Preparation process of interface regulation and control artificial antiferromagnetic coupling field structure

By changing the composition ratio of the interface magnetic layer and non-magnetic layer and adjusting the lattice adaptation ratio, the interlayer exchange coupling strength of the artificial antiferromagnet is enhanced, solving the problem of weak interlayer exchange coupling in the existing technology, and realizing Effective regulation and application expansion of antiferromagnetic coupling strength.

CN118829346APending Publication Date: 2024-10-22INST OF SENSOR TECH GANSU ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410807125.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

The interlayer exchange coupling effect in existing artificial antiferromagnets is weak, making it difficult to effectively control the antiferromagnetic coupling strength, which limits their expansion in applications such as magnetic sensors and magnetic random access memories.

Method used

By changing the composition ratio of the interface magnetic layer and non-magnetic layer in the artificial antiferromagnetic structure, the lattice adaptation ratio is adjusted, thereby adjusting the interlayer exchange coupling strength, increasing the change rate of thin film magnetoresistance, and enhancing the antiferromagnetic coupling strength.

Benefits of technology

It achieves effective adjustment of the coupling strength of artificial antiferromagnetic films, increases the interlayer exchange coupling strength and magnetoresistance change rate, and expands its application fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118829346A_ABST
    Figure CN118829346A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation process of an interface regulation and control artificial antiferromagnetic coupling field structure, and relates to the technical field of spintronics and information. The artificial antiferromagnetic structure comprises a substrate, a buffer layer, a seed layer, a lower magnetic layer, a lower interface magnetic layer, a non-magnetic layer, an upper interface magnetic layer, an upper magnetic layer and a protective layer from bottom to top. According to the method, in an artificial antiferromagnetic structure, the atomic ratio in a non-magnetic layer / magnetic layer interface magnetic layer is changed, and the position of a Fermi level is adjusted through the atomic ratio, so that a band gap between a conduction band and a valence band is minimum, electrons are prone to transition, the number of spin polarization conductive electrons in the magnetic layer is increased, spin polarization of the conductive electrons of a spacing layer is induced, and therefore, the electromagnetic field of the magnetic layer is improved. And the interlayer exchange coupling strength is enhanced, so that an antiferromagnetic coupling field is enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the fields of information technology and spin electronics, and specifically relates to a preparation process of an interface-regulated artificial antiferromagnetic coupling field structure. Background Art

[0002] Artificial antiferromagnetic structure: magnetic layer / non-magnetic layer / magnetic layer, two ferromagnetic layers are separated by a thin spacer layer of non-magnetic transition metal, and the magnetic layers are coupled through interlayer exchange. Theorists have designed various models to help better understand the mechanism of interlayer exchange coupling, such as: free electron model, Ruderman-Kittel-Kasuya-Yosida (RKKY) model, hole confinement model, quantum interference model, Anderson model. These models all rely on some simplified assumptions, but share the same basic physical picture for the coupling mechanism: the ferromagnetic layer induces the spin polarization of the conduction electrons in the spacer layer, and this polarization extends to the entire spacer layer and eventually interacts with the second ferromagnetic layer, resulting in an effective exchange interaction.

[0003] The interlayer exchange coupling in artificial antiferromagnets is much weaker than the direct exchange (or superexchange coupling) between the internal magnetic moments of antiferromagnets, which makes the arrangement of magnetic moments in artificial antiferromagnets easier to control. In artificial antiferromagnets, the interlayer coupling type of adjacent ferromagnetic layers is controlled by changing the thickness of the non-magnetic spacer layer to be ferromagnetic coupling (parallel arrangement) or antiferromagnetic coupling (antiparallel arrangement), and as the thickness of the spacer layer increases, the interlayer exchange coupling strength is gradually suppressed.

[0004] Artificial antiferromagnetic structures have the advantages of relatively low stray fields, good thermal stability, and fast high-frequency response, and are widely used in magnetic sensors and magnetic random access memories. By regulating the stray fields of artificial antiferromagnetic structures, their stability and sensitivity can be regulated; in addition, the coupling between magnetic layers will also produce additional degrees of freedom. The physical mechanisms for regulating the strength of the interlayer coupling of artificial antiferromagnetic structures include mechanisms based on the band structure of the conduction electrons in the intermediate layer, mechanisms based on the interface effect between the magnetic layer and the intermediate layer, and mechanisms based on the strength of the spin coupling inside the magnetic layer. Therefore, designing artificial antiferromagnetic structures of different systems and conducting in-depth research on interlayer exchange coupling will help expand their application areas and provide relevant technical support, and are of great significance and value in both basic research and application. Summary of the invention

[0005] The invention provides a preparation process of an interface-regulated artificial antiferromagnetic coupling field structure, aiming to provide a new regulation method to enhance the antiferromagnetic coupling strength.

[0006] To this end, the present invention adopts the following technical solutions: A structure for interface-regulated artificial antiferromagnetic coupling field, wherein the artificial antiferromagnetic structure is, from bottom to top, a substrate, a buffer layer, a seed layer, a lower magnetic layer, a lower interface magnetic layer, a non-magnetic layer, an upper interface magnetic layer, an upper magnetic layer and a protective layer.

[0007] A preparation process of the structure of the interface regulating artificial antiferromagnetic coupling field comprises the following steps: 1) Fix the cleaned and dried substrate on the substrate table of the vacuum sputtering chamber to achieve the required vacuum degree; 2) sputtering a tantalum layer on the upper surface of the substrate to form a buffer layer; 3) Sputtering a platinum layer on the upper surface of the buffer layer to form a seed layer; 4) Sputtering the lower magnetic layer [Pt / CoFe]2 on the upper surface of the seed layer; 5) Prepare the lower interface magnetic layer [Pt / Co x Fe 1-x ], where 0≤x≤1; 6) Sputtering a non-magnetic layer Ir on the lower interface magnetic layer; 7) Sputtering the upper interface magnetic layer [Pt / Co x Fe 1-x ], where 0≤x≤1; 8) Sputtering an upper magnetic layer [CoFe / Pt]2 on the upper surface of the upper interface magnetic layer; 9) A tantalum layer is sputtered on the upper magnetic layer to form a protective layer to obtain a finished product.

[0008] Furthermore, in step 2), the thickness of the buffer layer is 5 nm, and in step 3), the thickness of the seed layer is 3 nm.

[0009] Furthermore, in the steps 4) and 8), the periods of the upper magnetic layer and the lower magnetic layer are both 2, the thickness of Pt is 2 nm, and the thickness of CoFe is 0.7 nm.

[0010] Furthermore, in the steps 5) and 7), the period of the lower interface magnetic layer and the upper interface magnetic layer is 1, the Pt thickness is 2nm, and the Co x Fe 1-x The thickness is 0.7nm.

[0011] Furthermore, in the step 6), the thickness of the non-magnetic layer Ir film is 0.7 nm, and the thickness of the protective layer tantalum layer in the step 9) is 5 nm.

[0012] Furthermore, the composition and preparation method of the lower interface magnetic layer and the upper interface magnetic layer are as follows: Type 1: The interface magnetic layer is [Pt / Fe]1, the period is 1, DC magnetron sputtering, the Pt thickness is 2nm, and the Fe thickness is 0.7nm; Or type 2, interface magnetic layer [Pt / Co 0.25 Fe 0.75 ]1, cycle 1, DC magnetron sputtering, Pt thickness 2nm, Co target and Fe target co-sputtering, thickness 0.7nm; Or type three, interface magnetic layer [Pt / Co 0.5 Fe 0.5 ]1, cycle 1, DC magnetron sputtering, Pt thickness 2nm, Co target and Fe target co-sputtering, thickness 0.7nm; Or type 4, interface magnetic layer [Pt / Co 0.75 Fe 0.25 ]1, cycle 1, DC magnetron sputtering, Pt thickness 2nm, Co target and Fe target co-sputtering, thickness 0.7nm; Or type five, interface magnetic layer [Pt / Co] 1, period 1, DC magnetron sputtering, Pt sputtering thickness is 2nm, Co thickness is 0.7nm.

[0013] The beneficial effects of the present invention are: 1. In an artificial antiferromagnetic structure, the composition ratio of the magnetic layer at the interface of the magnetic layer / non-magnetic layer / magnetic layer is changed, and the lattice matching ratio is adjusted by changing the composition ratio of the interface, resulting in a change in the interlayer exchange coupling strength. The present invention provides a new method for adjusting the coupling strength of artificial antiferromagnetic films.

[0014] 2. In the artificial antiferromagnetic structure, the antiferromagnetic coupling strength of the film is adjusted by changing the thickness of the non-magnetic layer. The increase in the thickness of the non-magnetic layer will reduce spin-related scattering, resulting in a decrease in the rate of change of the film resistance. The present invention increases the rate of change of the film magnetoresistance by adjusting the composition ratio of the interface magnetic layer and the lattice matching ratio. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 This is the hysteresis loop of the artificial antiferromagnetic structure with Fe as the interface magnetic layer; Figure 2 The interface magnetic layer is Co 0.25 Fe 0.75 The hysteresis loop of the artificial antiferromagnetic structure; Figure 3 The interface magnetic layer is Co 0.5 Fe 0.5 The hysteresis loop of the artificial antiferromagnetic structure; Figure 4 The interface magnetic layer is Co 0.75 Fe 0.25The hysteresis loop of the artificial antiferromagnetic structure; Figure 5 The hysteresis loop of the artificial antiferromagnetic structure with Co as the interface magnetic layer; Figure 6 Artificial antiferromagnetic Co x Fe 1-x , where 0≤x≤1, the curve of the antiferromagnetic coupling field varying with Co content. DETAILED DESCRIPTION

[0016] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments: A structure for artificial antiferromagnetic coupling field controlled by interface, wherein the structure of artificial antiferromagnetic is as follows from bottom to top: substrate, buffer layer, seed layer, lower magnetic layer, lower interface magnetic layer, non-magnetic layer, upper interface magnetic layer, upper magnetic layer and protective layer. The lower interface magnetic layer and the upper interface magnetic layer are prepared by co-sputtering of two targets and using the same preparation process, Co x Fe 1-x The thickness is equal to 0.7nm.

[0017] Example 1 A method for preparing an interface-regulated artificial antiferromagnetic coupling field, the specific steps are as follows: 1) Fix the cleaned and dried substrate on the substrate stage of the vacuum sputtering chamber to a thickness of 8.0×10 -6 Vacuum degree of Pa.

[0018] 2) DC magnetron sputtering, sputtering gas pressure 0.2Pa, sputtering power 10W, controlling the time, sputtering a tantalum buffer layer with a thickness of 5nm on the substrate.

[0019] 3) DC magnetron sputtering, sputtering gas pressure 0.3Pa, sputtering power 20W, controlling the time, sputtering growth seed layer of platinum layer with a thickness of 3nm on the tantalum layer.

[0020] 4) DC magnetron sputtering, sputtering the lower magnetic layer [Pt / CoFe]2 on the platinum layer, with a period of 2, Pt sputtering gas pressure of 0.3Pa, sputtering power of 20W, and thickness of 2nm; CoFe sputtering gas pressure of 0.3Pa, sputtering power of 10W, and thickness of 0.7nm.

[0021] 5) DC magnetron sputtering, sputtering the lower interface magnetic layer [Pt / Fe]1 on the lower magnetic layer [Pt / CoFe]2, with a period of 1, a Pt sputtering pressure of 0.3Pa, a sputtering power of 20W, and a thickness of 2nm; a Fe sputtering pressure of 0.6Pa, a sputtering power of 55W, and a thickness of 0.7nm.

[0022] 6) DC magnetron sputtering, sputtering gas pressure 0.3Pa, sputtering power 10W, controlling time, sputtering Ir non-magnetic layer on the lower interface magnetic layer [Pt / Fe]1, the iridium layer thickness is 0.7nm.

[0023] 7) DC magnetron sputtering, sputtering the upper interface magnetic layer [Fe / Pt]1 on the Ir layer, with a period of 1, a Pt sputtering pressure of 0.3 Pa, a sputtering power of 20 W, and a thickness of 2 nm; the Fe sputtering pressure of 0.6 Pa, a sputtering power of 55 W, and a thickness of 0.7 nm.

[0024] 8) DC magnetron sputtering, sputtering the upper magnetic layer [CoFe / Pt]2 on the upper interface magnetic layer [Fe / Pt]1, with a period of 2, a Pt sputtering pressure of 0.3Pa, a sputtering power of 20W, and a thickness of 2nm; the CoFe sputtering pressure of 0.3Pa, a sputtering power of 10W, and a thickness of 0.7nm.

[0025] 9) DC magnetron sputtering, sputtering gas pressure 0.3Pa, sputtering power 20W, controlling time, sputtering Ta cover layer on the upper magnetic layer [CoFe / Pt]2, the platinum layer thickness is 5nm.

[0026] Example 2 A method for preparing an interface-regulated artificial antiferromagnetic coupling field, the specific steps are as follows: 1) Fix the cleaned and dried substrate on the substrate stage of the vacuum sputtering chamber to a thickness of 8.0×10 -6 Vacuum degree of Pa.

[0027] 2) DC magnetron sputtering, sputtering gas pressure 0.2Pa, sputtering power 10W, controlling the time, sputtering a tantalum buffer layer with a thickness of 5nm on the substrate.

[0028] 3) DC magnetron sputtering, sputtering gas pressure 0.3Pa, sputtering power 20W, controlling the time, sputtering growth seed layer of platinum layer with a thickness of 3nm on the tantalum layer.

[0029] 4) DC magnetron sputtering, sputtering the lower magnetic layer [Pt / CoFe]2 on the platinum layer, with a period of 2, Pt sputtering gas pressure of 0.3Pa, sputtering power of 20W, and thickness of 2nm; CoFe sputtering gas pressure of 0.3Pa, sputtering power of 10W, and thickness of 0.7nm.

[0030] 5) DC magnetron sputtering, sputtering the lower interface magnetic layer [Pt / Co 0.25 Fe 0.75 ]1, the period is 1, the Pt sputtering pressure is 0.3Pa, the sputtering power is 20W, and the thickness is 2nm; the Co target and Fe target are co-sputtered, the sputtering pressure is 0.6Pa, the thickness is 0.7nm, the Co target sputtering power is 25W, and the Fe target sputtering power is 45W.

[0031] 6) DC magnetron sputtering, sputtering pressure 0.3Pa, sputtering power 10W, control time, on the lower interface magnetic layer [Pt / Co 0.25 Fe 0.75 ]1 is sputtered with an Ir non-magnetic layer, and the thickness of the iridium layer is 0.7nm.

[0032] 7) DC magnetron sputtering, sputtering the upper interface magnetic layer [Co 0.25 Fe 0.75 / Pt]1, the period is 1, the Pt sputtering pressure is 0.3Pa, the sputtering power is 20W, and the thickness is 2nm; the Co target and Fe target are co-sputtered, the sputtering pressure is 0.6Pa, the thickness is 0.7nm, the Co target sputtering power is 25W, and the Fe target sputtering power is 45W.

[0033] 8) DC magnetron sputtering, on the upper interface magnetic layer [Co 0.25 Fe 0.75 An upper magnetic layer [CoFe / Pt]2 is sputtered on [Si / Pt]1 with a period of 2, a Pt sputtering pressure of 0.3 Pa, a sputtering power of 20 W, and a thickness of 2 nm; a CoFe sputtering pressure of 0.3 Pa, a sputtering power of 10 W, and a thickness of 0.7 nm.

[0034] 9) DC magnetron sputtering, sputtering gas pressure 0.3Pa, sputtering power 20W, controlling time, sputtering Ta capping layer on the upper magnetic layer [CoFe / Pt]2, the thickness of the tantalum layer is 5nm.

[0035] Example 3 A method for preparing an interface-regulated artificial antiferromagnetic coupling field, the specific steps are as follows: 1) Fix the cleaned and dried substrate on the substrate stage of the vacuum sputtering chamber to a thickness of 8.0×10 -6 Vacuum degree of Pa.

[0036] 2) DC magnetron sputtering, sputtering gas pressure 0.2Pa, sputtering power 10W, controlling the time, sputtering a tantalum buffer layer with a thickness of 5nm on the substrate.

[0037] 3) DC magnetron sputtering, sputtering gas pressure 0.3Pa, sputtering power 20W, controlling the time, sputtering growth seed layer of platinum layer with a thickness of 3nm on the tantalum layer.

[0038] 4) DC magnetron sputtering, sputtering the lower magnetic layer [Pt / CoFe]2 on the platinum layer, with a period of 2, Pt sputtering gas pressure of 0.3Pa, sputtering power of 20W, and thickness of 2nm; CoFe sputtering gas pressure of 0.3Pa, sputtering power of 10W, and thickness of 0.7nm.

[0039] 5) DC magnetron sputtering, sputtering the lower interface magnetic layer [Pt / Co 0.5 Fe 0.5 ]1, the period is 1, the Pt sputtering pressure is 0.3Pa, the sputtering power is 20W, and the thickness is 2nm; the Co target and Fe target are co-sputtered, the sputtering pressure is 0.6Pa, the thickness is 0.7nm, the Co target sputtering power is 35W, and the Fe target sputtering power is 35W.

[0040] 6) DC magnetron sputtering, sputtering pressure 0.3Pa, sputtering power 10W, control time, on the lower interface magnetic layer [Pt / Co 0.5 Fe 0.5 ]1 is sputtered with an Ir non-magnetic layer, and the thickness of the iridium layer is 0.7nm.

[0041] 7) DC magnetron sputtering, sputtering the upper interface magnetic layer [Co 0.5 Fe 0.5 / Pt]1, the period is 1, the Pt sputtering pressure is 0.3Pa, the sputtering power is 20W, and the thickness is 2nm; the Co target and Fe target are co-sputtered, the sputtering pressure is 0.6Pa, the thickness is 0.7nm, the Co target sputtering power is 35W, and the Fe target sputtering power is 35W.

[0042] 8) DC magnetron sputtering, on the upper interface magnetic layer [Co 0.5 Fe 0.5 An upper magnetic layer [CoFe / Pt]2 is sputtered on [Si / Pt]1 with a period of 2, a Pt sputtering pressure of 0.3 Pa, a sputtering power of 20 W, and a thickness of 2 nm; a CoFe sputtering pressure of 0.3 Pa, a sputtering power of 10 W, and a thickness of 0.7 nm.

[0043] 9) DC magnetron sputtering, sputtering gas pressure 0.3Pa, sputtering power 20W, controlling time, sputtering Ta capping layer on the upper magnetic layer [CoFe / Pt]2, the thickness of the tantalum layer is 5nm.

[0044] Example 4 A method for preparing an interface-regulated artificial antiferromagnetic coupling field, the specific steps are as follows: 1) Fix the cleaned and dried substrate on the substrate stage of the vacuum sputtering chamber to a thickness of 8.0×10 -6 Vacuum degree of Pa.

[0045] 2) DC magnetron sputtering, sputtering gas pressure 0.2Pa, sputtering power 10W, controlling the time, sputtering a tantalum buffer layer with a thickness of 5nm on the substrate.

[0046] 3) DC magnetron sputtering, sputtering gas pressure 0.3Pa, sputtering power 20W, controlling the time, sputtering growth seed layer of platinum layer with a thickness of 3nm on the tantalum layer.

[0047] 4) DC magnetron sputtering, sputtering the lower magnetic layer [Pt / CoFe]2 on the platinum layer, with a period of 2, Pt sputtering gas pressure of 0.3Pa, sputtering power of 20W, and thickness of 2nm; CoFe sputtering gas pressure of 0.3Pa, sputtering power of 10W, and thickness of 0.7nm.

[0048] 5) DC magnetron sputtering, sputtering different composition lower interface magnetic layer [Pt / Co 0.75 Fe 0.25 ]1, the period is 1, the Pt sputtering pressure is 0.3Pa, the sputtering power is 20W, and the thickness is 2nm; the Co target and Fe target are co-sputtered, the sputtering pressure is 0.6Pa, the thickness is 0.7nm, the Co target sputtering power is 45W, and the Fe target sputtering power is 25W.

[0049] 6) DC magnetron sputtering, sputtering pressure 0.3Pa, sputtering power 10W, control time, on the lower interface magnetic layer [Pt / Co 0.75 Fe 0.25 ]1 is sputtered with an Ir non-magnetic layer, and the thickness of the iridium layer is 0.7nm.

[0050] 7) DC magnetron sputtering, sputtering the upper interface magnetic layer [Co 0.75 Fe 0.25 / Pt]1, the period is 1, the Pt sputtering pressure is 0.3Pa, the sputtering power is 20W, and the thickness is 2nm; the Co target and Fe target are co-sputtered, the sputtering pressure is 0.6Pa, the thickness is 0.7nm, the Co target sputtering power is 45W, and the Fe target sputtering power is 25W.

[0051] 8) DC magnetron sputtering, on the upper interface magnetic layer [Co 0.75 Fe 0.25 An upper magnetic layer [CoFe / Pt]2 is sputtered on [Si / Pt]1 with a period of 2, a Pt sputtering pressure of 0.3 Pa, a sputtering power of 20 W, and a thickness of 2 nm; a CoFe sputtering pressure of 0.3 Pa, a sputtering power of 10 W, and a thickness of 0.7 nm.

[0052] 9) DC magnetron sputtering, sputtering gas pressure 0.3Pa, sputtering power 20W, controlling time, sputtering Ta capping layer on the upper magnetic layer [CoFe / Pt]2, the thickness of the tantalum layer is 5nm.

[0053] Example 5 A method for preparing an interface-regulated artificial antiferromagnetic coupling field, the specific steps are as follows: 1) Fix the cleaned and dried substrate on the substrate stage of the vacuum sputtering chamber to a thickness of 8.0×10 -6 Vacuum degree of Pa.

[0054] 2) DC magnetron sputtering, sputtering gas pressure 0.2Pa, sputtering power 10W, controlling the time, sputtering a tantalum buffer layer with a thickness of 5nm on the substrate.

[0055] 3) DC magnetron sputtering, sputtering gas pressure 0.3Pa, sputtering power 20W, controlling the time, sputtering growth seed layer of platinum layer with a thickness of 3nm on the tantalum layer.

[0056] 4) DC magnetron sputtering, sputtering the lower magnetic layer [Pt / CoFe]2 on the platinum layer, with a period of 2, Pt sputtering gas pressure of 0.3Pa, sputtering power of 20W, and thickness of 2nm; CoFe sputtering gas pressure of 0.3Pa, sputtering power of 10W, and thickness of 0.7nm.

[0057] 5) DC magnetron sputtering, sputtering a lower interface magnetic layer [Pt / Co]1 of different composition on the lower magnetic layer [Pt / CoFe]2, with a period of 1, Pt sputtering gas pressure of 0.3Pa, sputtering power of 20W, and thickness of 2nm; Co sputtering gas pressure of 0.6Pa, sputtering power of 55W, and thickness of 0.7nm.

[0058] 6) DC magnetron sputtering, sputtering gas pressure 0.3Pa, sputtering power 10W, controlling time, sputtering Ir non-magnetic layer on the lower interface magnetic layer [Pt / Co]1, the iridium layer thickness is 0.7nm.

[0059] 7) DC magnetron sputtering, sputtering the upper interface magnetic layer [Co / Pt]1 on the Ir layer, with a period of 1, a Pt sputtering pressure of 0.3 Pa, a sputtering power of 20 W, and a thickness of 2 nm; a Co sputtering pressure of 0.6 Pa, a sputtering power of 55 W, and a thickness of 0.7 nm.

[0060] 8) DC magnetron sputtering, sputtering the upper magnetic layer [CoFe / Pt]2 on the upper interface magnetic layer [Co / Pt]1, with a period of 2, a Pt sputtering pressure of 0.3Pa, a sputtering power of 20W, and a thickness of 2nm; a CoFe sputtering pressure of 0.3Pa, a sputtering power of 10W, and a thickness of 0.7nm.

[0061] 9) DC magnetron sputtering, sputtering gas pressure 0.3Pa, sputtering power 20W, controlling time, sputtering Ta capping layer on the upper magnetic layer [CoFe / Pt]2, the thickness of the tantalum layer is 5nm.

[0062] The artificial antiferromagnetic sample 1 prepared by Example 1 is: Ta(5nm) / Pt(3nm) / [Pt(2nm) / CoFe(0.7nm)]2 / [Pt(2nm) / Fe(0.7nm)] / Ir(0.7nm) / [Fe(0.7nm) / Pt(2nm)] / [CoFe(0.7nm) / Pt(2nm)]2 / Ta(5nm); The artificial antiferromagnetic sample 2 prepared by Example 2 is: Ta(5nm) / Pt(3nm) / [Pt(2nm) / CoFe(0.7nm)]2 / [Pt(2nm) / Co 0.25 Fe 0.75 (0.7nm)] / Ir(0.7nm) / [(Co 0.25 Fe 0.75 (0.7nm) / Pt(2nm)] / [CoFe(0.7nm) / Pt(2nm)]2 / Ta(5nm); The artificial antiferromagnetic sample 3 prepared by Example 3 is: Ta(5nm) / Pt(3nm) / [Pt(2nm) / CoFe(0.7nm)]2 / [Pt(2nm) / Co 0.5 Fe 0.5 (0.7nm)] / Ir(0.7nm) / [Co 0.5 Fe 0.5 (0.7nm) / Pt(2nm)] / [CoFe(0.7nm) / Pt(2nm)]2 / Ta(5nm); The artificial antiferromagnetic sample 4 prepared by Example 4 is: Ta(5nm) / Pt(3nm) / [Pt(2nm) / CoFe(0.7nm)]2 / [Pt(2nm) / Co 0.75 Fe 0.25 (0.7nm)] / Ir(0.7nm) / [Co 0.75 Fe 0.25 (0.7nm) / Pt(2nm)] / [CoFe(0.7nm) / Pt(2nm)]2 / Ta(5nm); The artificial antiferromagnetic sample 5 prepared by Example 5 is: Ta(5nm) / Pt(3nm) / [Pt(2nm) / CoFe(0.7nm)]2 / [Pt(2nm) / Co(0.7nm)] / Ir(0.7nm) / [(Co(0.7nm) / Pt(2nm)] / [CoFe(0.7nm) / Pt(2nm)]2 / Ta(5nm); Samples 1 to 5 were magnetized and the hysteresis loops are shown in Figure 1-Figure 5 .

[0063] Artificial antiferromagnetic CoxFe1-x, where 0≤x≤1, the curve of antiferromagnetic coupling field changing with Co content is shown in Figure 6 .

[0064] All samples are characterized by artificial antiferromagnetic structures, with an antiferromagnetic coupling platform existing at low fields.

[0065] The Co content is around 0.75, which has the strongest antiferromagnetic coupling field.

[0066] In the artificial antiferromagnetic structure, the composition of the magnetic layer at the interface of the non-magnetic layer / magnetic layer is changed, and the position of the Fermi level is adjusted by the ratio of the composition, so that the band gap between the conduction band and the valence band is minimized, electrons are easy to transition, the number of spin-polarized conductive electrons in the ferromagnetic film is increased, and the interlayer exchange coupling strength is enhanced, resulting in an enhancement of the antiferromagnetic coupling field.

[0067] Therefore, the artificial antiferromagnetic film structure: substrate / buffer layer / seed layer / lower magnetic layer / lower interface magnetic layer / isolation layer / upper interface magnetic layer / upper magnetic layer / covering layer, by changing the atomic composition at the interface of the magnetic layer / isolation layer, can regulate the antiferromagnetic coupling field. This method provides a new solution for regulating the size of the antiferromagnetic coupling field.

Claims

1. A process for preparing an interface-regulated artificial antiferromagnetic coupling field structure, characterized in that: The structure is as follows from bottom to top: substrate, buffer layer, seed layer, lower magnetic layer, lower interface magnetic layer, non-magnetic layer, upper interface magnetic layer, upper magnetic layer and protective layer; the upper and lower interface magnetic layers are made of [Pt / Co] with different atomic ratios. x Fe 1-x ] structure, and the antiferromagnetic coupling enhancement is achieved by regulating the interface structure between the interface magnetic layer and the non-magnetic layer; The preparation method comprises the following steps: 1) Fix the cleaned and dried substrate on the substrate table of the vacuum sputtering chamber to achieve the required vacuum degree; 2) sputtering a buffer layer on the upper surface of the substrate; 3) Sputtering a seed layer on the upper surface of the buffer layer; 4) sputtering the lower magnetic layer on the upper surface of the seed layer; 5) Prepare the lower interface magnetic layer [Pt / Co x Fe 1-x ], where 0≤x≤1; 6) sputtering a non-magnetic layer on the lower interface magnetic layer; 7) Sputtering the upper interface magnetic layer [Pt / Co x Fe 1-x ], where 0≤x≤1; 8) sputtering an upper magnetic layer on the upper surface of the upper interface magnetic layer; 9) Sputter a protective layer on the upper magnetic layer to obtain a finished product.

2. The preparation process of the interface-regulated artificial antiferromagnetic coupling field structure according to claim 1, characterized in that: The lower interface magnetic layer and the upper interface magnetic layer are prepared by co-sputtering of two targets.

3. The preparation process of the interface-regulated artificial antiferromagnetic coupling field structure according to claim 1, characterized in that: The lower interface magnetic layer and the upper interface magnetic layer are prepared using the same process.

4. The preparation process of the interface-regulated artificial antiferromagnetic coupling field structure according to claim 1, characterized in that: The components and preparation methods of the lower interface magnetic layer and the upper interface magnetic layer are as follows: Type 1: The interface magnetic layer is [Pt / Fe]1, the period is 1, DC magnetron sputtering, the Pt thickness is 2nm, and the Fe thickness is 0.7nm; Or type 2, interface magnetic layer [Pt / Co 0.25 Fe 0.75 ]1, cycle 1, DC magnetron sputtering, Pt thickness 2nm, Co target and Fe target co-sputtering, thickness 0.7nm; Or type three, interface magnetic layer [Pt / Co 0.5 Fe 0.5 ]1, cycle 1, DC magnetron sputtering, Pt thickness 2nm, Co target and Fe target co-sputtering, thickness 0.7nm; Or type 4, interface magnetic layer [Pt / Co 0.75 Fe 0.25 ]1, cycle 1, DC magnetron sputtering, Pt thickness 2nm, Co target and Fe target co-sputtering, thickness 0.7nm; Or type five, interface magnetic layer [Pt / Co] 1, period 1, DC magnetron sputtering, Pt sputtering thickness is 2nm, Co thickness is 0.7nm.

5. The preparation process of the interface-regulated artificial antiferromagnetic coupling field structure according to claim 1, characterized in that: The thickness of the buffer layer Ta in step 2) is 5 nm, and the thickness of the seed layer Pt in step 3) is 3 nm.

6. The process for preparing the structure of interface-controlled artificial antiferromagnetic coupling field according to claim 1, characterized in that: In the steps 4) and 8), the periods of the upper magnetic layer and the lower magnetic layer [Pt / CoFe]2 are both 2, the thickness of Pt is 2nm, and the thickness of CoFe is 0.7nm.

7. The process for preparing the interface-regulated artificial antiferromagnetic coupling field structure according to claim 1, characterized in that: The thickness of the non-magnetic layer Ir film in step 6) is 0.7 nm, and the thickness of the protective layer Ta in step 9) is 5 nm.