rotating module, used for rotating the base of the reaction chamber of the epitaxial furnace by a preset angle when pin-marking defects of the epitaxial wafer occur continuously; A second judgment module is used to judge whether the position of the pin mark defect of the epitaxial wafer changes after the base of the reaction chamber of the epitaxial furnace rotates by a preset angle; The third judgment module is used to judge that the cause of the pin mark defect is the wear of the demolding pin when the position of the pin mark defect of the epitaxial wafer changes; An adjustment module, used for adjusting the process conditions of the reaction chamber of the epitaxial furnace when the position of the pin-mark defect of the epitaxial wafer does not change; The fourth judgment module is used to judge whether the pin mark defect of the epitaxial wafer continues to occur. When the pin mark defect of the epitaxial wafer no longer occurs, it is judged that the cause of the pin mark defect is the process conditions of the epitaxial furnace reaction chamber; after adjusting the process conditions of the epitaxial furnace reaction chamber, if the pin mark defect of the epitaxial wafer continues to occur, it is judged that the cause of the pin mark defect is a problem with the polishing wafer.
7. The device according to claim 6, characterized in that The rotation module is specifically used to rotate the base of the epitaxial furnace reaction chamber 120° clockwise; or, to rotate the base of the epitaxial furnace reaction chamber 240° clockwise; or, to rotate the base of the epitaxial furnace reaction chamber 120° counterclockwise; or, to rotate the base of the epitaxial furnace reaction chamber 240° counterclockwise.
8. The device according to claim 6, characterized in that The adjustment module is specifically used to adjust the power ratio of the bottom heating module of the epitaxial furnace reaction chamber, where the power ratio is the ratio of the power of the bottom heating module to the total heating power, and the total heating power is the sum of the power of the bottom heating module and the power of the top heating module of the epitaxial furnace reaction chamber.
9. The device according to claim 8, characterized in that The adjustment module is specifically used to adjust the value of the power ratio, prepare epitaxial wafers, and determine whether the prepared epitaxial wafers have pin mark defects; if the prepared epitaxial wafers still have pin mark defects, return to the previous step and continue to adjust the value of the power ratio; if the prepared epitaxial wafers no longer have pin mark defects or the number of times the value of the power ratio is adjusted reaches a preset number, end the adjustment of the value of the power ratio.
10. The device according to claim 6, characterized in that The first judgment module is specifically used to judge that the pin mark defects of the epitaxial wafers occur continuously when more than N epitaxial wafers have pin mark defects among M epitaxial wafers produced continuously, wherein N and M are integers greater than 1 and N is less than M.