A high wear-resistant and anti-fingerprint stainless steel belt and its preparation process

By synthesizing silica and titanium dioxide-graphene sol and combining anodizing technology, the problems of scratches, fingerprints and stains in use of stainless steel strips are solved, and high wear resistance and fingerprint resistance are improved, and the use is extended. life.

CN118835298BActive Publication Date: 2024-12-03JIANGSU YONGJIN METAL TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411311654.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-20
Publication Date
2024-12-03
Estimated Expiration
2044-09-20

AI Technical Summary

Technical Problem

Traditional stainless steel belts are prone to scratches, fingerprints and stains during use, reducing their aesthetics and service life. The existing treatment methods are difficult to effectively improve their wear resistance and fingerprint resistance.

Method used

A high wear-resistant and fingerprint-resistant stainless steel strip is prepared by synthesizing silica and titanium dioxide-graphene sol, combined with anodizing technology, a composite electroplating layer is formed to improve the hydrophobicity and wear resistance of the stainless steel strip.

Benefits of technology

It significantly improves the fingerprint resistance and wear resistance of the stainless steel belt, enhances the hydrophobicity and stain resistance of its surface, and extends the service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention relates to the technical field of stainless steel strips, and specifically to a highly wear-resistant and anti-fingerprint stainless steel strip and a preparation process thereof. The present invention performs electroplating treatment on the surface of the stainless steel strip, and adds a composite sol to the electroplating solution. The present invention prepares a composite sol by compounding the graphene loaded with microspheres with silicon dioxide and titanium dioxide sols, and the addition of the sol can improve the hydrophobicity of the surface of the stainless steel strip. Graphene is modified using maleic anhydride so that the modified graphene oxide has better dispersibility and surface activity, and then styrene microspheres are loaded on the modified graphene. At this time, the anhydride groups on the styrene microspheres can react with the anhydride groups on the modified graphene, and the two have good compatibility, thereby increasing the loading amount of styrene microspheres on the modified graphene and improving the anti-fingerprint and wear resistance of the stainless steel strip.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of stainless steel strips, in particular to a highly wear-resistant and anti-fingerprint stainless steel strip and a preparation process thereof. Background Art

[0002] With the widespread application of stainless steel products in modern industry and daily life, people have put forward higher requirements for the appearance, wear resistance and anti-fingerprint performance of stainless steel products. However, traditional stainless steel products are prone to scratches, fingerprints and stains during use, which reduces their overall appearance and service life. The existing technology usually changes the structure and morphology of the stainless steel surface by chemical treatment, mechanical grinding or sandblasting to increase its surface hardness and wear resistance. However, when these methods are used to treat stainless steel belts, fingerprints and stains are still prone to appear on the surface of the stainless steel belts during use.

[0003] In order to solve the above problems and improve the wear resistance and anti-fingerprint properties of the stainless steel belt, the present invention provides a highly wear-resistant and anti-fingerprint stainless steel belt and a preparation process thereof. Summary of the invention

[0004] The object of the present invention is to provide a highly wear-resistant and anti-fingerprint stainless steel belt and a preparation process thereof, so as to solve the problems raised in the above background technology.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0006] A preparation process of a highly wear-resistant and anti-fingerprint stainless steel belt comprises the following steps:

[0007] Step 1: Take ethyl orthosilicate, methanol, deionized water, and hydrochloric acid, stir evenly to obtain a silica sol; take benzoyl acetone and methanol, stir evenly, add acrylic acid and tetrabutyl titanate, stir evenly, add graphene loaded with microspheres, stir for 2-3 hours, and obtain a titanium dioxide-graphene sol;

[0008] Step 2: Take silica sol and titanium dioxide-graphene sol, stir them evenly to obtain a composite sol;

[0009] Step 3: Take the steel strip, alkali wash and pickle wash to obtain the pre-treated steel strip;

[0010] Step 4: Anodizing the pretreated steel strip to obtain a highly wear-resistant and anti-fingerprint stainless steel strip;

[0011] The electrolyte used for anodizing includes the following components: deionized water, sulfuric acid, phytic acid, disodium ethylenediaminetetraacetic acid, nano-aluminum oxide, and composite sol.

[0012] More optimally, the mass ratio of the silica sol to the titanium dioxide-graphene sol is 1:(1-1.2).

[0013] More optimally, the preparation method of the microsphere-loaded graphene is: take styrene microspheres and deionized water, stir evenly, add modified graphene, heat to 70-75° C., stir for 7-8 hours, cool, centrifuge, wash, and dry to obtain microsphere-loaded graphene.

[0014] Preferably, the method for preparing the styrene microspheres comprises the following steps:

[0015] S1: Take isoamyl acetate and maleic anhydride, stir evenly, add styrene and azobisisobutyronitrile, purge with nitrogen for 30-40 minutes, heat in a water bath at 80-85°C for 2-3 hours, centrifuge, wash and dry to obtain compound A;

[0016] S2: Take ethylamine and ammonia water, stir evenly to obtain reagent A; take compound A, deionized water, and reagent A, stir at 70-75°C for 40-50 minutes, introduce nitrogen, heat to 160-162°C, stir for 5-5.5 days, dialyze, and freeze-dry to obtain styrene microspheres.

[0017] More optimally, the preparation method of modified graphene is: take graphene oxide and maleic anhydride, mix them evenly, react at 120-122°C for 4-5h, wash with deionized water, dropwise add sodium hydroxide aqueous solution, centrifuge, wash, filter, add ethanol, ultrasonically disperse, add perfluorodecyltrichlorosilane, stir and react for 6-8h, centrifuge, wash, and dry to obtain modified graphene.

[0018] More optimally, the steel strip comprises the following components, in mass percentage: 0.30wt%-0.7wt% Mn, 0.25wt%-0.30wt% Si, 0.15wt%-0.20wt% C, 0.02wt%-0.045wt% P, 0.01wt%-0.045wt% S, 0.1wt%-0.25wt% Cr, 0.1wt%-0.25wt% Ni, and the balance is Fe.

[0019] More optimally, the mass ratio of the styrene microspheres, deionized water, and modified graphene is (7-8):200:0.2.

[0020] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0021] (1) The present invention uses maleic anhydride and styrene copolymerization to prepare a styrene microsphere, and then uses ethylamine and ammonia water to aminize it to enhance its hydrophobicity;

[0022] The present invention first uses maleic anhydride to modify graphene, so that the modified graphene oxide has better dispersibility and surface activity, and then loads styrene microspheres on the modified graphene. At this time, the anhydride groups on the styrene microspheres can react with the anhydride groups on the modified graphene, and the two have good compatibility, thereby increasing the loading amount of the styrene microspheres on the modified graphene and improving the anti-fingerprint property of the stainless steel strip. At the same time, perfluorodecyltrichlorosilane is added to the graphene oxide of the present invention during modification, thereby improving the hydrophobic and oleophobic properties of the stainless steel strip, i.e., the anti-fingerprint property.

[0023] (2) The present invention prepares a silicon dioxide and titanium dioxide sol, the addition of which can improve the hydrophobicity of the surface of the stainless steel strip. Then, the present invention composites the graphene loaded with microspheres with the sol and adds them together to the electroplating solution. The sol-gel process can provide a uniform and stable carrier, so that the graphene loaded with microspheres is more evenly distributed in the electroplating layer, thereby enhancing the wear resistance and anti-fingerprint properties of the stainless steel strip. DETAILED DESCRIPTION

[0024] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] There is no special restriction on the purchase manufacturers of all raw materials involved in the present invention, and exemplary include: nano-alumina: can be purchased from Sumitomo Chemical of Japan, α-Al2O3 particles, particle size less than 500 nm; graphene oxide: can be purchased from Merck, model: 796034;

[0026] Embodiment 1: A preparation process of a highly wear-resistant and anti-fingerprint stainless steel belt, comprising the following steps:

[0027] Step 1: Preparation of styrene microspheres:

[0028] Take 300 mL of isoamyl acetate and 15 g of maleic anhydride, stir evenly, add 16 g of styrene and 0.2 g of azobisisobutyronitrile, purge with nitrogen for 35 min, heat in a water bath at 83 °C for 2.5 h, centrifuge, wash and dry to obtain compound A;

[0029] Take 2.4 g of ethylamine and 1 g of ammonia water, stir evenly to obtain reagent A; take 10 g of compound A, 90 mL of deionized water, and reagent A, stir at 73°C for 45 min, introduce nitrogen gas to pressurize to 0.6 mPa, heat to 161°C, stir for 5 days, dialyze, and freeze-dry to obtain styrene microspheres;

[0030] Step 2: Preparation of modified graphene:

[0031] Take 0.1 g of graphene oxide and 3 g of maleic anhydride, mix them evenly, react at 121 ° C for 4.5 h, wash with deionized water until the pH value reaches 7, add 1 mol / L sodium hydroxide aqueous solution until the pH value reaches 11, centrifuge, wash, filter, add 100 mL of ethanol, ultrasonically disperse, add 2 g of perfluorodecyltrichlorosilane, stir and react for 7 h, centrifuge, wash, and dry to obtain modified graphene;

[0032] Step 3: Preparation of graphene loaded microspheres:

[0033] Take 8 g of styrene microspheres and 200 mL of deionized water, stir evenly, add 0.2 g of modified graphene, heat to 73 ° C, stir for 7.5 h, cool, centrifuge, wash, and dry to obtain graphene loaded with microspheres;

[0034] Step 4: Preparation of composite sol:

[0035] Take 20 g of ethyl orthosilicate, 110 g of methanol, 5 mL of deionized water, and 3.5 g of hydrochloric acid, stir evenly to obtain a silica sol;

[0036] Take 16.2g of benzoyl acetone and 110g of methanol, stir evenly, add 15g of acrylic acid and 43g of tetrabutyl titanate, stir evenly, add 0.5g of microsphere-loaded graphene, stir for 2.5h, and obtain titanium dioxide-graphene sol;

[0037] Take 10 g of silica sol and 10 g of titanium dioxide-graphene sol, stir evenly to obtain a composite sol;

[0038] Step 5:

[0039] The steel strip is placed in an alkaline washing solution at 57° C. for 8 minutes, taken out, washed, and dried to obtain an alkaline washed steel strip; the alkaline washing solution comprises the following components: 10 g / L sodium hydroxide, 20 g / L sodium carbonate, and 1 g / L sodium dodecyl sulfate;

[0040] The steel strip comprises the following components, in percentage by mass: 0.6wt% of Mn, 0.27wt% of Si, 0.17wt% of C, 0.03wt% of S, 0.03wt% of P, 0.2wt% of Cr, 0.2wt% of Ni, and the balance is Fe;

[0041] The alkali-washed steel strip is placed in a pickling solution at a temperature of 43°C for 23 minutes, taken out, washed, and dried to obtain a pickled steel strip. After pickling, the steel strip is annealed at 740°C for 42 seconds to obtain a pretreated steel strip. The pickling solution includes the following components: 0.08 g / L sodium dodecyl sulfonate, 2 g / L benzotriazole, and 32% hydrochloric acid. The concentration of the pickling solution is 80 g / L.

[0042] Anodizing the pretreated steel strip to obtain a highly wear-resistant and anti-fingerprint stainless steel strip;

[0043] The working conditions of anodization are: 1 kW AC power supply, 0.3 A constant current, 100 Hz frequency, and 12 min time; the electrolyte used for anodization is: 100 mL deionized water as solvent, including 0.5 g sulfuric acid, 0.8 g phytic acid, 5 g disodium ethylenediaminetetraacetic acid, 0.1 g nano-aluminum oxide, and 1 g composite sol.

[0044] Embodiment 2: A preparation process of a highly wear-resistant and anti-fingerprint stainless steel belt, comprising the following steps:

[0045] Step 1: Preparation of styrene microspheres:

[0046] Take 300 mL of isoamyl acetate and 15 g of maleic anhydride, stir evenly, add 16 g of styrene and 0.2 g of azobisisobutyronitrile, purge with nitrogen for 35 min, heat in a water bath at 82 °C for 2.5 h, centrifuge, wash and dry to obtain compound A;

[0047] Take 2.4 g of ethylamine and 1 g of ammonia water, stir evenly to obtain reagent A; take 10 g of compound A, 90 mL of deionized water, and reagent A, stir at 72°C for 45 min, introduce nitrogen gas to pressurize to 0.6 mPa, heat to 161°C, stir for 5 days, dialyze, and freeze-dry to obtain styrene microspheres;

[0048] Step 2: Preparation of modified graphene:

[0049] Take 0.1g of graphene oxide and 3g of maleic anhydride, mix them evenly, react at 120°C for 4h, wash with deionized water until the pH value reaches 7, add 1mol / L sodium hydroxide aqueous solution until the pH value reaches 11, centrifuge, wash, filter, add 100mL of ethanol, ultrasonically disperse, add 2g of perfluorodecyltrichlorosilane, stir and react for 6h, centrifuge, wash, and dry to obtain modified graphene;

[0050] Step 3: Preparation of graphene loaded microspheres:

[0051] Take 7 g of styrene microspheres and 200 mL of deionized water, stir evenly, add 0.2 g of modified graphene, heat to 70 ° C, stir for 7 h, cool, centrifuge, wash, and dry to obtain graphene loaded with microspheres;

[0052] Step 4: Preparation of composite sol:

[0053] Take 20 g of ethyl orthosilicate, 110 g of methanol, 5 mL of deionized water, and 3.5 g of hydrochloric acid, stir evenly to obtain a silica sol;

[0054] Take 16.2g of benzoyl acetone and 110g of methanol, stir evenly, add 15g of acrylic acid and 43g of tetrabutyl titanate, stir evenly, add 0.5g of microsphere-loaded graphene, stir for 2h, and obtain titanium dioxide-graphene sol;

[0055] Take 10 g of silica sol and 11 g of titanium dioxide-graphene sol, stir evenly to obtain a composite sol;

[0056] Step 5:

[0057] The steel strip is placed in an alkaline washing solution at 55° C. for 5 minutes, taken out, washed, and dried to obtain an alkaline washed steel strip; the alkaline washing solution comprises the following components: 10 g / L sodium hydroxide, 20 g / L sodium carbonate, and 1 g / L sodium dodecyl sulfate;

[0058] The steel strip comprises the following components, in percentage by mass: 0.30wt% Mn, 0.25wt% Si, 0.15wt% C, 0.01wt% S, 0.02wt% P, 0.1wt% Cr, 0.25wt% Ni, and the balance is Fe;

[0059] The alkali-washed steel strip is placed in a pickling solution at a temperature of 45°C for immersion for 20 minutes, taken out, washed, and dried to obtain a pickled steel strip. After pickling, the steel strip is annealed at 750°C for 40 seconds to obtain a pretreated steel strip. The pickling solution includes the following components: 0.08 g / L sodium dodecyl sulfonate, 2 g / L benzotriazole, and 32% hydrochloric acid. The concentration of the pickling solution is 80 g / L.

[0060] Anodizing the pretreated steel strip to obtain a highly wear-resistant and anti-fingerprint stainless steel strip;

[0061] The working conditions of anodization are: 1 kW AC power supply, 0.3 A constant current, 100 Hz frequency, and 10 min time; the electrolyte used for anodization is: 100 mL deionized water as solvent, including 0.5 g sulfuric acid, 0.8 g phytic acid, 5 g disodium ethylenediaminetetraacetic acid, 0.1 g nano-aluminum oxide, and 1 g composite sol.

[0062] Embodiment 3: A process for preparing a highly wear-resistant and anti-fingerprint stainless steel belt, comprising the following steps:

[0063] Step 1: Preparation of styrene microspheres:

[0064] Take 300 mL of isoamyl acetate and 15 g of maleic anhydride, stir evenly, add 16 g of styrene and 0.2 g of azobisisobutyronitrile, purge with nitrogen for 40 min, heat in a water bath at 85 ° C for 3 h, centrifuge, wash and dry to obtain compound A;

[0065] Take 2.4 g of ethylamine and 1 g of ammonia water, stir evenly to obtain reagent A; take 10 g of compound A, 90 mL of deionized water, and reagent A, stir at 75°C for 50 min, introduce nitrogen gas to pressurize to 0.6 mPa, heat to 162°C, stir for 5.5 days, dialyze, and freeze-dry to obtain styrene microspheres;

[0066] Step 2: Preparation of modified graphene:

[0067] Take 0.1g of graphene oxide and 3g of maleic anhydride, mix them evenly, react at 122°C for 5h, wash with deionized water until the pH value reaches 7, add 1mol / L sodium hydroxide aqueous solution until the pH value reaches 11, centrifuge, wash, filter, add 100mL of ethanol, ultrasonically disperse, add 2g of perfluorodecyltrichlorosilane, stir and react for 8h, centrifuge, wash, and dry to obtain modified graphene;

[0068] Step 3: Preparation of graphene loaded microspheres:

[0069] Take 7.5 g of styrene microspheres and 200 mL of deionized water, stir evenly, add 0.2 g of modified graphene, heat to 75 ° C, stir for 8 h, cool, centrifuge, wash, and dry to obtain graphene loaded with microspheres;

[0070] Step 4: Preparation of composite sol:

[0071] Take 20 g of ethyl orthosilicate, 110 g of methanol, 5 mL of deionized water, and 3.5 g of hydrochloric acid, stir evenly to obtain a silica sol;

[0072] Take 16.2g of benzoyl acetone and 110g of methanol, stir evenly, add 15g of acrylic acid and 43g of tetrabutyl titanate, stir evenly, add 0.5g of microsphere-loaded graphene, stir for 3h, and obtain titanium dioxide-graphene sol;

[0073] Take 10 g of silica sol and 12 g of titanium dioxide-graphene sol, stir evenly to obtain a composite sol;

[0074] Step 5:

[0075] The steel strip is placed in an alkaline washing solution at 60° C. for 10 minutes, taken out, washed, and dried to obtain an alkaline washed steel strip; the alkaline washing solution comprises the following components: 10 g / L sodium hydroxide, 20 g / L sodium carbonate, and 1 g / L sodium dodecyl sulfate;

[0076] The steel strip comprises the following components, in percentage by mass: 0.7wt% of Mn, 0.30wt% of Si, 0.20wt% of C, 0.045wt% of S, 0.045wt% of P, 0.25wt% of Cr, 0.25wt% of Ni, and the balance is Fe;

[0077] The alkali-washed steel strip is placed in a pickling solution at a temperature of 45°C, immersed for 25 minutes, taken out, washed, and dried to obtain a pickled steel strip. After pickling, the steel strip is annealed at 750°C for 45 seconds to obtain a pretreated steel strip. The pickling solution includes the following components: 0.08 g / L sodium dodecyl sulfonate, 2 g / L benzotriazole, and 32% hydrochloric acid. The concentration of the pickling solution is 80 g / L.

[0078] Anodizing the pretreated steel strip to obtain a highly wear-resistant and anti-fingerprint stainless steel strip;

[0079] The working conditions of anodization are: 1 kW AC power supply, 0.3 A constant current, 100 Hz frequency, and 15 min time; the electrolyte used for anodization is: 100 mL deionized water as solvent, including 0.5 g sulfuric acid, 0.8 g phytic acid, 5 g disodium ethylenediaminetetraacetic acid, 0.1 g nano-aluminum oxide, and 1 g composite sol.

[0080] Comparative Example 1: No styrene microspheres were added, and the rest was the same as Example 1:

[0081] Step 1: Preparation of modified graphene:

[0082] Take 0.1 g of graphene oxide and 3 g of maleic anhydride, mix them evenly, react at 121 ° C for 4.5 h, wash with deionized water until the pH value reaches 7, add 1 mol / L sodium hydroxide aqueous solution until the pH value reaches 11, centrifuge, wash, filter, add 100 mL of ethanol, ultrasonically disperse, add 2 g of perfluorodecyltrichlorosilane, stir and react for 7 h, centrifuge, wash, and dry to obtain modified graphene;

[0083] Step 2: Preparation of composite sol:

[0084] Take 20 g of ethyl orthosilicate, 110 g of methanol, 5 mL of deionized water, and 3.5 g of hydrochloric acid, stir evenly to obtain a silica sol;

[0085] Take 16.2g of benzoyl acetone and 110g of methanol, stir evenly, add 15g of acrylic acid and 43g of tetrabutyl titanate, stir evenly, add 0.5g of modified graphene, stir for 2.5h, and obtain titanium dioxide-graphene sol;

[0086] Take 10 g of silica sol and 10 g of titanium dioxide-graphene sol, stir evenly to obtain a composite sol;

[0087] Step 5:

[0088] The steel strip is placed in an alkaline washing solution at 57° C. for 8 minutes, taken out, washed, and dried to obtain an alkaline washed steel strip; the alkaline washing solution comprises the following components: 10 g / L sodium hydroxide, 20 g / L sodium carbonate, and 1 g / L sodium dodecyl sulfate;

[0089] The steel strip comprises the following components, in percentage by mass: 0.6wt% of Mn, 0.27wt% of Si, 0.17wt% of C, 0.03wt% of S, 0.03wt% of P, 0.2wt% of Cr, 0.2wt% of Ni, and the balance is Fe;

[0090] The alkali-washed steel strip is placed in a pickling solution at a temperature of 43°C for 23 minutes, taken out, washed, and dried to obtain a pickled steel strip. After pickling, the steel strip is annealed at 740°C for 42 seconds to obtain a pretreated steel strip. The pickling solution includes the following components: 0.08 g / L sodium dodecyl sulfonate, 2 g / L benzotriazole, and 32% hydrochloric acid. The concentration of the pickling solution is 80 g / L.

[0091] Anodizing the pretreated steel strip to obtain a highly wear-resistant and anti-fingerprint stainless steel strip;

[0092] The working conditions of anodization are: 1 kW AC power supply, 0.3 A constant current, 100 Hz frequency, and 12 min time; the electrolyte used for anodization is: 100 mL deionized water as solvent, including 0.5 g sulfuric acid, 0.8 g phytic acid, 5 g disodium ethylenediaminetetraacetic acid, 0.1 g nano-aluminum oxide, and 1 g composite sol.

[0093] Comparative Example 2: Graphene is not modified using maleic anhydride, and the rest is the same as Example 1:

[0094] Step 1: Preparation of styrene microspheres:

[0095] Take 300 mL of isoamyl acetate and 15 g of maleic anhydride, stir evenly, add 16 g of styrene and 0.2 g of azobisisobutyronitrile, purge with nitrogen for 35 min, heat in a water bath at 83 °C for 2.5 h, centrifuge, wash and dry to obtain compound A;

[0096] Take 2.4 g of ethylamine and 1 g of ammonia water, stir evenly to obtain reagent A; take 10 g of compound A, 90 mL of deionized water, and reagent A, stir at 73°C for 45 min, introduce nitrogen gas to pressurize to 0.6 mPa, heat to 161°C, stir for 5 days, dialyze, and freeze-dry to obtain styrene microspheres;

[0097] Step 2: Preparation of modified graphene:

[0098] Take 0.1 g of graphene oxide and 100 mL of ethanol, disperse by ultrasonication, add 2 g of perfluorodecyltrichlorosilane, stir and react for 7 h, centrifuge, wash and dry to obtain modified graphene;

[0099] Step 3: Preparation of graphene loaded microspheres:

[0100] Take 8 g of styrene microspheres and 200 mL of deionized water, stir evenly, add 0.2 g of modified graphene, heat to 73 ° C, stir for 7.5 h, cool, centrifuge, wash, and dry to obtain graphene loaded with microspheres;

[0101] Step 4: Preparation of composite sol:

[0102] Take 20g of ethyl orthosilicate, 110g of methanol, 5mL of deionized water, and 3.5g of hydrochloric acid, stir evenly to obtain silica sol;

[0103] Take 16.2g of benzoyl acetone and 110g of methanol, stir evenly, add 15g of acrylic acid and 43g of tetrabutyl titanate, stir evenly, add 0.5g of microsphere-loaded graphene, stir for 2.5h, and obtain titanium dioxide-graphene sol;

[0104] Take 10 g of silica sol and 10 g of titanium dioxide-graphene sol, stir evenly to obtain a composite sol;

[0105] Step 5:

[0106] The steel strip is placed in an alkaline washing solution at 57° C. for 8 minutes, taken out, washed, and dried to obtain an alkaline washed steel strip; the alkaline washing solution comprises the following components: 10 g / L sodium hydroxide, 20 g / L sodium carbonate, and 1 g / L sodium dodecyl sulfate;

[0107] The steel strip comprises the following components, in percentage by mass: 0.6wt% of Mn, 0.27wt% of Si, 0.17wt% of C, 0.03wt% of S, 0.03wt% of P, 0.2wt% of Cr, 0.2wt% of Ni, and the balance is Fe;

[0108] The alkali-washed steel strip is placed in a pickling solution at a temperature of 43°C for 23 minutes, taken out, washed, and dried to obtain a pickled steel strip. After pickling, the steel strip is annealed at 740°C for 42 seconds to obtain a pretreated steel strip. The pickling solution includes the following components: 0.08 g / L sodium dodecyl sulfonate, 2 g / L benzotriazole, and 32% hydrochloric acid. The concentration of the pickling solution is 80 g / L.

[0109] Anodizing the pretreated steel strip to obtain a highly wear-resistant and anti-fingerprint stainless steel strip;

[0110] The working conditions of anodization are: 1 kW AC power supply, 0.3 A constant current, 100 Hz frequency, and 12 min time; the electrolyte used for anodization is: 100 mL deionized water as solvent, including 0.5 g sulfuric acid, 0.8 g phytic acid, 5 g disodium ethylenediaminetetraacetic acid, 0.1 g nano-aluminum oxide, and 1 g composite sol.

[0111] Comparative Example 3: No graphene loaded with microspheres is added to the sol, and the rest is the same as Example 1:

[0112] Step 1: Preparation of styrene microspheres:

[0113] Take 300 mL of isoamyl acetate and 15 g of maleic anhydride, stir evenly, add 16 g of styrene and 0.2 g of azobisisobutyronitrile, purge with nitrogen for 35 min, heat in a water bath at 83 °C for 2.5 h, centrifuge, wash and dry to obtain compound A;

[0114] Take 2.4 g of ethylamine and 1 g of ammonia water, stir evenly to obtain reagent A; take 10 g of compound A, 90 mL of deionized water, and reagent A, stir at 73°C for 45 min, introduce nitrogen gas to pressurize to 0.6 mPa, heat to 161°C, stir for 5 days, dialyze, and freeze-dry to obtain styrene microspheres;

[0115] Step 2: Preparation of modified graphene:

[0116] Take 0.1 g of graphene oxide and 3 g of maleic anhydride, mix them evenly, react at 121 ° C for 4.5 h, wash with deionized water until the pH value reaches 7, add 1 mol / L sodium hydroxide aqueous solution until the pH value reaches 11, centrifuge, wash, filter, add 100 mL of ethanol, ultrasonically disperse, add 2 g of perfluorodecyltrichlorosilane, stir and react for 7 h, centrifuge, wash, and dry to obtain modified graphene;

[0117] Step 3: Preparation of graphene loaded microspheres:

[0118] Take 8 g of styrene microspheres and 200 mL of deionized water, stir evenly, add 0.2 g of modified graphene, heat to 73 ° C, stir for 7.5 h, cool, centrifuge, wash, and dry to obtain graphene loaded with microspheres;

[0119] Step 4: Preparation of composite sol:

[0120] Take 20 g of ethyl orthosilicate, 110 g of methanol, 5 mL of deionized water, and 3.5 g of hydrochloric acid, stir evenly to obtain a silica sol;

[0121] Take 16.2g of benzoyl acetone and 110g of methanol, stir evenly, add 15g of acrylic acid and 43g of tetrabutyl titanate, stir evenly to obtain titanium dioxide sol;

[0122] Take 10g of silica sol and 10g of titanium dioxide sol, stir them evenly to obtain a composite sol;

[0123] Step 5:

[0124] The steel strip is placed in an alkaline washing solution at 57° C. for 8 minutes, taken out, washed, and dried to obtain an alkaline washed steel strip; the alkaline washing solution comprises the following components: 10 g / L sodium hydroxide, 20 g / L sodium carbonate, and 1 g / L sodium dodecyl sulfate;

[0125] The steel strip comprises the following components, in percentage by mass: 0.6wt% of Mn, 0.27wt% of Si, 0.17wt% of C, 0.03wt% of S, 0.03wt% of P, 0.2wt% of Cr, 0.2wt% of Ni, and the balance is Fe;

[0126] The alkali-washed steel strip is placed in a pickling solution at a temperature of 43°C for 23 minutes, taken out, washed, and dried to obtain a pickled steel strip. After pickling, the steel strip is annealed at 740°C for 42 seconds to obtain a pretreated steel strip. The pickling solution includes the following components: 0.08 g / L sodium dodecyl sulfonate, 2 g / L benzotriazole, and 32% hydrochloric acid. The concentration of the pickling solution is 80 g / L.

[0127] Anodizing the pretreated steel strip to obtain a highly wear-resistant and anti-fingerprint stainless steel strip;

[0128] The working conditions of anodization are: an AC power supply of 1 kW, a constant current of 0.3 A, a frequency of 100 Hz, and a time of 12 min; the electrolyte used for anodization is: 100 mL of deionized water as a solvent, including 0.5 g of sulfuric acid, 0.8 g of phytic acid, 5 g of disodium ethylenediaminetetraacetic acid, 0.1 g of nano-aluminum oxide, 0.1 g of graphene loaded with microspheres, and 1 g of composite sol.

[0129] experiment:

[0130] The stainless steel strips prepared in Examples 1-3 and Comparative Examples 1-3 were used for performance testing. The wear resistance was tested using an MMV-1A multifunctional material friction behavior tester. The grinding material was GCr15 with a diameter of 5 mm and a rotation speed of 250 r·min. -1 , the load is 400g, the grinding time is 30min, and the wear amount is obtained; the water contact angle of the stainless steel belt is tested, and the data obtained are as follows:

[0131]

[0132] Conclusion: From the comparison of the data in the table, it can be seen that in Comparative Example 1, no styrene microspheres are added, the hydrophobicity of the stainless steel strip deteriorates, the water contact angle drops to 118°, and the anti-fingerprint property of the stainless steel strip deteriorates. Comparative Example 2 does not use maleic anhydride to modify the graphene, the number of styrene microspheres loaded on the modified graphene decreases, the dispersibility of the graphene deteriorates, and the performance of the stainless steel strip decreases. Comparative Example 3 does not add microsphere-loaded graphene to the sol, and the performance of the stainless steel strip decreases. Examples 1-3 of the present invention prepare a silica and titanium dioxide sol, the addition of which can improve the hydrophobicity of the surface of the stainless steel strip, and then the present invention composites the microsphere-loaded graphene with the sol and adds them together to the electroplating solution. The sol-gel process can provide a uniform and stable carrier, so that the microsphere-loaded graphene is more evenly distributed in the electroplating layer, thereby enhancing the wear resistance and anti-fingerprint property of the stainless steel strip.

[0133] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A preparation process of a highly wear-resistant and anti-fingerprint stainless steel belt, characterized in that: The following steps are involved: Step 1: Take ethyl orthosilicate, methanol, deionized water, and hydrochloric acid, stir evenly to obtain a silica sol; take benzoyl acetone and methanol, stir evenly, add acrylic acid and tetrabutyl titanate, stir evenly, add graphene loaded with microspheres, stir for 2-3 hours, and obtain a titanium dioxide-graphene sol; Step 2: Take silica sol and titanium dioxide-graphene sol, stir them evenly to obtain a composite sol; Step 3: Take the steel strip, alkali wash and pickle wash to obtain the pre-treated steel strip; Step 4: Anodizing the pretreated steel strip to obtain a highly wear-resistant and anti-fingerprint stainless steel strip; The electrolyte used for anodizing includes the following components: deionized water, sulfuric acid, phytic acid, disodium ethylenediaminetetraacetic acid, nano-aluminum oxide, and composite sol; The preparation method of the microsphere-loaded graphene is as follows: taking styrene microspheres and deionized water, stirring evenly, adding modified graphene, heating to 70-75° C., stirring for 7-8 hours, cooling, centrifuging, washing, and drying to obtain the microsphere-loaded graphene; The preparation method of the styrene microspheres comprises the following steps: S1: Take isoamyl acetate and maleic anhydride, stir evenly, add styrene and azobisisobutyronitrile, purge with nitrogen for 30-40 minutes, heat in a water bath at 80-85°C for 2-3 hours, centrifuge, wash and dry to obtain compound A; S2: Take ethylamine and ammonia water, stir evenly to obtain reagent A; take compound A, deionized water, and reagent A, stir at 70-75°C for 40-50 minutes, introduce nitrogen, heat to 160-162°C, stir for 5-5.5 days, dialyze, and freeze-dry to obtain styrene microspheres; The preparation method of modified graphene is as follows: take graphene oxide and maleic anhydride, mix them evenly, react them at 120-122° C. for 4-5 hours, wash them with deionized water, dropwise add sodium hydroxide aqueous solution, centrifuge, wash, filter, add ethanol, ultrasonically disperse, add perfluorodecyltrichlorosilane, stir and react for 6-8 hours, centrifuge, wash, and dry to obtain modified graphene.

2. The process for preparing a highly wear-resistant and anti-fingerprint stainless steel strip according to claim 1, characterized in that: The mass ratio of the silica sol to the titanium dioxide-graphene sol is 1:(1-1.2).

3. The preparation process of a highly wear-resistant and anti-fingerprint stainless steel belt according to claim 1, characterized in that: The steel strip includes the following components, in percentage by mass: 0.30wt%-0.7wt% of Mn, 0.25wt%-0.30wt% of Si, 0.15wt%-0.20wt% of C, 0.02wt%-0.045wt% of P, 0.01wt%-0.045wt% of S, 0.1wt%-0.25wt% of Cr, 0.1wt%-0.25wt% of Ni, and the balance is Fe.

4. The process for preparing a highly wear-resistant and anti-fingerprint stainless steel strip according to claim 1, characterized in that: The mass ratio of the styrene microspheres, deionized water and modified graphene is (7-8):200:0.

2.

5. A highly wear-resistant and anti-fingerprint stainless steel belt prepared according to the preparation process of a highly wear-resistant and anti-fingerprint stainless steel belt according to any one of claims 1 to 4.