A battery production process, back contact battery and photovoltaic module

By using LPCVD and rinsing technology to deposit polycrystalline silicon layers of different thicknesses on both sides of the silicon wafer of the back contact cell, combined with high-temperature diffusion and laser doping, the problem of low deposition efficiency in the production of back contact cells was solved, achieving high-efficiency production and improved economic benefits.

CN118825134BActive Publication Date: 2024-11-19GOLDEN SOLAR (QUANZHOU) NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411297143.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-11-19
Estimated Expiration
2044-09-18

AI Technical Summary

Technical Problem

In the existing technology, the production process of back contact batteries requires the deposition of polycrystalline silicon layers on the front and back sides of the silicon wafer separately, which leads to problems such as low deposition efficiency, long production cycle and low economic benefits.

Method used

By depositing polycrystalline silicon layers of the same thickness on both the back and front sides of a silicon wafer simultaneously using low-pressure chemical vapor deposition (LPCVD), and removing a portion of the polycrystalline silicon layer on the front side of the wafer by rinsing, combined with high-temperature diffusion and laser doping, the thickness and doping concentration of the polycrystalline silicon layers on both sides of the silicon wafer can be differentiated.

Benefits of technology

It improves deposition efficiency, reduces equipment costs, shortens production cycles, and enhances battery conversion efficiency and economic benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118825134B_ABST
    Figure CN118825134B_ABST
Patent Text Reader

Abstract

The invention discloses a battery production process, a back contact battery and a photovoltaic module, and relates to the technical field of back contact batteries. The battery production process deposits and forms a polysilicon layer on the front and back of a silicon wafer at the same time, and then rinses and removes part of the polysilicon layer on the front of the silicon wafer, so that the thickness of the polysilicon layer on the front and back of the silicon wafer is different, thereby realizing the deposition of polysilicon layers of different thicknesses on both sides of the silicon wafer, improving deposition efficiency, reducing equipment costs, shortening production cycles, and improving economic benefits. In addition, different concentrations of doping of the polysilicon layer on the front and back of the silicon wafer are achieved through high-temperature diffusion and subsequent laser doping, thereby improving conversion efficiency, further reducing equipment costs, and improving economic benefits.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of back-contact batteries, and in particular relates to a battery production process, a back-contact battery and a photovoltaic module. Background Art

[0002] At present, in the application of tunneling polycrystalline passivation process, a thinner polysilicon layer is required on the front of the back contact cell to reduce optical absorption and increase current, and a thicker polysilicon layer is required on the back of the back contact cell to ensure the conductivity of the film layer and prevent the back polycrystalline from being damaged by chemical solutions. However, the tunneling polycrystalline is generally prepared by tubular PECVD (plasma enhanced chemical vapor deposition), which can only achieve single-sided deposition each time, so it takes two depositions to complete the coating of the front and back of the silicon wafer, with low deposition efficiency, high equipment cost, long production cycle and low economic benefits.

[0003] It should be noted that this part of the present invention only provides background technology related to the present invention and does not necessarily constitute prior art or known technology. Summary of the invention

[0004] The purpose of the present invention is to overcome the defects of the prior art that the front and back sides of silicon wafers need to be deposited sequentially during the production process, resulting in low deposition efficiency, long production cycle and low economic benefits. A battery production process, a back-contact battery and a photovoltaic module are provided. The battery production process deposits on the front and back sides of the silicon wafer at the same time to form a polysilicon layer, and then rinses and removes part of the polysilicon layer located on the front side of the silicon wafer, so that the thickness of the polysilicon layer located on the front and back sides of the silicon wafer is different, thereby realizing the deposition of polysilicon layers of different thicknesses on both sides of the silicon wafer, improving deposition efficiency, reducing equipment costs, shortening the production cycle and improving economic benefits. In addition, different concentrations of doping of the polysilicon layers on the front and back sides of the silicon wafer are achieved through high-temperature diffusion and subsequent laser doping, thereby improving conversion efficiency, further reducing equipment costs and improving economic benefits.

[0005] In order to achieve the above object, in a first aspect, the present invention provides a battery production process, comprising the following steps:

[0006] S1. Provide double-sided polished silicon wafers;

[0007] S2. depositing a protective layer on the back side of the silicon wafer;

[0008] S3. A velvet surface is formed on the front side of the silicon wafer by velvet cleaning, and then the protective layer is removed;

[0009] S4. depositing a first semiconductor layer and a second semiconductor layer on the back side and the front side of the silicon wafer respectively by low pressure chemical vapor deposition, wherein the first semiconductor layer comprises a first tunneling oxide layer, a first polysilicon layer, a first oxidation barrier layer and a second polysilicon layer which are sequentially arranged, and the second semiconductor layer comprises a second tunneling oxide layer, a third polysilicon layer, a second oxidation barrier layer and a fourth polysilicon layer which are sequentially arranged;

[0010] S5. Rinsing and removing the fourth polysilicon layer;

[0011] S6. Simultaneously performing high temperature diffusion on the first polysilicon layer, the second polysilicon layer and the third polysilicon layer to form a first doped layer, a second doped layer and a third doped layer, respectively;

[0012] S7. Remove the first oxide barrier layer by laser doping, and perform secondary doping on the first doping layer and the second doping layer to form a combined doping layer, wherein the phosphorus doping concentration of the combined doping layer is 1e20cm -3 -5e20cm -3 ;

[0013] S8. Cleaning and removing the second oxidation barrier layer and the combined doped layer due to the high temperature diffusion of S6 on the phosphorus silicon glass layer, while removing the second oxidation barrier layer;

[0014] S9. forming an anti-reflection layer on the third doped layer, and then forming a mask layer on the combined doped layer;

[0015] S10. Etching an opening on the first tunneling oxide layer, the combined doping layer and the mask layer to form a first opening region;

[0016] S11. Rinsing and removing the first tunneling oxide layer, the combined doping layer and the mask layer remaining in the first opening region, and then cleaning and removing the mask layer outside the first opening region;

[0017] S12. Depositing a third semiconductor layer on the back side of the silicon wafer so that a portion of the third semiconductor layer covers the side of the first semiconductor layer away from the silicon wafer, and another portion extends into the first opening area and covers the silicon wafer, the third semiconductor layer comprising an intrinsic amorphous silicon layer and a fourth doped layer arranged in sequence.

[0018] Preferably, S4 includes:

[0019] Evacuate and introduce oxygen until a first preset pressure is reached, then maintain the pressure and suffocate with oxygen to form a first tunneling oxide layer on the back side of the silicon wafer and a second tunneling oxide layer on the front side of the silicon wafer, wherein the thickness of the first tunneling oxide layer and the second tunneling oxide layer are both 1 nm to 2 nm;

[0020] Passing silane to react on the first tunnel oxide layer to form a first polysilicon layer, and react on the second tunnel oxide layer to form a third polysilicon layer, the thickness of the first polysilicon layer and the third polysilicon layer are both 15nm-30nm;

[0021] Evacuate and introduce oxygen until a second preset pressure is reached, then maintain the pressure and suffocate with oxygen to react and form a first oxidation barrier layer on the first polysilicon layer, and react and form a second oxidation barrier layer on the third polysilicon layer, wherein the thickness of the first oxidation barrier layer and the second oxidation barrier layer are both 0.8 nm-1.6 nm;

[0022] Silane is introduced to react on the first oxidation barrier layer to form a second polysilicon layer, and to react on the second oxidation barrier layer to form a fourth polysilicon layer. The thickness of the second polysilicon layer and the fourth polysilicon layer are both 80nm-110nm.

[0023] Preferably, in S4, the holding conditions for forming the first tunneling oxide layer and the second tunneling oxide layer are: the first preset gas pressure is 10000Pa-30000Pa, the holding time is 900s-1800s, and the holding temperature is 550°C-650°C;

[0024] And / or, the reaction conditions for forming the first polysilicon layer and the third polysilicon layer are: silane flow rate is 600sccm-800sccm, reaction temperature is 550°C-650°C, reaction gas pressure is 30Pa-60Pa, and reaction time is 250s-450s;

[0025] And / or, the holding conditions for forming the first oxidation barrier layer and the second oxidation barrier layer are: the second preset gas pressure is 10000Pa-30000Pa, the holding time is 500s-1500s, and the holding temperature is 550°C-650°C;

[0026] And / or, the reaction conditions for forming the second polysilicon layer and the fourth polysilicon layer are: silane flow rate is 600 sccm-800 sccm, reaction temperature is 550° C.-650° C., reaction gas pressure is 30 Pa-60 Pa, and reaction time is 1300 s-1600 s.

[0027] Preferably, in S5, the rinsing liquid used is an aqueous solution containing sodium hydroxide, the sodium hydroxide concentration is 1%-3%, the rinsing time is 5s-10s, and the rinsing temperature is 20°C-25°C.

[0028] Preferably, S6 includes:

[0029] Phosphorus oxychloride, oxygen and nitrogen are introduced for diffusion;

[0030] Oxygen and nitrogen are introduced for high temperature propulsion.

[0031] Preferably, in S6, the diffusion conditions are: diffusion temperature is 700° C.-800° C., phosphorus oxychloride flow rate is 50 sccm-500 sccm, oxygen flow rate is 100 sccm-1000 sccm, nitrogen flow rate is 100 sccm-1000 sccm, diffusion pressure is 50 mbar-300 mbar, and diffusion time is 300 s-900 s;

[0032] And / or, the high temperature advancement conditions are: high temperature advancement temperature is 820°C-840°C, oxygen flow rate is 1000sccm-2000sccm, nitrogen flow rate is 1000sccm-2000sccm, high temperature advancement gas pressure is 100mbar-500mbar, and high temperature advancement time is 900s-1200s.

[0033] Preferably, in S7, the doping laser is an ultraviolet laser or a green laser with a power of 5KW-18KW and a frequency of 300KHz-800KHz.

[0034] Preferably, in S8, the cleaning liquid used is an aqueous solution containing hydrofluoric acid, the mass percentage of hydrofluoric acid is 1%-10%, the mass percentage of deionized water is 90%-99%, the cleaning time is 120s-360s, and the cleaning temperature is 15°C-35°C.

[0035] Preferably, in S9, an anti-reflection layer and a mask layer are formed by plasma enhanced chemical vapor deposition, wherein the thickness of the anti-reflection layer is 100 nm-150 nm, and the thickness of the mask layer is 60 nm-90 nm.

[0036] Preferably, after S12, the battery production process further includes:

[0037] S13. Etching openings on the third semiconductor layer to form second opening regions that are alternately arranged with the first opening regions and spaced apart;

[0038] S14. Forming a conductive film layer on the back side of the silicon wafer;

[0039] S15. An isolation groove is formed on the conductive film layer so that a portion of the conductive film layer separated from each other extends into the first opening region and covers the third semiconductor layer, and another portion extends into the second opening region and covers the first semiconductor layer;

[0040] S16. Form a first electrode on the portion of the conductive film layer extending into the first opening region, and form a second electrode on the portion of the conductive film layer extending into the second opening region.

[0041] In a second aspect, the present invention provides a back-contact battery, which is manufactured by the above-mentioned battery production process.

[0042] In a third aspect, the present invention provides a photovoltaic module comprising the above-mentioned back contact cell.

[0043] Beneficial effects:

[0044] Through research, it is found that in the application of tunneling polycrystalline passivation process, polycrystalline silicon layers need to be deposited on both the front and back sides of the silicon wafer, and the thickness of the polycrystalline silicon layers on the two sides is different. The thinner polycrystalline silicon layer on the front side can reduce optical absorption and increase current, and the thicker polycrystalline silicon layer on the back side can ensure the conductivity of the film layer and prevent the back polycrystalline from being damaged by chemical solutions. It is well known that the current tubular PECVD can only achieve single-sided deposition, and the deposition efficiency is low. Based on this, further research is conducted to propose the present invention.

[0045] The battery production process provided by the present invention adopts the above-mentioned technical scheme, especially first depositing a polysilicon layer of the same thickness on the back and front of a silicon wafer simultaneously by low-pressure chemical vapor deposition (LPCVD), and then removing part of the polysilicon layer on the front of the silicon wafer by rinsing, so that the thickness of the polysilicon layer on the front and back of the silicon wafer is different, thereby realizing the deposition of polysilicon layers of different thicknesses on both sides of the silicon wafer, improving deposition efficiency, reducing equipment costs, shortening production cycles, and improving economic benefits; and realizing different concentrations of doping of the polysilicon layer on the front and back of the silicon wafer by high-temperature diffusion and subsequent laser doping, thereby improving conversion efficiency, further reducing equipment costs, and improving economic benefits.

[0046] The back contact battery provided by the present invention is produced by the above-mentioned battery production process, has a better deposition effect, and has good product quality.

[0047] The photovoltaic module provided by the present invention includes the above-mentioned back contact cell, has better photoelectric conversion efficiency and high photovoltaic power generation efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0049] Figure 1 This is a schematic diagram of the structure of a silicon wafer after double-sided polishing and cleaning according to an embodiment of the present invention;

[0050] Figure 2 This is a schematic diagram of the structure of forming a protective layer on the back side of a silicon wafer according to an embodiment of the present invention;

[0051] Figure 3 This is a schematic diagram of a structure in which a velvet surface is formed on the front side of a silicon wafer and a protective layer is removed from the back side according to an embodiment of the present invention;

[0052] Figure 4 This is a schematic diagram of a structure in which a first semiconductor layer is formed on the back side of a silicon wafer and a second semiconductor layer is formed on the front side according to an embodiment of the present invention;

[0053] Figure 5 This is a schematic diagram of a structure in which a mask layer is formed on the back side of a silicon wafer and an anti-reflection layer is formed on the front side according to an embodiment of the present invention;

[0054] Figure 6 This is a schematic diagram of a structure in which a first opening area is formed on the back side of a silicon wafer according to an embodiment of the present invention;

[0055] Figure 7 It is a schematic diagram of the structure of forming a third semiconductor layer and a second opening area on the back side of a silicon wafer according to an embodiment of the present invention;

[0056] Figure 8 It is a schematic diagram of the structure of forming a conductive film layer and an isolation groove on the back side of a silicon wafer according to an embodiment of the present invention;

[0057] Fig. 9 It is a schematic diagram of the structure of forming a first electrode and a second electrode on the back side of a silicon wafer according to an embodiment of the present invention.

[0058] Description of reference numerals:

[0059] 1-silicon wafer; 2-protective layer; 3-first tunneling oxide layer; 4-first polysilicon layer; 5-first oxidation barrier layer; 6-second polysilicon layer; 7-second tunneling oxide layer; 8-third polysilicon layer; 9-second oxidation barrier layer; 10-fourth polysilicon layer; 11-combined doping layer; 12-anti-reflection layer; 13-mask layer; 14-intrinsic amorphous silicon layer; 15-fourth doping layer; 16-conductive film layer; 17-first electrode; 18-second electrode; 19-third doping layer. DETAILED DESCRIPTION

[0060] In the present invention, unless otherwise specified, directional words such as "upper, lower, left, right" are generally understood in conjunction with the directions shown in the drawings and actual applications.

[0061] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.

[0062] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.

[0063] The endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. Among them, the terms "optional" and "optional" all mean that they may be included or not included (or may be present or not).

[0064] In the first aspect, the present invention provides a battery production process, which first deposits a polysilicon layer of the same thickness on the back and front of a silicon wafer simultaneously by low-pressure chemical vapor deposition (LPCVD), and then removes part of the polysilicon layer on the front of the silicon wafer by rinsing, so that the thickness of the polysilicon layer on the front and back of the silicon wafer is different, thereby achieving the deposition of polysilicon layers of different thicknesses on both sides of the silicon wafer, improving deposition efficiency, reducing equipment costs, shortening production cycles, and improving economic benefits; and achieving different concentrations of doping of the polysilicon layer on the front and back of the silicon wafer by high-temperature diffusion and subsequent laser doping, thereby improving conversion efficiency, further reducing equipment costs, and improving economic benefits.

[0065] The battery production process includes the following steps:

[0066] S1. Provide double-sided polished silicon wafers;

[0067] S2. depositing a protective layer on the back side of the silicon wafer;

[0068] S3. A velvet surface is formed on the front side of the silicon wafer by velvet cleaning, and then the protective layer is removed;

[0069] S4. depositing a first semiconductor layer and a second semiconductor layer on the back side and the front side of the silicon wafer respectively by low pressure chemical vapor deposition, wherein the first semiconductor layer comprises a first tunneling oxide layer, a first polysilicon layer, a first oxidation barrier layer and a second polysilicon layer which are sequentially arranged, and the second semiconductor layer comprises a second tunneling oxide layer, a third polysilicon layer, a second oxidation barrier layer and a fourth polysilicon layer which are sequentially arranged;

[0070] S5. Rinsing and removing the fourth polysilicon layer;

[0071] S6. Simultaneously performing high temperature diffusion on the first polysilicon layer, the second polysilicon layer and the third polysilicon layer to form a first doped layer, a second doped layer and a third doped layer, respectively;

[0072] S7. Remove the first oxide barrier layer by laser doping, and perform secondary doping on the first doping layer and the second doping layer to form a combined doping layer, wherein the phosphorus doping concentration of the combined doping layer is 1e20cm -3 -5e20cm -3 ;

[0073] S8. Cleaning and removing the second oxidation barrier layer and the combined doped layer due to the high temperature diffusion of S6 on the phosphorus silicon glass layer, while removing the second oxidation barrier layer;

[0074] S9. forming an anti-reflection layer on the third doped layer, and then forming a mask layer on the combined doped layer;

[0075] S10. Etching an opening on the first tunneling oxide layer, the combined doping layer and the mask layer to form a first opening region;

[0076] S11. Rinsing and removing the first tunneling oxide layer, the combined doping layer and the mask layer remaining in the first opening region, and then cleaning and removing the mask layer outside the first opening region;

[0077] S12. Depositing a third semiconductor layer on the back side of the silicon wafer so that a portion of the third semiconductor layer covers the side of the first semiconductor layer away from the silicon wafer, and another portion extends into the first opening area and covers the silicon wafer, the third semiconductor layer comprising an intrinsic amorphous silicon layer and a fourth doped layer arranged in sequence.

[0078] It should be noted that, in S1, the silicon wafer is preferably an N-type single crystal silicon wafer, and the silicon wafer can be a Czochralski single crystal silicon wafer or a cast single crystal silicon wafer.

[0079] In S2, the protective layer is a silicon nitride layer, which has a strong property of resisting corrosion by alkaline solutions, can resist alkaline corrosion in the texturing solution and protect the silicon wafer, and the thickness of the protective layer is 50nm-100nm. A reasonable thickness of the protective layer can maintain the integrity of the polishing surface and help improve the passivation level. Specifically, the protective layer can be formed by sputtering or CVD (chemical vapor deposition) method, preferably by PECVD (plasma enhanced chemical vapor deposition) method.

[0080] In S3, the silicon wafer is subjected to single-sided texturing to form a pyramid texturing surface on the front side to reduce the reflectivity. In this process, since a protective layer is provided on the back side of the silicon wafer, the texturing liquid will not affect the back side of the silicon wafer. After the texturing is completed, the protective layer is removed, and the back side of the silicon wafer is a polished surface. The texturing cleaning conditions are: the texturing time is 8min-40min, the texturing temperature is 65℃-85℃, the texturing liquid is an alkaline mixed solution, and the texturing liquid is a mixture of potassium hydroxide, a texturing additive and water, wherein the mass percentage of potassium hydroxide is 1%-5%, the mass percentage of the texturing additive is 0.5%-1%, and the texturing additive contains at least one of benzoic acid, aminotrimethylphosphonic acid, polyepoxysuccinic acid, and polyaspartic acid.

[0081] S4 consists of four stages:

[0082] The first stage: evacuate and introduce oxygen until the first preset pressure is reached, then maintain the pressure and suffocate the oxygen to form a first tunneling oxide layer on the back of the silicon wafer and a second tunneling oxide layer on the front of the silicon wafer, and the thickness of the first tunneling oxide layer and the second tunneling oxide layer are both 1nm-2nm. Preferably, in the first stage, the pressure holding conditions for forming the first tunneling oxide layer and the second tunneling oxide layer are: the first preset pressure is 10000Pa-30000Pa, the pressure holding time is 900s-1800s, and the pressure holding temperature is 550℃-650℃.

[0083] The second stage: silane is introduced to react on the first tunnel oxide layer to form a first polysilicon layer, and on the second tunnel oxide layer to form a third polysilicon layer, the thickness of the first polysilicon layer and the third polysilicon layer are both 15nm-30nm. Preferably, in the second stage, the reaction conditions for forming the first polysilicon layer and the third polysilicon layer are: silane flow rate is 600sccm-800sccm, reaction temperature is 550℃-650℃, reaction gas pressure is 30Pa-60Pa, and reaction time is 250s-450s.

[0084] The third stage: evacuate and introduce oxygen until the second preset pressure is reached, then maintain the pressure and suffocate the oxygen to react on the first polysilicon layer to form a first oxidation barrier layer, and react on the third polysilicon layer to form a second oxidation barrier layer, the thickness of the first oxidation barrier layer and the second oxidation barrier layer are both 0.8nm-1.6nm. Preferably, in the third stage, the pressure holding conditions for forming the first oxidation barrier layer and the second oxidation barrier layer are: the second preset pressure is 10000Pa-30000Pa, the pressure holding time is 500s-1500s, and the pressure holding temperature is 550℃-650℃.

[0085] The fourth stage: silane is introduced to react on the first oxidation barrier layer to form a second polysilicon layer, and on the second oxidation barrier layer to form a fourth polysilicon layer, the thickness of the second polysilicon layer and the fourth polysilicon layer are both 80nm-110nm. Preferably, in the fourth stage, the reaction conditions for forming the second polysilicon layer and the fourth polysilicon layer are: silane flow rate is 600sccm-800sccm, reaction temperature is 550℃-650℃, reaction gas pressure is 30Pa-60Pa, and reaction time is 1300s-1600s.

[0086] In S5, the front side of the silicon wafer is rinsed by water rinsing to remove the fourth polysilicon layer, so that the thickness of the polysilicon layer on the front side and the back side of the silicon wafer is different. In this process, since there is a second oxidation barrier layer between the third polysilicon layer and the fourth polysilicon layer, the second oxidation barrier layer can protect the third polysilicon layer to prevent the third polysilicon layer from being damaged or even removed. The rinsing liquid used is an aqueous solution containing sodium hydroxide, the concentration of sodium hydroxide is 1%-3%, the rinsing time is 5s-10s, and the rinsing temperature is 20℃-25℃.

[0087] S6 consists of two stages:

[0088] The first stage: introducing phosphorus oxychloride, oxygen and nitrogen for diffusion. Preferably, in the first stage, the diffusion conditions are: diffusion temperature is 700°C-800°C, phosphorus oxychloride flow rate is 50sccm-500sccm, oxygen flow rate is 100sccm-1000sccm, nitrogen flow rate is 100sccm-1000sccm, diffusion pressure is 50mbar-300mbar, and diffusion time is 300s-900s.

[0089] The second stage: introducing oxygen and nitrogen for high temperature advancement. Preferably, in the second stage, the high temperature advancement conditions are: high temperature advancement temperature is 820°C-840°C, oxygen flow rate is 1000sccm-2000sccm, nitrogen flow rate is 1000sccm-2000sccm, high temperature advancement gas pressure is 100mbar-500mbar, and high temperature advancement time is 900s-1200s.

[0090] In S6, since the first polysilicon layer and the third polysilicon layer are relatively thin, the first polysilicon layer and the third polysilicon layer require a relatively low doping concentration. In this regard, a first oxidation barrier layer is provided outside the first polysilicon layer, and the first oxidation barrier layer can play a certain role in blocking diffusion of the first polysilicon layer, so as to reduce the doping of the first polysilicon layer, so that the doping concentration of the first doped layer is relatively low; a second oxidation barrier layer is provided outside the third polysilicon layer, and the second oxidation barrier layer can play a certain role in blocking diffusion of the third polysilicon layer, so as to reduce the doping of the third polysilicon layer, so that the doping concentration of the third doped layer is relatively low. Specifically, the first oxidation barrier layer and the second oxidation barrier layer are both silicon oxide layers.

[0091] In S7, the first doping layer and the second doping layer are doped for a second time by laser doping. In this process, the high temperature generated by the laser and the diffusion of phosphorus impurities destroy the first oxidation barrier layer to remove the first oxidation barrier layer, and the first doping layer and the second doping layer are combined to form a combined doping layer. Since the combined doping layer is doped for a second time, and the third doping layer is not doped for a second time, the doping concentrations of the combined doping layer and the third doping layer are different, that is, the doping concentrations of the polysilicon layer on the front and back of the silicon wafer are different. Specifically, the doping laser is an ultraviolet laser or a green laser, that is, the doping laser is a flat-top picosecond green laser (wavelength of 532nm) or a flat-top picosecond ultraviolet laser (wavelength of 355nm), with a power of 5KW-18KW and a frequency of 300KHz-800KHz.

[0092] In S8, the cleaning liquid used is an aqueous solution containing hydrofluoric acid, the mass percentage of hydrofluoric acid is 1%-10%, the mass percentage of deionized water is 90%-99%, the cleaning time is 120s-360s, and the cleaning temperature is 15℃-35℃.

[0093] In S9, an anti-reflection layer and a mask layer are formed by plasma enhanced chemical vapor deposition, wherein the anti-reflection layer and the mask layer are both silicon nitride layers, the thickness of the anti-reflection layer is 100nm-150nm, and the thickness of the mask layer is 60nm-90nm.

[0094] S9 consists of two stages:

[0095] The first stage: silane and ammonia are introduced, and react to form an anti-reflection layer under the condition of turning on the glow. Preferably, in the first stage, the reaction conditions for forming the anti-reflection layer are: reaction temperature of 400°C-450°C, silane flow rate of 1200sccm-1600sccm, ammonia flow rate of 5000sccm-8000sccm, reaction time of 1000s-1500s, reaction pressure of 500mtorr-3000mtorr, and power of 4000W-6000W.

[0096] The second stage: silane and ammonia are introduced, and react to form a mask layer under the condition of turning on the glow. Preferably, in the second stage, the reaction conditions for forming the mask layer are: reaction temperature of 400°C-450°C, silane flow rate of 1200sccm-1600sccm, ammonia flow rate of 3000sccm-5000sccm, reaction time of 400s-800s, reaction pressure of 500mtorr-3000mtorr, and power of 4000W-6000W.

[0097] In S10, laser or mask etching is used to etch an opening on the mask layer, the combined doping layer and the first tunneling oxide layer on the back of the silicon wafer to form a first opening area, and the mask layer, the combined doping layer and the first tunneling oxide layer in the first opening area are etched away, and the width of the first opening area W1 is 0.3 mm-0.6 mm. Laser etching is preferred, and the laser used for etching is an ultraviolet laser or a green laser, and the pulse width is less than 100 ns.

[0098] In S11, the first tunneling oxide layer, the combined doping layer and the mask layer remaining in the first opening region are removed by rinsing on water; and then the mask layer outside the first opening region is cleaned and removed.

[0099] In S12, a third semiconductor layer is deposited on the back of the silicon wafer by PECVD (plasma enhanced chemical vapor deposition), wherein the intrinsic amorphous silicon layer has a thickness of 5nm-15nm, the fourth doped layer is a P-type doped amorphous or microcrystalline silicon layer, the thickness of the fourth doped layer is 10nm-35nm, and the boron doping concentration in the fourth doped layer is 1e19cm -3 -4e20cm -3 .

[0100] Preferably, after S12, the battery production process further includes:

[0101] S13. Etching openings on the third semiconductor layer to form second opening regions that are alternately arranged with the first opening regions and spaced apart;

[0102] S14. Forming a conductive film layer on the back side of the silicon wafer;

[0103] S15. An isolation groove is formed on the conductive film layer so that a portion of the conductive film layer separated from each other extends into the first opening region and covers the third semiconductor layer, and another portion extends into the second opening region and covers the first semiconductor layer;

[0104] S16. Form a first electrode on the portion of the conductive film layer extending into the first opening region, and form a second electrode on the portion of the conductive film layer extending into the second opening region.

[0105] It should be noted that in S13, an opening is etched on the third semiconductor layer on the back of the silicon wafer by laser or mask etching to form a second opening area, and the third semiconductor layer in the second opening area is etched away. The width of the second opening area W2 is 0.1 mm-0.3 mm. Laser etching is preferred, and the etching laser is an ultraviolet laser or a green laser, and the pulse width is less than 50 ns.

[0106] In S14, a conductive film layer is deposited on the back of the silicon wafer using physical vapor deposition technology (PVD) or activated plasma deposition technology (RPD). The thickness of the conductive film layer is 40nm-80nm. The material of the conductive film layer can be an indium oxide film doped with tin oxide, titanium oxide, zinc oxide or gallium oxide, or a zinc oxide film doped with aluminum oxide, gallium oxide or boron oxide.

[0107] In S15, an isolation groove is formed on the conductive film layer by laser or etching. The isolation groove is used to achieve the insulation function between two adjacent conductive film layers. The isolation groove is located between the first opening area and the second opening area. The width of the isolation groove W3 is 30μm-200μm.

[0108] In S16, the silver gate electrode can be formed by screen printing and low temperature sintering, or the gate line electrode can be formed by electroplating. Preferably, the gate line electrode is formed by electroplating (the first electrode and the second electrode are both formed by electroplating).

[0109] In a second aspect, the present invention provides a back-contact battery, which is manufactured by the above-mentioned battery production process.

[0110] In a third aspect, the present invention provides a photovoltaic module comprising the above-mentioned back contact cell.

[0111] The embodiments of the present invention are described in detail below, which are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention.

[0112] Example 1

[0113] A back contact battery is prepared by the following steps:

[0114] S1. Figure 1 As shown, the N-type single crystal silicon wafer 1 is double-sided polished and cleaned, and the silicon wafer 1 is a Czochralski single crystal silicon wafer 1.

[0115] S2. Figure 2 As shown, a protection layer 2 is deposited on the back side of the silicon wafer 1 by sputtering, and the thickness of the protection layer 2 is 70 nm.

[0116] S3. Figure 3As shown, a textured surface is formed on the front side of the silicon wafer 1 through textured cleaning, and then the protective layer 2 is removed, wherein the textured cleaning conditions are: the textured time is 20 minutes, the textured temperature is 75°C, the textured liquid is an alkaline mixed solution, and the textured liquid is a mixture of potassium hydroxide, a textured additive and water, wherein the mass percentage of potassium hydroxide is 3%, the mass percentage of the textured additive is 0.75%, and the textured additive contains benzoic acid and aminotri(methylene)phosphoric acid.

[0117] S4. Figure 4 As shown, by low-pressure chemical vapor deposition, the first semiconductor layer and the second semiconductor layer are deposited on the back and front of the silicon wafer 1 respectively at the same time, and the deposition process is:

[0118] In the first stage, vacuum is first drawn, and then oxygen is introduced until the pressure reaches 20000 Pa, and then the oxygen is stopped, and the pressure is maintained for 1300 seconds. The pressure maintenance temperature is 600°C, and the thickness of the first tunneling oxide layer 3 and the second tunneling oxide layer 7 formed are both 1.5 nm;

[0119] In the second stage, silane is introduced, the silane flow rate is 700 sccm, the reaction temperature is 600° C., the reaction pressure is 40 Pa, the reaction time is 350 s, and the thickness of the formed first polysilicon layer 4 and the third polysilicon layer 8 are both 20 nm;

[0120] In the third stage, vacuum is firstly drawn, and then oxygen is introduced until the gas pressure reaches 20000 Pa, and then the oxygen is stopped, and the pressure is maintained for 1000 seconds. The pressure maintenance temperature is 600° C. The thickness of the first oxidation barrier layer 5 and the second oxidation barrier layer 9 formed are both 1.2 nm;

[0121] In the fourth stage, silane is introduced with a flow rate of 700 sccm, a reaction temperature of 600° C., a reaction pressure of 40 Pa, and a reaction time of 1400 s. The thickness of the formed second polysilicon layer 6 and the fourth polysilicon layer 10 are both 100 nm.

[0122] S5. Figure 5 As shown, the fourth polysilicon layer 10 is rinsed and removed, wherein the rinsing liquid used is an aqueous solution containing sodium hydroxide, the sodium hydroxide concentration is 2%, the rinsing time is 7 seconds, and the rinsing temperature is 22°C.

[0123] S6. Figure 5 As shown, the first polysilicon layer 4, the second polysilicon layer 6 and the third polysilicon layer 8 are simultaneously subjected to high temperature diffusion to form a first doping layer, a second doping layer and a third doping layer 19, respectively. The high temperature diffusion process is:

[0124] In the first stage, phosphorus oxychloride, oxygen and nitrogen were introduced for diffusion, the diffusion temperature was 750°C, the phosphorus oxychloride flow rate was 300 sccm, the oxygen flow rate was 500 sccm, the nitrogen flow rate was 5000 sccm, the diffusion pressure was 150 mbar, and the diffusion time was 600 s;

[0125] In the second stage, oxygen and nitrogen were introduced for high-temperature advancement. The high-temperature advancement temperature was 830°C, the oxygen flow rate was 1500sccm, the nitrogen flow rate was 1500sccm, the high-temperature advancement pressure was 300mbar, and the high-temperature advancement time was 1000s.

[0126] S7. Figure 5 As shown, the first oxidation barrier layer 5 is removed by laser doping, and the first doping layer and the second doping layer are doped again to form a combined doping layer 11. The phosphorus doping concentration of the combined doping layer 11 is 3e20cm -3 , where the doped laser is a green laser with a power of 6KW and a frequency of 300KHz.

[0127] S8. Figure 5 As shown, the second oxidation barrier layer 9 and the phosphosilicate glass layer produced by the high-temperature diffusion of S6 on the combined doping layer 11 are cleaned and removed, and the second oxidation barrier layer 9 is removed at the same time, wherein the cleaning liquid used is an aqueous solution containing hydrofluoric acid, the mass percentage of hydrofluoric acid is 5%, the mass percentage of deionized water is 95%, the cleaning time is 5 minutes, and the cleaning temperature is 20°C.

[0128] S9. Figure 5 As shown, an anti-reflection layer 12 is formed on the third doping layer 19, and then a mask layer 13 is formed on the combined doping layer 11. The deposition process is as follows:

[0129] In the first stage, silane and ammonia are introduced and reacted to form an anti-reflection layer 12 under the condition of turning on the glow. The reaction temperature is 420° C., the silane flow rate is 1400 sccm, the ammonia flow rate is 6000 sccm, the reaction time is 1200 s, the reaction pressure is 2000 mtorr, the power is 5000 W, and the thickness of the formed anti-reflection layer 12 is 120 nm.

[0130] In the second stage, silane and ammonia are introduced and reacted under the condition of turning on the glow to form a mask layer 13. The reaction temperature is 420°C, the silane flow rate is 1400sccm, the ammonia flow rate is 4000sccm, the reaction time is 600s, the reaction pressure is 2000mtorr, the power is 5000W, and the thickness of the formed mask layer 13 is 70nm.

[0131] S10. Figure 6As shown, an opening is etched on the first tunneling oxide layer 3, the combined doping layer 11 and the mask layer 13 to form a first opening area. The width of the first opening area W1 is 0.4 mm. The laser used for etching is a green laser with a pulse width of 50 ns.

[0132] S11. Rinsing to remove the first tunneling oxide layer 3, the combined doping layer 11 and the mask layer 13 remaining in the first opening region, and then cleaning to remove the mask layer 13 outside the first opening region.

[0133] S12. Figure 7 As shown, a third semiconductor layer is deposited on the back of the silicon wafer 1. The third semiconductor layer includes an intrinsic amorphous silicon layer 14 and a fourth doped layer 15 arranged in sequence. The intrinsic amorphous silicon layer 14 has a thickness of 10 nm, the fourth doped layer 15 has a thickness of 20 nm, and the boron doping concentration in the fourth doped layer 15 is 3e20 cm -3 .

[0134] S13. Figure 7 As shown, an opening is etched on the third semiconductor layer to form a second opening area that is alternately arranged with the first opening area and spaced apart. The width of the second opening area W2 is 0.2 mm. The laser used for etching is a green laser with a pulse width of 20 ns.

[0135] S14. Figure 8 As shown, a conductive film layer 16 is formed on the back of the silicon wafer 1 by physical vapor deposition (PVD) technology. The thickness of the conductive film layer 16 is 60 nm, and the material of the conductive film layer 16 is a tin oxide-doped indium oxide film.

[0136] S15. Figure 8 As shown, an isolation groove W3 is opened on the conductive film layer 16 by laser, and the width of the isolation groove W3 is 100 μm.

[0137] S16. Fig. 9 As shown, a first electrode 17 is formed on a portion of the conductive film layer 16 extending into the first opening region by electroplating, and a second electrode 18 is formed on a portion of the conductive film layer 16 extending into the second opening region.

[0138] Example 2

[0139] The method of Example 1 is followed, except that the reaction conditions for forming the second polysilicon layer 6 and the fourth polysilicon layer 10 in S4 are adjusted so that the silane flow rate is 600 sccm, the reaction temperature is 550°C, the reaction gas pressure is 30 Pa, the reaction time is 1300 s, and the thickness of the second polysilicon layer and the fourth polysilicon layer 10 formed are both 80 nm.

[0140] Example 3

[0141] The method of Example 1 is referred to, except that the rinsing conditions in S5 are adjusted so that the sodium hydroxide concentration is 1%, the rinsing time is 5 s, and the rinsing temperature is 20°C.

[0142] Example 4

[0143] The method of Example 1 is followed, except that the high-temperature advancement conditions in S6 are adjusted so that the high-temperature advancement temperature is 820°C, the oxygen flow rate is 1000sccm, the nitrogen flow rate is 1000sccm, the high-temperature advancement gas pressure is 100mbar, and the high-temperature advancement time is 900s.

[0144] Example 5

[0145] The method of Example 1 is followed, except that the laser doping conditions in S7 are adjusted so that the doping laser is an ultraviolet laser with a power of 18KW and a frequency of 800KHz, and the phosphorus doping concentration of the combined doping layer 11 is 5e20cm -3 .

[0146] Comparative Example 1

[0147] The method of Example 1 is followed, except that the reaction conditions for forming the second polysilicon layer 6 and the fourth polysilicon layer 10 in S4 are adjusted so that the silane flow rate is 400 sccm, the reaction temperature is 660°C, the reaction gas pressure is 20 Pa, the reaction time is 500 s, and the thickness of the second polysilicon layer and the fourth polysilicon layer 10 formed are both 60 nm.

[0148] Comparative Example 2

[0149] The method of Example 1 is referred to, except that the rinsing conditions in S5 are adjusted so that the sodium hydroxide concentration is 0.5%, the rinsing time is 3 seconds, and the rinsing temperature is 15°C.

[0150] Comparative Example 3

[0151] The method of Example 1 is referred to, except that the high-temperature advancement conditions in S6 are adjusted so that the high-temperature advancement temperature is 700°C, the oxygen flow rate is 800sccm, the nitrogen flow rate is 800sccm, the high-temperature advancement gas pressure is 70mbar, and the high-temperature advancement time is 700s.

[0152] Comparative Example 4

[0153] The method of Example 1 is followed, except that the laser doping conditions in S7 are adjusted so that the doping laser is an ultraviolet laser with a power of 25KW and a frequency of 1200KHz, and the phosphorus doping concentration of the combined doping layer 11 is 8e20cm -3 .

[0154] Test Case

[0155] The back contact cells obtained in the above examples and comparative examples were subjected to performance tests, and the results are shown in the following performance index comparison table.

[0156] Performance index comparison table:

[0157]

[0158] It can be seen from the above performance index comparison table that, relative to the comparative example, the embodiment scheme of the present invention is adopted, firstly, a polysilicon layer of the same thickness is deposited on the back and front sides of the silicon wafer 1 simultaneously by low-pressure chemical vapor deposition (LPCVD), and then a part of the polysilicon layer located on the front side of the silicon wafer 1 is removed by rinsing, so that the thickness of the polysilicon layer located on the front and back sides of the silicon wafer 1 is different, thereby realizing the deposition of polysilicon layers of different thicknesses on both sides of the silicon wafer 1, improving deposition efficiency, reducing equipment costs, shortening production cycles, and improving economic benefits; and realizing doping of the polysilicon layers of different concentrations on the front and back sides of the silicon wafer 1 by high-temperature diffusion and subsequent laser doping, thereby improving conversion efficiency, further reducing equipment costs, and improving economic benefits.

[0159] Furthermore, according to Example 1 and Examples 2-5, it can be seen that the preferred battery structure of the present invention is more conducive to reducing optical absorption while ensuring conductivity, increasing current, and improving battery conversion efficiency.

[0160] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A battery production process, characterized in that: The following steps are involved: S1. Provide double-sided polished silicon wafers; S2. depositing a protective layer on the back side of the silicon wafer; S3. By cleaning the velvet surface, a velvet surface is formed on the front side of the silicon wafer, and then the protective layer is removed; S4. depositing a first semiconductor layer and a second semiconductor layer on the back side and the front side of the silicon wafer respectively by low pressure chemical vapor deposition, wherein the first semiconductor layer comprises a first tunneling oxide layer, a first polysilicon layer, a first oxidation barrier layer and a second polysilicon layer arranged in sequence, and the second semiconductor layer comprises a second tunneling oxide layer, a third polysilicon layer, a second oxidation barrier layer and a fourth polysilicon layer arranged in sequence, the first polysilicon layer and the third polysilicon layer have the same thickness, and the second polysilicon layer and the fourth polysilicon layer have the same thickness; S5. Rinsing and removing the fourth polysilicon layer, so that the thickness of the polysilicon layer located on the front and back sides of the silicon wafer is different; S6. Simultaneously performing high temperature diffusion on the first polysilicon layer, the second polysilicon layer and the third polysilicon layer to form a first doped layer, a second doped layer and a third doped layer, respectively; S7. removing the first oxidation barrier layer by laser doping, and performing secondary doping on the first doping layer and the second doping layer to form a combined doping layer, wherein the phosphorus doping concentration of the combined doping layer is 1e20cm -3 -5e20cm -3 , the combined doping layer and the third doping layer have different doping concentrations; S8. Cleaning and removing the second oxidation barrier layer and the combined doped layer due to the high temperature diffusion of S6 produced by the phosphorus silicon glass layer, while removing the second oxidation barrier layer; S9. forming an anti-reflection layer on the third doped layer, and then forming a mask layer on the combined doped layer; S10. Etching an opening on the first tunneling oxide layer, the combined doping layer and the mask layer to form a first opening region; S11. Rinsing and removing the first tunneling oxide layer, the combined doping layer and the mask layer remaining in the first opening region, and then cleaning and removing the mask layer outside the first opening region; S12. Depositing a third semiconductor layer on the back side of the silicon wafer so that a portion of the third semiconductor layer covers the side of the first semiconductor layer away from the silicon wafer, and another portion extends into the first opening area and covers the silicon wafer, wherein the third semiconductor layer includes an intrinsic amorphous silicon layer and a fourth doping layer arranged in sequence.

2. The battery production process according to claim 1, characterized in that: S4 includes: Evacuating and introducing oxygen until a first preset pressure is reached, and then maintaining the pressure and sealing with oxygen to form the first tunneling oxide layer on the back side of the silicon wafer and the second tunneling oxide layer on the front side of the silicon wafer, wherein the thickness of the first tunneling oxide layer and the second tunneling oxide layer are both 1 nm-2 nm; Passing silane to react on the first tunnel oxide layer to form the first polysilicon layer, and to react on the second tunnel oxide layer to form the third polysilicon layer, wherein the thickness of the first polysilicon layer and the third polysilicon layer are both 15 nm-30 nm; Evacuate and introduce oxygen until a second preset pressure is reached, then maintain the pressure and ventilate with oxygen to form a first oxidation barrier layer on the first polysilicon layer and a second oxidation barrier layer on the third polysilicon layer, wherein the thickness of the first oxidation barrier layer and the second oxidation barrier layer are both 0.8 nm to 1.6 nm; Silane is introduced to react on the first oxidation barrier layer to form the second polysilicon layer, and to react on the second oxidation barrier layer to form the fourth polysilicon layer. The thickness of the second polysilicon layer and the fourth polysilicon layer are both 80nm-110nm.

3. The battery production process according to claim 2, characterized in that: In S4, the holding conditions for forming the first tunneling oxide layer and the second tunneling oxide layer are: the first preset gas pressure is 10000Pa-30000Pa, the holding time is 900s-1800s, and the holding temperature is 550°C-650°C; and / or, the reaction conditions for forming the first polysilicon layer and the third polysilicon layer are: silane flow rate is 600 sccm-800 sccm, reaction temperature is 550° C.-650° C., reaction gas pressure is 30 Pa-60 Pa, and reaction time is 250 s-450 s; And / or, the holding conditions for forming the first oxidation barrier layer and the second oxidation barrier layer are: the second preset gas pressure is 10000Pa-30000Pa, the holding time is 500s-1500s, and the holding temperature is 550°C-650°C; And / or, the reaction conditions for forming the second polysilicon layer and the fourth polysilicon layer are: silane flow rate is 600sccm-800sccm, reaction temperature is 550°C-650°C, reaction gas pressure is 30pa-60pa, and reaction time is 1300s-1600s.

4. The battery production process according to claim 1, characterized in that: In S5, the rinsing liquid used is an aqueous solution containing sodium hydroxide, the sodium hydroxide concentration is 1%-3%, the rinsing time is 5s-10s, and the rinsing temperature is 20℃-25℃.

5. The battery production process according to claim 1, characterized in that S6 include: Phosphorus oxychloride, oxygen and nitrogen are introduced for diffusion; Oxygen and nitrogen are introduced for high temperature propulsion.

6. The battery production process according to claim 5, characterized in that: In S6, the diffusion conditions are: diffusion temperature is 700°C-800°C, phosphorus oxychloride flow rate is 50sccm-500sccm, oxygen flow rate is 100sccm-1000sccm, nitrogen flow rate is 100sccm-1000sccm, diffusion pressure is 50mbar-300mbar, and diffusion time is 300s-900s; And / or, the high temperature advancement conditions are: high temperature advancement temperature is 820°C-840°C, oxygen flow rate is 1000sccm-2000sccm, nitrogen flow rate is 1000sccm-2000sccm, high temperature advancement gas pressure is 100mbar-500mbar, and high temperature advancement time is 900s-1200s.

7. The battery production process according to claim 1, characterized in that: In S7, the doped laser is an ultraviolet laser or a green laser with a power of 5KW-18KW and a frequency of 300KHz-800KHz.

8. The battery production process according to claim 1, characterized in that: In S8, the cleaning liquid used is an aqueous solution containing hydrofluoric acid, the mass percentage of hydrofluoric acid is 1%-10%, the mass percentage of deionized water is 90%-99%, the cleaning time is 120s-360s, and the cleaning temperature is 15℃-35℃.

9. The battery production process according to claim 1, characterized in that: In S9, the anti-reflection layer and the mask layer are formed by plasma enhanced chemical vapor deposition, wherein the thickness of the anti-reflection layer is 100 nm-150 nm, and the thickness of the mask layer is 60 nm-90 nm.

10. The battery production process according to claim 1, characterized in that: After S12, the battery production process further includes: S13. Etching openings on the third semiconductor layer to form second opening regions that are alternately and spaced apart from the first opening regions; S14 forming a conductive film layer on the back side of the silicon wafer; S15. An isolation groove is formed on the conductive film layer so that a portion of the conductive film layer separated from each other extends into the first opening area and covers the third semiconductor layer, and another portion extends into the second opening area and covers the first semiconductor layer; S16. Form a first electrode on the portion of the conductive film layer extending into the first opening region, and form a second electrode on the portion of the conductive film layer extending into the second opening region.

11. A back contact battery, characterized in that: The battery is prepared by the battery production process according to any one of claims 1 to 10.

12. A photovoltaic module, characterized in that: Comprising a back contact cell as claimed in claim 11.