A degradable composite material for injection molding and preparation method thereof
By combining polypropylene, a self-made organosilicon acrylate polymer, and glutamic acid-modified nano-CaCO3, the problem of difficult processing of injection molding materials under high temperature and high pressure was solved, the melt flow and mechanical properties of the materials were improved, and better injection molding effect and biodegradability were achieved.
Patent Information
- Application Number
- CN202411298588.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-18
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-09-18
AI Technical Summary
Existing injection molding materials are difficult to process under high temperature and high pressure conditions, have poor starch melting properties, and poor mechanical properties, making it difficult to meet the needs of injection molding.
A biodegradable composite material for injection molding was prepared by combining polypropylene, a self-made organosilicon acrylate polymer, glutamic acid-modified nano-CaCO3, heat stabilizer, plasticizer, UV absorber and degrader, and then plasticizing and extruding it into fibers after mechanical mixing and vacuum drying.
It improves the melt flowability and processing performance of the material, enhances mechanical strength and toughness, improves surface quality, and increases biodegradability.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of injection molding degradable materials, and specifically relates to a degradable composite material for injection molding and a preparation method thereof. Background Art
[0002] Traditional plastic products are mostly made by injection molding with plastic molds, which can achieve efficient production on intelligent assembly lines. Due to their low manufacturing cost and ease of use, they are widely used in catering, medical, automotive, aerospace and other fields. In order to respond to the national environmental protection policy of "green travel, low-carbon production", it is necessary to increase the research and development of new materials and new processes.
[0003] Injection molding products usually use rubber injection molding, plastic injection molding and molding injection molding. Plastic injection molding is a method of plastic products. At present, molten polyethylene, polypropylene, ABS, PA, polystyrene and other plastics are injected into plastic product molds under pressure and cooled to form plastic products. However, these plastic materials have poor degradability and put great pressure on the environment. Therefore, the research on biodegradable composite materials is the main research direction of the contemporary plastics industry.
[0004] For example, the Chinese invention patent with publication number CN116875015A discloses a degradable composite material for injection molding, which is made of the following raw materials in parts by weight: 50-70 parts of polylactic acid, 15-25 parts of polycaprolactone, 30-40 parts of starch, 3-8 parts of composite degradation catalytic fiber, 5-10 parts of sepiolite powder, 5-10 parts of talc, 2-5 parts of clay, and 1-3 parts of plasticizer.
[0005] For example, the Chinese invention patent with publication number CN104151687A discloses a degradable injection molding material, which includes, by mass percentage: 30-33% polyethylene; 25-30% polystyrene; 11-14% clay; 16-19% starch; 7-9% photosensitizer; 6-9% plasticizer; 3-5% biodegradable agent; and 5-8% impact-resistant modifier.
[0006] In the prior art, the above technical solutions all have excellent degradation performance, but the defects of the above prior art are that a considerable proportion of starch is added to the material, the starch content component in the formula is too high, and it cannot be processed under high temperature and high speed conditions, and the starch has poor melt processing performance; the heat resistance and mechanical properties of the material itself are not good enough; and injection molding is to heat the plastic particles to a molten state and then inject them into the mold for molding. The material needs to have good fluidity to fill the small cavity of the mold, and the finished product is required to have excellent mechanical properties such as strength and hardness.
[0007] Therefore, the existing technology still has huge room for improvement, and there is an urgent need to introduce new process technologies to solve the above problems and seek more feasible solutions. Summary of the invention
[0008] In order to solve the technical problems existing in the above technical solutions, the purpose of the present invention is to provide a degradable composite material for injection molding and a preparation method thereof.
[0009] The purpose of the present invention can be achieved through the following technical scheme: a degradable composite material for injection molding comprises: 60-80 parts of polypropylene, 8-16 parts of homemade silicone acrylate polymer, 10-18 parts of glutamic acid modified nano-CaCO3, 2-5 parts of heat stabilizer, 1-2 parts of plasticizer, 0.2-0.6 parts of UV absorber, 1-2 parts of polylactic acid, 1-2 parts of polybutylene terephthalate-adipate, and 0.5-1 parts of degradation agent.
[0010] The polypropylene is a mixture of homopolymer polypropylene and copolymer polypropylene;
[0011] The heat stabilizer is: any one of zinc stearate, magnesium stearate, dibutyltin dilaurate or a mixture of two thereof;
[0012] The plasticizer is any one of xylitol, mannitol and sorbitol;
[0013] The degradation agent is any one of di-tert-butyl peroxide, diisopropylbenzene peroxide and benzoyl peroxide;
[0014] The UV absorber is at least one of 2-(2H-benzotriazole-2-yl)-4-(tert-butyl-6-sec-butyl)phenol and 2-(2H-benzotriazole-2-yl)-4,6-di(1-methyl-1-phenylethyl)phenol.
[0015] Furthermore, the degradable composite material for injection molding includes, by weight: 70 parts of polypropylene, 12 parts of homemade silicone acrylate polymer, 14 parts of glutamic acid modified nano-CaCO3, 3 parts of heat stabilizer, 2 parts of plasticizer, 0.4 parts of UV absorber, 1.5 parts of polylactic acid, 1.5 parts of polybutylene terephthalate-adipate, and 0.8 parts of degradation agent.
[0016] Homemade silicone acrylate polymer: In a four-necked flask equipped with a stirrer, a constant pressure dropping funnel, a thermometer, and a condenser, add 150 g of deionized water, 1.8 g of sodium dodecyl sulfate and 0.4 g of octylphenol polyoxyethylene ether as a composite emulsifier, 0.6 g of sodium bicarbonate, and 0.6 g of acrylic acid; heat the reaction vessel to 42 degrees Celsius in an oil bath and continue stirring for 15 minutes; then add 1.5 g of vinyl triethoxysilane, 22 g of n-butyl acrylate, 7.6 g of ethyl acrylate, and 3.6 g of methyl methacrylate to the reaction vessel and stir for 1 hour. The temperature of the mixed solution was raised to 75 degrees Celsius, and then 12 g of a 2.5% KPS initiator aqueous solution was added dropwise within 1 hour; after the addition was completed, 25 g of n-butyl acrylate, 9.5 g of methyl methacrylate, 7 g of ethyl acrylate, and 0.4 g of acrylic acid were added dropwise within 1 hour; after the addition was completed, 8 g of a 2.5% KPS initiator aqueous solution was added dropwise within the next 40 minutes; then the mixture was kept warm at 74-76 degrees Celsius for 2 hours; finally The mixed solution was then cooled to 50 degrees Celsius, and 0.2 g of sodium dodecyl sulfate and 0.2 g of octylphenol polyoxyethylene ether were added; the mixture was stirred for 30 minutes, and the pH of the reaction solution was adjusted to 7-8 with aqueous ammonia, and the material was filtered out with a 300-mesh filter to obtain a homemade silicone-modified core-shell acrylate emulsion. Subsequently, a 10% concentration of CaCl2 aqueous solution was added, and after demulsification, filtering, washing and drying, a powdered homemade silicone acrylate polymer was obtained.
[0017] The preparation method of the glutamic acid modified nano-CaCO3 is as follows: 16g of nano-CaCO3 is mixed with 180g of distilled water, and then the mixed solution is ultrasonically dispersed for 2h; after the ultrasonication is completed; the mixed solution is transferred to a three-necked flask, and then placed in a constant temperature water bath, heated to 70 degrees Celsius, and the stirring rate is 800r / min; then 2g of glutamic acid is added to carry out a modification test; after continuing to stir for 2h, the solution after the reaction is filtered, washed, and vacuum dried to prepare the glutamic acid modified nano-CaCO3.
[0018] A biodegradable composite material for injection molding and a preparation method thereof. Polypropylene, a self-made silicone acrylate polymer, glutamic acid-modified nano-CaCO3, a heat stabilizer, a plasticizer, a UV absorber, and a degradation agent are poured into a physical stirring system for mechanical and physical uniform mixing; after uniform mixing, the mixture is vacuum dried; then the dried mixture is placed in a heating system for plasticization; then the plasticized mixture is subjected to secondary melt molding by a booster screw, and finally the fusion is subjected to high-pressure multi-porous extrusion and wire drawing molding; after cooling and shaping, it is then cut into particles at high speed, so as to prepare an injection molding biodegradable composite material.
[0019] During the preparation of the degradable composite material for injection molding, the plasticizing temperature is 200-210 degrees Celsius.
[0020] During the preparation of the degradable composite material for injection molding, the extrusion pressure of high-pressure extrusion is 3-4 MPa.
[0021] The present invention has the beneficial effects:
[0022] 1. The present invention introduces glutamic acid to modify nano-CaCO3, wherein the two carboxyl groups in glutamic acid are involved in the bonding of calcium ions, so the modification effect is better, the surface polarity is greatly increased, the dispersibility of nano-calcium carbonate is improved, and the agglomeration phenomenon is reduced; and the interfacial compatibility can be enhanced, and the mechanical strength and toughness can also be improved; when it is incorporated into the injection molding degradable material, the material's complex viscosity can be reduced, the crystallinity can be increased, and the polymer can be made more uniform, thereby showing more excellent mechanical properties;
[0023] 2. The self-made organosilicon acrylate polymer introduced in the present invention has a core-shell structure, wherein the organosilicon serves as a core layer and the acrylate serves as a shell layer; the core layer provides toughness and the shell layer provides strength; the tensile strength of the composite material can be greatly improved; and the main chain is composed of silicon-oxygen bonds, which have a longer bond length and a greater bond energy, and have better flexibility than carbon-carbon bonds; and the introduction of the self-made organosilicon acrylate polymer into the injection-molded degradable composite material can reduce the friction coefficient of the material surface and improve the wear resistance of the composite material;
[0024] 3. In the composite material of the present application, glutamic acid-modified nano-CaCO3 and homemade silicone acrylate polymer are used in combination, wherein the glutamic acid-modified nano-CaCO3 and the silicone acrylate polymer have good interfacial compatibility; wherein the homemade silicone acrylate polymer can reduce the internal friction of polypropylene and reduce the viscosity of the composite material, thereby improving its melt fluidity and processing performance; and in the compound use with glutamic acid-modified nano-CaCO3, the dispersion effect of glutamic acid-modified nano-CaCO3 and the rheological regulation of homemade silicone acrylate can make the composite material flow more smoothly in the molten state, which is helpful to obtain better surface quality and more complex shapes in the injection molding process;
[0025] 4. Among the components of the present application, although the heat stabilizer itself is not degradable, it can improve the long-term stability and service life of the material, indirectly affecting the environmental friendliness of the material; and the incorporation of the degradation agent in the formula can promote the decomposition of the material after use, and under the synergistic effect of the two with the UV absorber, it can greatly improve the biodegradability of the injection molding composite material. DETAILED DESCRIPTION
[0026] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with embodiment, and the illustrative embodiments of the present invention and its description are only used to explain the present invention, and are not used as limitation of the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper limit and the lower limit of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the range is also included in the present invention. The upper limit and lower limit of these smaller ranges can be independently included or excluded in the scope.
[0027] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0028] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.
[0029] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0030] The "parts" indicated in the following examples are all parts by weight.
[0031] Example 1
[0032] A degradable composite material for injection molding comprises: 60 parts of polypropylene, 8 parts of self-made silicone acrylate polymer, 10 parts of glutamic acid modified nano-CaCO3, 2 parts of heat stabilizer, 1 part of plasticizer, 0.2 parts of UV absorber, 1 part of polylactic acid, 1 part of polybutylene terephthalate-adipate, and 0.5 parts of degradation agent;
[0033] The polypropylene is a mixture of homopolymer polypropylene and copolymer polypropylene;
[0034] The heat stabilizer is: dibutyltin dilaurate;
[0035] The plasticizer is: xylitol;
[0036] The degradation agent is: benzoyl peroxide;
[0037] The UV absorber is: 2-(2H-benzotriazole-2-yl)-4-(tert-butyl-6-sec-butyl)phenol;
[0038] In the specific implementation, this Example 1 selected 30 parts of 1100N polypropylene, 18 parts of EPS30R polypropylene, and 12 parts of 7227 polypropylene.
[0039] The preparation and synthesis method of the self-made organosilicon acrylate polymer is as follows: 150g of deionized water, 1.8g of sodium dodecyl sulfate, 0.4g of octylphenol polyoxyethylene ether, 0.6g of sodium bicarbonate and 0.6g of acrylic acid are added to a four-necked flask equipped with a stirrer, a constant pressure dropping funnel, a thermometer and a condenser; the reaction container is heated to 42 degrees Celsius in an oil bath and stirred for 15 minutes; then 1.5g of vinyl triethoxysilane, 22g of n-butyl acrylate, 7.6g of ethyl acrylate and 3.6g of methyl methacrylate are added to the reaction container and stirred for 1 hour; the temperature of the mixed solution is raised to 75 degrees Celsius, and then 12g of a KPS initiator aqueous solution with a concentration of 2.5% is cumulatively added within 1 hour; after the addition is completed, 25g of acrylic acid is cumulatively added within 1 hour. n-butyl acrylate, 9.5g methyl methacrylate, 7g ethyl acrylate, 0.4g acrylic acid; after the addition is completed, within the following 40 minutes, a cumulative 8g of a 2.5% KPS initiator aqueous solution is added; then, the mixture is kept warm at 74-76 degrees Celsius for 2h; finally, the mixed solution is cooled to 50 degrees Celsius, and 0.2g of sodium dodecyl sulfate and 0.2g of octylphenol polyoxyethylene ether are added; stirred for 30 minutes, and the pH value of the reaction solution is adjusted to 7-8 with ammonia water, and the material is filtered with a 300-mesh filter to obtain a homemade silicone modified core-shell acrylate emulsion, and then a 10% concentration of CaCl2 aqueous solution is added. After demulsification, filtering, washing and drying, a powdery homemade silicone acrylate polymer is prepared.
[0040] The preparation method of the glutamic acid modified nano-CaCO3 is as follows: 16g of nano-CaCO3 is mixed with 180g of distilled water, and then the mixed solution is ultrasonically dispersed for 2h; after the ultrasonication is completed; the mixed solution is transferred to a three-necked flask, and then placed in a constant temperature water bath, heated to 70 degrees Celsius, and the stirring rate is 800r / min; then 2g of glutamic acid is added to carry out a modification test; after continuing to stir for 2h, the solution after the reaction is filtered, washed, and vacuum dried to prepare the glutamic acid modified nano-CaCO3.
[0041] A biodegradable composite material for injection molding and a preparation method thereof: polypropylene, self-made silicone acrylate polymer, glutamic acid modified nano-CaCO3, heat stabilizer, plasticizer, UV absorber and degradation agent are poured into a physical stirring system for mechanical and physical uniform mixing; after uniform mixing, the mixture is vacuum dried; then the dried mixture is placed in a heating system for plasticization, and the plasticization temperature is 180-190 degrees Celsius; then the plasticized mixture is subjected to secondary melt molding by a booster screw, and finally the fusion is subjected to high-pressure multi-porous extrusion wire drawing, and the extrusion pressure of the high-pressure extrusion is 3-4MPa; after cooling and shaping, it is then cut into particles at high speed to prepare a biodegradable composite material for injection molding.
[0042] Example 2
[0043] A degradable composite material for injection molding comprises: 65 parts of polypropylene, 10 parts of self-made silicone acrylate polymer, 12 parts of glutamic acid modified nano-CaCO3, 2 parts of heat stabilizer, 1 part of plasticizer, 0.4 parts of UV absorber, 1.2 parts of polylactic acid, 1.2 parts of polybutylene terephthalate-adipate, and 0.6 parts of degradation agent;
[0044] The polypropylene is a mixture of homopolymer polypropylene and copolymer polypropylene;
[0045] The heat stabilizer is: zinc stearate;
[0046] The plasticizer is: sorbitol;
[0047] The degradation agent is: di-tert-butyl peroxide;
[0048] The UV absorber is any one of: 2-(2H-benzotriazole-2-yl)-4,6-di(1-methyl-1-phenylethyl)phenol;
[0049] In the specific implementation, this Example 2 selected 30 parts of 1100N polypropylene, 15 parts of EPS30R polypropylene, and 20 parts of 7227 polypropylene;
[0050] Among them, in Example 2, the preparation method of the homemade silicone acrylate polymer, the preparation method of glutamic acid modified nano-CaCO3, and the preparation method of the degradable composite material for injection molding are all consistent with those in Example 1.
[0051] Example 3
[0052] A degradable composite material for injection molding comprises: 70 parts of polypropylene, 12 parts of self-made silicone acrylate polymer, 14 parts of glutamic acid modified nano-CaCO3, 3 parts of heat stabilizer, 2 parts of plasticizer, 0.4 parts of UV absorber, 1.5 parts of polylactic acid, 1.5 parts of polybutylene terephthalate-adipate, and 0.8 parts of degradation agent;
[0053] The polypropylene is a mixture of homopolymer polypropylene and copolymer polypropylene;
[0054] The heat stabilizer is a mixture of zinc stearate and magnesium stearate;
[0055] The plasticizer is: mannitol;
[0056] The degradation agent is: dicumyl peroxide;
[0057] The UV absorber is: 2-(2H-benzotriazole-2-yl)-4-(tert-butyl-6-sec-butyl)phenol;
[0058] In specific implementation, this Example 3 selected 35 parts of 1100N polypropylene, 20 parts of EPS30R polypropylene, and 15 parts of 7227 polypropylene;
[0059] Among them, in Example 3, the preparation method of the homemade silicone acrylate polymer, the preparation method of glutamic acid modified nano-CaCO3, and the preparation method of the degradable composite material for injection molding are all consistent with Example 1.
[0060] Example 4
[0061] A degradable composite material for injection molding comprises: 75 parts of polypropylene, 14 parts of self-made silicone acrylate polymer, 16 parts of glutamic acid modified nano-CaCO3, 4 parts of heat stabilizer, 2 parts of plasticizer, 0.6 parts of UV absorber, 2 parts of polylactic acid, 2 parts of polybutylene terephthalate-adipate, and 1 part of degradation agent;
[0062] The polypropylene is a mixture of homopolymer polypropylene and copolymer polypropylene;
[0063] The heat stabilizer is a mixture of zinc stearate and magnesium stearate;
[0064] The plasticizer is: sorbitol;
[0065] The degradation agent is: di-tert-butyl peroxide;
[0066] The UV absorber is at least one of: 2-(2H-benzotriazole-2-yl)-4,6-di(1-methyl-1-phenylethyl)phenol;
[0067] In specific implementation, this Example 4 uses 40 parts of 1100N polypropylene, 20 parts of EPS30R polypropylene, and 15 parts of 7227 polypropylene;
[0068] Among them, in Example 4, the preparation method of the homemade silicone acrylate polymer, the preparation method of glutamic acid modified nano-CaCO3, and the preparation method of the degradable composite material for injection molding are all consistent with Example 1.
[0069] Example 5
[0070] A degradable composite material for injection molding comprises: 80 parts of polypropylene, 16 parts of self-made silicone acrylate polymer, 18 parts of glutamic acid modified nano-CaCO3, 5 parts of heat stabilizer, 2 parts of plasticizer, 0.6 parts of UV absorber, 2 parts of polylactic acid, 2 parts of polybutylene terephthalate-adipate, and 1 part of degradation agent;
[0071] The polypropylene is a mixture of homopolymer polypropylene and copolymer polypropylene;
[0072] The heat stabilizer is a mixture of magnesium stearate and dibutyltin dilaurate;
[0073] The plasticizer is: mannitol;
[0074] The degradation agent is: dicumyl peroxide;
[0075] The UV absorber is at least one of: 2-(2H-benzotriazole-2-yl)-4,6-di(1-methyl-1-phenylethyl)phenol;
[0076] In specific implementation, this embodiment 5 uses 40 parts of 1100N polypropylene, 20 parts of EPS30R polypropylene, and 20 parts of 7227 polypropylene;
[0077] Among them, in Example 5, the preparation method of the homemade silicone acrylate polymer, the preparation method of glutamic acid modified nano-CaCO3, and the preparation method of the degradable composite material for injection molding are all consistent with Example 1.
[0078] Comparative Example 1
[0079] A degradable composite material for injection molding includes: 70 parts of polypropylene, 12 parts of self-made silicone acrylate polymer, 14 parts of nano-CaCO3, 3 parts of heat stabilizer, 2 parts of plasticizer, 0.4 parts of UV absorber, 1.5 parts of polylactic acid, 1.5 parts of polybutylene terephthalate-adipate, and 0.8 parts of degradation agent;
[0080] The polypropylene is a mixture of homopolymer polypropylene and copolymer polypropylene;
[0081] The heat stabilizer is a mixture of zinc stearate and magnesium stearate;
[0082] The plasticizer is: mannitol;
[0083] The degradation agent is: dicumyl peroxide;
[0084] The UV absorber is: 2-(2H-benzotriazole-2-yl)-4-(tert-butyl-6-sec-butyl)phenol;
[0085] In specific implementation, this comparative example 1 selected 35 parts of 1100N polypropylene, 20 parts of EPS30R polypropylene, and 15 parts of 7227 polypropylene.
[0086] This comparative example 1 is based on Example 3, except that the comparative example 1 uses nano-CaCO3 without any modification. Except for the above-mentioned different components, the preparation methods of the homemade silicone acrylate polymer and the degradable composite material for injection molding are the same as those of Example 3.
[0087] Comparative Example 2
[0088] A degradable composite material for injection molding comprises: 70 parts of polypropylene, 26 parts of glutamic acid modified nano-CaCO3, 3 parts of heat stabilizer, 2 parts of plasticizer, 0.4 parts of UV absorber, 1.5 parts of polylactic acid, 1.5 parts of polybutylene terephthalate-adipate, and 0.8 parts of degradation agent.
[0089] This comparative example 2 is based on Example 3, except that 12 parts of the homemade silicone acrylate polymer are replaced with an equal amount of glutamic acid-modified nano-CaCO3. Except for the above-mentioned different formulas, the preparation method of the degradable composite material for injection molding is the same as that of Example 3.
[0090] Comparative Example 3
[0091] A degradable composite material for injection molding comprises: 70 parts of polypropylene, 26 parts of self-made silicone acrylate polymer, 3 parts of heat stabilizer, 2 parts of plasticizer, 0.4 parts of UV absorber, 1.5 parts of polylactic acid, 1.5 parts of polybutylene terephthalate adipate and 0.8 parts of degradation agent.
[0092] This comparative example 3 is based on Example 3, except that 14 parts of glutamic acid-modified nano-CaCO3 are replaced by an equal amount of homemade silicone acrylate polymer. Except for the above-mentioned different formulas, the preparation method of the degradable composite material for injection molding is the same as that of Example 3.
[0093] Comparative Example 4
[0094] A degradable composite material for injection molding comprises: 70 parts of polypropylene, 14 parts of glutamic acid modified nano-CaCO3, 3 parts of heat stabilizer, 2 parts of plasticizer, 0.4 parts of UV absorber, 1.5 parts of polylactic acid, 1.5 parts of polybutylene terephthalate-adipate, and 0.8 parts of degradation agent.
[0095] This comparative example 4 is based on Example 3, except that the addition of the homemade silicone acrylate polymer is omitted. Except for the above-mentioned different formulas, the preparation method of the degradable composite material for injection molding is the same as that of Example 3.
[0096] Comparative Example 5
[0097] A degradable composite material for injection molding comprises: 70 parts of polypropylene, 12 parts of self-made silicone acrylate polymer, 3 parts of heat stabilizer, 2 parts of plasticizer, 0.4 parts of UV absorber, 1.5 parts of polylactic acid, 1.5 parts of polybutylene terephthalate-adipate, and 0.8 parts of degradation agent;
[0098] This comparative example 5 is based on Example 3, except that the addition of glutamic acid-modified nano-CaCO3 is omitted. Except for the above-mentioned different formulas, the preparation method of the degradable composite material for injection molding is the same as that of Example 3.
[0099] Comparative Example 6
[0100] A degradable composite material for injection molding includes: 70 parts of polypropylene, 3 parts of heat stabilizer, 2 parts of plasticizer, 0.4 parts of UV absorber, 1.5 parts of polylactic acid, 1.5 parts of polybutylene terephthalate-adipate, and 0.8 parts of degradation agent;
[0101] The polypropylene of Comparative Example 6 is specifically: 35 parts of 1100N polypropylene, 20 parts of EPS30R polypropylene, and 15 parts of 7227 polypropylene;
[0102] This comparative example 6 is based on Example 3, except that the addition of glutamic acid-modified nano-CaCO3 and homemade silicone acrylate polymer is omitted. Except for the above-mentioned different formulas, the preparation method of the degradable composite material for injection molding is consistent with that of Example 3.
[0103] Test example
[0104] The performance of the degradable composite materials for injection molding prepared in Examples 1-5 and Comparative Examples 1-6 was tested;
[0105] Rheological properties test of injection molding materials: The rheological test was carried out on a double-tube extrusion capillary rheometer. The capillary rheometer was set as follows: capillary die diameter 1.0 mm, aspect ratio 16:1, test temperature range 120-260 degrees Celsius, temperature deviation 0.1, melting time 10 minutes; the viscous flow activation energy of the composite material can be calculated;
[0106] With reference to GB / T 1040.1-2018 "Determination of tensile properties of plastics", the tensile strength of the degradable composite materials for injection molding prepared in Examples 1-5 and Comparative Examples 1-6 was completed;
[0107] The scratch resistance is tested with reference to PV3592, with a load of 10N. The scratch resistance is judged by measuring the △L on the surface of the material. The smaller the △L value, the better the scratch resistance of the material.
[0108] With reference to GB / T 1634.1-2019 “Determination of Deformation Temperature of Plastics under Load”, the heat deformation temperature of the degradable composite materials for injection molding prepared in Examples 1-5 and Comparative Examples 1-6 was tested.
[0109] The performance test results are shown in Table 1;
[0110] Table 1
[0111]
[0112] Comprehensive performance analysis: Examples 1-5 of the present application all have lower viscous flow activation energy. The lower the viscous flow activation energy, the less energy is required during flow; especially for injection molding materials; stronger fluidity can be used to mold more complex situations and obtain better surface quality during injection molding.
[0113] The components in comparative example 1 contain nano-CaCO3 without any modification. Because it is unmodified, nano-CaCO3 is easy to agglomerate, and the cross-linking and entanglement effect with the matrix molecular chain is obvious, which significantly increases the difficulty of the movement of the molecular chain; it is also impossible to obtain a more uniform dispersion in the composite material; the technical solution of the present application reduces the agglomeration phenomenon by introducing glutamic acid modified nano-CaCO3; and can enhance interfacial compatibility, and can also improve mechanical strength and toughness; it is incorporated into the injection molding degradable material, and can also reduce the material complex viscosity, increase crystallinity, make the polymer more uniform, and thus show more excellent mechanical properties. Among them, the two carboxyl groups in glutamic acid can participate in the bonding of calcium ions, so the modification effect obtained is better, greatly increasing the surface polarity and improving the dispersibility of nano calcium carbonate.
[0114] The performance indicators of viscosity flow activation energy, tensile strength, scratch resistance and heat deformation temperature of Comparative Example 2 are all poor; Comparative Example 2 replaces the homemade silicone acrylate polymer with an equal amount of glutamic acid-modified nano-CaCO3;
[0115] The results show that the various properties do not increase with the increase of the content of glutamate-modified nano-CaCO3; the possible reason is that there is a threshold value for the content of glutamate-modified nano-CaCO3. When the content of glutamate-modified nano-CaCO3 is too high, it is easy to agglomerate and cross-link with the matrix; and it may occupy the free volume of some chain segments in polypropylene. The reduction of free volume correspondingly increases the difficulty of chain segment movement, so the viscosity of the composite material increases accordingly, and the various mechanical properties also decrease.
[0116] In Comparative Example 3, 14 parts of glutamic acid-modified nano-CaCO3 were replaced by an equal amount of homemade silicone acrylate polymer; the data showed that the various properties did not increase with the proportion of homemade silicone acrylate polymer in the composite material; the introduced homemade silicone acrylate polymer had a core-shell structure, in which silicone served as the core layer and acrylate served as the shell layer; the core layer provided toughness and the shell layer provided strength; the tensile strength of the composite material could be greatly improved; and the main chain was composed of silicon-oxygen bonds, which had a longer bond length and greater bond energy, and had better flexibility than carbon-carbon bonds; and the introduction of homemade silicone acrylate polymer in the injection-molded degradable composite material could reduce the friction coefficient of the material surface and improve the wear resistance of the composite material.
[0117] Among them, Comparative Example 4 is a comparative example without adding the homemade silicone acrylate polymer, and Comparative Example 5 is a comparative example without adding glutamic acid modified nano-CaCO3; compared with Comparative Example 6 in which neither component is added, although adding either glutamic acid modified nano-CaCO3 or homemade silicone acrylate polymer alone can achieve certain performance improvement effects;
[0118] However, combined with the performance test results of Comparative Examples 2 and 3, the data show that the melt fluidity and various mechanical properties of the composite material do not increase linearly with the increase in the content of any of the above components; only when glutamic acid modified nano-CaCO3 and homemade silicone acrylate polymer are compounded in a certain proportion as in Examples 1-5, can more excellent melt fluidity and mechanical properties be achieved. The possible reason is that the compounding of glutamic acid modified nano-CaCO3 and homemade silicone acrylate polymer, wherein the glutamic acid modified nano-CaCO3 and the silicone acrylate polymer have good interface compatibility; wherein the homemade silicone acrylate polymer can reduce the internal friction of polypropylene and reduce the viscosity of the composite material, thereby improving its melt fluidity and processing performance; and in the compounding use with glutamic acid modified nano-CaCO3, the dispersion effect of glutamic acid modified nano-CaCO3 and the rheological regulation of homemade silicone acrylate can make the composite material flow more smoothly in the molten state, which is helpful to obtain better surface quality and more complex shapes during the injection molding process.
[0119] Furthermore, in the components of the present application, a heat stabilizer is added. Although the heat stabilizer itself is not degradable, it can improve the long-term stability and service life of the material, indirectly affecting the environmental friendliness of the material; and the incorporation of a degradation agent in the formula can promote the decomposition of the material after use, and under the synergistic effect of the two with the UV absorber, the biodegradability of the injection molding composite material can be greatly improved.
[0120] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A degradable composite material for injection molding, It is characterized in that The composition is as follows by weight: 60-80 parts of polypropylene, 8-16 parts of self-made silicone acrylate polymer, glutamic acid modified nano-CaCO 3 10-18 parts, heat stabilizer 2-5 parts, plasticizer 1-2 parts, UV absorber 0.2-0.6 parts, polylactic acid 1-2 parts, polybutylene terephthalate-adipate 1-2 parts, degradation agent 0.5-1 parts; The preparation and synthesis method of the self-made organosilicon acrylate polymer is as follows: deionized water, sodium dodecyl sulfate, octylphenol polyoxyethylene ether, sodium bicarbonate and acrylic acid are added to a four-necked flask; the reaction container is heated to 42 degrees Celsius in an oil bath and stirred for 15 minutes; vinyl triethoxysilane, n-butyl acrylate, ethyl acrylate and methyl methacrylate are then added to the reaction container and stirred for 1 hour; the temperature of the mixed solution is raised to 75 degrees Celsius, and then a KPS initiator aqueous solution is added dropwise within 1 hour; after the addition is completed, n-butyl acrylate is added dropwise within 1 hour. butyl ester, methyl methacrylate, ethyl acrylate, acrylic acid; after the addition is completed, a 2.5% KPS initiator aqueous solution is added within the next 40 minutes; then the mixture is kept at 74-76 degrees Celsius for 2 hours; finally, the mixed solution is cooled to 50 degrees Celsius, and sodium dodecyl sulfate and octylphenol polyoxyethylene ether are added; stirred for 30 minutes, and the pH of the reaction solution is adjusted to 7-8 with ammonia water, and the material is filtered with a 300-mesh filter to prepare a self-made silicone-modified core-shell acrylate emulsion, and then 10% CaCl is added 2 The aqueous solution is demulsified, filtered, washed and dried to prepare a powdered homemade silicone acrylate polymer.
2. The degradable composite material for injection molding according to claim 1, It is characterized in that The composition is as follows by weight: 70 parts of polypropylene, 12 parts of homemade silicone acrylate polymer, glutamic acid modified nano-CaCO 3 14 parts, 3 parts of heat stabilizer, 2 parts of plasticizer, 0.4 parts of UV absorber, 1.5 parts of polylactic acid, 1.5 parts of polybutylene terephthalate-adipate, and 0.8 parts of degradation agent.
3. The degradable composite material for injection molding according to claim 1, It is characterized in that The heat stabilizer is any one of zinc stearate, magnesium stearate and dibutyltin dilaurate or a mixture of two of them.
4. The degradable composite material for injection molding according to claim 1, It is characterized in that The plasticizer is any one of xylitol, mannitol and sorbitol.
5. The degradable composite material for injection molding according to claim 1, It is characterized in that The degradation agent is any one of di-tert-butyl peroxide, dicumyl peroxide and benzoyl peroxide.
6. The degradable composite material for injection molding according to claim 1, It is characterized in that The UV absorber is at least one of 2-(2H-benzotriazole-2-yl)-4-(tert-butyl-6-sec-butyl)phenol and 2-(2H-benzotriazole-2-yl)-4,6-di(1-methyl-1-phenylethyl)phenol.
7. A degradable composite material for injection molding according to any one of claims 1 to 6, It is characterized in that The glutamate-modified nano-CaCO 3 Preparation method: Take nano CaCO 3 Mix with distilled water, and then disperse the mixed solution by ultrasonication for 2h; after the ultrasonication is completed; The mixed solution was transferred to a three-necked flask, and then placed in a constant temperature water bath, heated to 70 degrees Celsius, and stirred at a rate of 800 r / min; glutamic acid was then added to carry out a modification test; After stirring for 2 hours, the solution after the reaction was filtered, washed, and vacuum dried to prepare glutamic acid modified nano-CaCO 3 .
8. A method for preparing a degradable composite material for injection molding according to any one of claims 1 to 6, It is characterized in that The preparation method of the degradable composite material for injection molding is as follows: polypropylene, self-made silicone acrylate polymer, glutamic acid modified nano-CaCO 3 , heat stabilizer, plasticizer, UV absorber, and degradation agent are poured into the physical stirring system for mechanical and physical uniform mixing; After being evenly mixed, the mixture is vacuum dried; the dried mixture is then placed in a heating system for plasticization; the plasticized mixture is then subjected to secondary melt molding by a booster screw, and finally the fusion is subjected to high-pressure multi-porous extrusion and wire drawing molding; after cooling and shaping, it is then cut into particles at high speed, thereby preparing an injection-molded biodegradable composite material.
9. The method for preparing a degradable composite material for injection molding according to claim 8, It is characterized in that During the preparation of the degradable composite material for injection molding, the plasticizing temperature is 200-210 degrees Celsius; during the preparation of the degradable composite material for injection molding, the extrusion pressure of high-pressure extrusion is 3-4MPa.