Composite hydrogel with'three-section 'hardness gradient as well as preparation method and application of composite hydrogel

By developing a dental pulp regeneration material with a three-stage hardness gradient composite hydrogel, the problems of poor induced differentiation of dental pulp regenerative stem cells and insufficient blood supply have been solved, dentin repair and blood vessel regeneration have been achieved, and dental treatment has been improved. Effect.

CN118846243APending Publication Date: 2024-10-29SHANXI MEDICAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410880636.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

The poor induction and differentiation of existing dental pulp regenerative stem cells and the lack of effective blood supply at the apical stenosis result in a poor prognosis for the treatment of pulp and periapical diseases, especially for permanent teeth and severe periapical diseases.

Method used

Develop a composite hydrogel with a three-stage hardness gradient, including modified gelatin, silk fibroin and hyaluronic acid. Photosensitive groups are introduced through the acylation reaction to form an injectable light-cured three-layer structure of loose, middle and dense layers. Hydrogel adapts to complex root canal morphology and promotes pulp regeneration and vascular induction.

Benefits of technology

It realizes dentin repair and induces vascular regeneration, is suitable for complex root canal filling and repair, improves tooth prognosis, and has broad application prospects, especially in the treatment of permanent teeth and severe periapical diseases.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118846243A_ABST
    Figure CN118846243A_ABST
Patent Text Reader

Abstract

The invention discloses composite hydrogel with'three-section 'hardness gradient as well as a preparation method and application of the composite hydrogel. Preparing a loose lower layer containing modified gelatin hydrogel; a middle layer containing high-concentration modified gelatin hydrogel is formed on the basis of the lower layer, and the mechanical property of the middle layer is matched with that of physiological dental pulp; on the basis of the middle layer, a compact upper layer hydrogel formed by covalent cross-linking curing of modified silk fibroin (SilMA), modified hyaluronic acid (HAMA) and modified gelatin is formed. The invention provides application of the hydrogel composite material in preparation of a material for promoting dental pulp regeneration or a filling and repairing material for irregular root canal inflammation. The photo-curing three-section type integrated hydrogel capable of being locally injected, prepared by the invention, has excellent effects of repairing dentin and inducing revascularization, and particularly has a wide application prospect in complex root canal filling and repairing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a medical modified polymer material, and in particular to a composite hydrogel with a "three-stage" hardness gradient, and a preparation method and application thereof. Background Art

[0002] Pulpitis and periapical disease are among the most common inflammatory oral diseases, with a reported global prevalence of 16%-86%. Tooth defects and edentulousness caused by periapical disease have a great impact on patients' physiology and psychology. At present, periapical disease mainly relies on root canal therapy (RCT), which is to remove the pulp and replace the damaged or infected pulp with inert materials. The pulp plays a vital role in maintaining immune defense, sensory system and regeneration of the pulp-dentin complex. Pulp removal often leads to loss of nutrition of the tooth, and the tooth's ability to resist fracture is greatly reduced, which may lead to susceptibility to root fracture and poor long-term results. In addition, the root canal anatomy is complex and varies greatly from person to person. The presence of lateral root canals and accessory root canals increases the failure rate of root canal treatment. For patients with severe apical destruction, root canal treatment is no longer applicable. Therefore, the regeneration of the dentin-pulp complex is of great significance for restoring tooth vitality, restoring tooth biological function and extending the life cycle of pulpless teeth. There is an urgent need to develop a new treatment method to deal with various types of pulp diseases in clinical practice. Pulp regeneration tissue engineering has emerged as the times require. It uses tissue engineering technology to improve pulp infection, restore pulp tissue function and normal anatomical morphology, extend tooth life and improve patients' quality of life.

[0003] Endodontic regeneration, also known as endodontic regenerative therapy, aims to remove diseased or necrotic pulp tissue and replace it with healthy, viable pulp tissue. In 2016, the American Association of Endodontists officially defined endodontic regeneration as the use of biological procedures to replace damaged tooth structures, including the pulp-dentin complex, root and other structures, to form physiological and functional pulp-like tissue and restore biological function.

[0004] Human dental pulp stem cells (hDPSCs) combined with bioactive scaffolds are considered to be an ideal substitute for pulp tissue. Stem cells can differentiate into vascular and avascular mineralized tissues, which are crucial in pulp tissue regeneration. Scaffold materials provide an ideal space for stem cell growth, providing a strong guarantee for pulp tissue regeneration. Although stem cell therapy as a clinical method has made breakthrough progress, due to the complex anatomical structure of the root canal system and the narrow apical foramen leading to poor blood supply, current treatment is limited to deciduous teeth and young permanent teeth. The prognosis for permanent teeth and severe periapical diseases is often poor. There are many problems in clinical practice, and it is urgent to develop a suitable and effective stem cell induction differentiation technology and transportation strategy to deal with the difficult problems caused by complex pulp and periapical diseases, give full play to the differentiation and regeneration functions of stem cells, and improve the prognosis of the tooth. Summary of the invention

[0005] In order to solve the technical problems of poor induction and differentiation of existing dental pulp regeneration stem cells and lack of effective blood supply to the narrow apex, the present invention provides an injectable light-cured three-stage integrated hydrogel integrating apical blood vessels and coronal dentin mineralization and a preparation method thereof.

[0006] In a first aspect of the present invention, a composite hydrogel having a "three-stage" hardness gradient is provided, comprising a three-layer structure:

[0007] (1) A loose and soft lower layer containing modified gelatin hydrogel (GelMA);

[0008] (2) forming a middle layer containing a relatively high concentration of modified gelatin hydrogel on the basis of the loose lower layer of step (1), the mechanical properties of which match those of the physiological dental pulp;

[0009] (3) On the basis of the middle layer in step (2), a dense upper layer hydrogel is formed by covalently cross-linking and solidification of modified silk fibroin (SilMA), modified hyaluronic acid (HAMA) and modified gelatin.

[0010] Furthermore, the modified silk fibroin, modified hyaluronic acid and modified gelatin all contain photosensitive groups.

[0011] The loose lower layer accounts for 10-20% of the volume fraction of the three-stage integrated hydrogel, the middle layer matching the physiological pulp mechanical properties accounts for 60-80% of the volume fraction of the three-stage integrated hydrogel, and the dense upper layer accounts for 10-20% of the volume fraction of the three-stage integrated hydrogel.

[0012] The second aspect of the present invention is a method for preparing the above-mentioned composite hydrogel with a "three-stage" hardness gradient, which comprises the following steps:

[0013] (1) subjecting silk fibroin, hyaluronic acid and gelatin to acylation reaction respectively, thereby obtaining silk fibroin containing a photosensitive group, hyaluronic acid containing a photosensitive group and gelatin containing a photosensitive group;

[0014] (2) preparing the gelatin containing photosensitizing groups into gelatin sol; mixing the silk fibroin containing photosensitizing groups, the hyaluronic acid containing photosensitizing groups and the gelatin containing photosensitizing groups into silk fibroin-hyaluronic acid-gelatin sol; (3) separately photocuring the gelatin sol with the two mechanical properties and the silk fibroin-hyaluronic acid-gelatin sol to form a three-section integrated hydrogel having a loose and soft upper layer, a middle layer matching the physiological mechanical properties of dental pulp and a dense upper layer.

[0015] Furthermore, in the silk fibroin-hyaluronic acid-gelatin sol, the concentration of silk fibroin is 1% wv, the concentration of hyaluronic acid is 4% wv, and the concentration of gelatin is 4-10% wv.

[0016] Furthermore, the concentration of gelatin in the gelatin sol is 3-15% wv.

[0017] Furthermore, the three-segment structures are combined into a three-segment integrated structure through chemical bonds or physical interlocking.

[0018] Furthermore, the light curing time is 3-15s.

[0019] The second aspect of the present invention provides a locally injectable light-curable three-stage integrated hydrogel composite material obtained by the preparation method, comprising a loose upper layer of modified gelatin hydrogel, a middle layer of modified gelatin hydrogel with a higher concentration matching the mechanical properties of dental pulp, and a lower layer of modified silk fibroin, modified hyaluronic acid, and modified gelatin covalently cross-linked hydrogel. The upper layer, the middle layer, and the lower layer are physically combined into a three-stage integrated structure.

[0020] The present invention comprises a step in which the loose lower layer is close to the apical foramen and at least partially contacts with the periapical tissue, and a step in which the dense upper layer is close to the coronal hard tissue.

[0021] The third aspect of the present invention provides a locally injectable light-curable three-stage integrated osteogenic hydrogel composite material for use in the preparation of a material for promoting dental pulp regeneration or a material for filling and repairing irregular root canal inflammation.

[0022] The beneficial effects of the present invention include but are not limited to:

[0023] The present invention firstly introduces photosensitive groups into gelatin, silk fibroin and hyaluronic acid by acylation reaction, then mixes them with PBS and LAP to obtain a hydrogel in a sol state, and finally performs a photocuring treatment to make the material undergo a sol-gel transition to obtain a hydrogel with a three-stage integrated structure.

[0024] The three-stage integrated hydrogel prepared by the present invention is injected after light curing to adapt to the complex root canal morphology.

[0025] The three-section integrated hydrogel prepared by the present invention realizes firm bonding due to its inherent covalent bond connection, thereby providing sufficient hardness to induce differentiation signals.

[0026] The locally injectable light-curable three-stage integrated hydrogel prepared by the present invention has excellent dentin repair and angiogenesis induction effects, and has broad application prospects, especially in complex root canal filling and repair.

[0027] The preparation process of the invention is simple and can be industrialized for mass production and popularized for application. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The infrared spectra of amidated gelatin, amidated silk fibroin, and amidated hyaluronic acid are shown.

[0029] Figure 2 The three-section integrated structure, injectability and shape plasticity of the hydrogel are shown.

[0030] Figure 3 The frozen sections of hydrogels with different hardness ranges are shown, where Low stiffness is the loose and soft gelatin layer in the lower layer, Medium stiffness is the gelatin layer in the middle layer that matches the physiological pulp mechanical properties, and High stiffness is the dense silk fibroin, hyaluronic acid and gelatin layer in the upper layer.

[0031] Figure 4 It shows that each layer of hydrogel has a good ability to promote cell proliferation over the culture time.

[0032] Figure 5 The results showed that the dense layer promoted the regeneration of dentin after 7 days of culture, and more DSPP protein was expressed.

[0033] Figure 6 It was shown that after 7 days of culture, the gelatin layer (middle layer) that matched the mechanical properties of physiological dental pulp promoted angiogenesis and had more CD31 protein expression.

[0034] Figure 7 It was shown that after 3 days of culture, the loosened lower layer promoted the growth of fibers around the root tip and had more VEGF expression. DETAILED DESCRIPTION

[0035] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0036] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that the upper and lower limits of the scope and each intermediate value therebetween are specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0037] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as commonly understood by those skilled in the art to which the invention belongs. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials related to the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0038] One aspect of the present invention provides a locally injectable, light-curable, three-stage integrated hydrogel, comprising (1) a loose lower layer containing modified gelatin; (2) an intermediate layer containing a gelatin hydrogel having a higher concentration matching the physiological mechanical properties of dental pulp, formed on the basis of the loose lower layer; and (3) a dense upper layer containing modified silk fibroin, hyaluronic acid and gelatin hydrogel, formed on the basis of the intermediate layer.

[0039] Example 1

[0040] This embodiment shows a method for preparing a locally injectable light-cured three-stage integrated osteogenic hydrogel composite material, which comprises the following steps:

[0041] Step (1): Preparation of methacrylated gelatin: Soak 5g of type A gelatin in 50ml of deionized water and stir thoroughly in a magnetic stirrer until completely dissolved. While stirring, heat the mixture in a water bath to 60°C (and maintain at this temperature). After 3 hours, the gelatin is completely dissolved and the solution is a light yellow transparent liquid. Adjust the temperature of the water bath to 50°C, add 4ml of methacrylic anhydride dropwise while stirring, and incubate for 3 hours to promote the modification of methacrylic anhydride on the gelatin. After the reaction is completed, add 250ml of PBS to terminate the reaction. Then transfer the diluted solution to a dialysis bag with a molecular weight cutoff of 12,000, protect it from light, and dialyze it with a large amount of deionized water in a constant temperature box at 40°C for 1 week. During this period, the deionized water is replaced every 4 hours. After the dialysis is completed, the dialysate is centrifuged at 10,000r / min for 5 minutes, and then filtered with a cell filter with a diameter of 70um to remove the unreacted white methacrylic anhydride precipitate. The filtrate was then transferred to a -80°C ultra-low temperature freezer and frozen overnight. The next day, it was placed in a freeze dryer and freeze-dried until completely dehydrated (about 3-4 days. The thinner the thickness of the filtrate frozen block, the easier it is to freeze-dry) to obtain a white sponge. Finally, the freeze-dried GelMA (methacrylylated gelatin) was placed in a brown bottle and refrigerated for storage.

[0042] Step (2): Preparation of methacryloyl hyaluronic acid: 1 g of hyaluronic acid is gradually added in batches to 100 ml of deionized water under uniform stirring. During the addition of hyaluronic acid, it is necessary to avoid the hyaluronic acid from forming lumps. Hyaluronic acid with a hydrophobic layer on the surface is difficult to dissolve. Stir at a speed of 200 r / min at room temperature until it is completely dissolved and the liquid is clear and transparent. Under ice bath conditions, 1 ml of methacrylic anhydride is added dropwise to the solution, and a 5 mol / L NaOH solution is used at the same time to keep the solution pH at 8.5. Protect from light and continue to fully react under ice bath conditions for 24 hours. After the reaction is completed, the reaction product is loaded into a dialysis bag with a molecular weight cutoff of 14,000 and dialyzed in deionized water at room temperature for 4 days. During this period, the deionized water is replaced every 4 hours. The dialyzate is then transferred to an ultra-low temperature refrigerator at -80°C and frozen overnight. The next day, it is placed in a freeze dryer and freeze-dried until completely dehydrated (about 3-4 days, the smaller the thickness of the filtrate frozen block, the easier it is to freeze-dry), to obtain a white flocculent substance. Finally, the freeze-dried MeHA (methacryloyl hyaluronic acid) is placed in a brown bottle and refrigerated for storage for later use.

[0043] Step (3): Preparation of methacrylylated silk fibroin:

[0044] Degumming: 150g of raw silk (SF) was placed in 6L of 0.05wt% NaCO3 aqueous solution and boiled at 100℃ for 30min to remove sericin, and repeated three times. After being fully washed and stretched, it was dried in an oven at 60℃ overnight to obtain refined silk, which was stretched for later use.

[0045] Dissolution of silk fibroin: Prepare 100 ml of LiBr (9M) solution.

[0046] The required weight of LiBr g = (86.844 g / mol) (9 mol / l) (the volume of LiBr solution required / 1000 ml)

[0047] It is calculated that 78.2 g of anhydrous lithium bromide is needed to prepare 100 ml of LiBr (9M) solution. First, dissolve 78.2 g of anhydrous lithium bromide in 50 ml of pure water, gently stir with a glass rod until completely dissolved, and then add pure water to make up the volume to 100 ml to prepare 9M LiBr. Note that before making the solution reach the final required volume, ensure that the lithium bromide is completely dissolved.

[0048] 20 g of extracted refined silk was dissolved in 100 ml of lithium bromide (BrLi, 9 M) aqueous solution to prepare 20% (weight / volume) RSF. The beaker was first covered with plastic wrap and then with aluminum foil, and then the beaker was transferred to a flow oven and incubated at 60 °C for 1 hour. The beaker in the oven was gently shaken every 20 minutes to promote complete dissolution of SF.

[0049] Silk fibroin methylation modification: Filter the above 100 ml solution into a beaker with 12 layers of gauze, and cover the beaker with plastic wrap and aluminum foil to minimize air absorption in the solution. Heat in a 60°C water bath and stir at 300 rpm for 10 minutes. Then increase the stirring rate to 800 rpm, slowly drip 6 ml of glycidyl methacrylate (GMA) to obtain a mixed solution with a GMA concentration of 424 mM, and continue to stir at 300 rpm for 6 hours at 60°C to allow GMA and SF molecules to fully react. The timing of the reaction between GMA and RSF is very critical. After dissolving SF in LiBr, GMA reacts immediately with RSF solution to produce a better RSF-GMA reactant than using freeze-dried RSF, and its mechanism is unknown. The prepared methacrylylated silk fibroin (Sil-MA) solution was dialyzed in distilled water for 4 days, frozen at -40°C for 12 hours, and then freeze-dried for 36 hours to obtain a white sponge, which was stored at -80°C in the dark until use.

[0050] 30 mg of the GelMA obtained in step (1) and 1 mg of the photoinitiator LAP were dissolved in 1 ml of PBS to obtain a photocurable GelMA solution A.

[0051] Take 50 mg of the GelMA obtained in step (1) and 1 mg of the photoinitiator LAP and dissolve them in 1 ml of PBS to obtain a photocurable GelMA solution B.

[0052] Take 30 mg of GelMA obtained in step (1), 10 mg of HAMA obtained in step (2), 10 mg of Sil-MA obtained in step (3) and 1 mg of photoinitiator LAP and dissolve them in 1 ml of PBS to obtain a photocurable GelMA / HAMA / Sil-MA mixed solution.

[0053] The photocurable GelMA solution A obtained above was placed in a 1 ml syringe and cured for 20 seconds using a visible blue light curing lamp to obtain GelMA gel 1;

[0054] The photocurable GelMA solution B was cured in a 1 ml syringe using a visible blue light curing lamp for 30 seconds to obtain GelMA gel 2;

[0055] The photocurable GelMA / HAMA / Sil-MA mixed solution was cured in a 1 ml syringe using a visible blue light curing lamp for 30 seconds to obtain a GelMA / HAMA / Sil-MA gel.

[0056] Take the prepared dentin fragments, first inject 10% GelMA gel 1 into the root apex; close to GelMA gel 1, inject 80% GelMA gel 2 into the root canal; close to GelMA gel 2, inject 10% GelMA / HAMA / Sil-MA gel into the crown of the root canal to seal the crown.

[0057] Example 2

[0058] This embodiment shows a method for preparing a locally injectable light-cured three-stage integrated osteogenic hydrogel composite material, which comprises the following steps:

[0059] Step (1): Preparation of methacrylic acid acylated gelatin: 5g of type A gelatin is soaked in 50ml of deionized water and stirred thoroughly in a magnetic stirrer until completely dissolved. While stirring, the mixture is heated in a water bath to 60°C (and maintained at this temperature). After 3 hours, the gelatin is completely dissolved and the solution is a light yellow transparent liquid. The temperature of the water bath is adjusted to 50°C, and 4ml of methacrylic anhydride is added dropwise while stirring. The mixture is incubated for 3 hours to promote the modification of methacrylic anhydride on the gelatin. After the reaction is completed, 250ml of PBS is added to terminate the reaction. The diluted solution is then transferred to a dialysis bag with a molecular weight cutoff of 12,000, protected from light, and dialyzed with a large amount of deionized water in a constant temperature box at 40°C for 1 week. During this period, the deionized water is replaced every 4 hours. After the dialysis is completed, the dialysate is centrifuged at 10,000r / min for 5 minutes and then filtered with a cell filter with a diameter of 70um to remove the unreacted white methacrylic anhydride precipitate. The filtrate was then transferred to a -80°C ultra-low temperature freezer and frozen overnight. The next day, it was placed in a freeze dryer and freeze-dried until completely dehydrated (about 3-4 days. The thinner the thickness of the filtrate frozen block, the easier it is to freeze-dry) to obtain a white sponge. Finally, the freeze-dried GelMA (methacrylylated gelatin) was placed in a brown bottle and refrigerated for storage.

[0060] Step (2): Preparation of methacryloyl hyaluronic acid: 1 g of hyaluronic acid is gradually added in batches to 100 ml of deionized water under uniform stirring. During the addition of hyaluronic acid, it is necessary to avoid the hyaluronic acid from forming lumps. Hyaluronic acid with a hydrophobic layer on the surface is difficult to dissolve. Stir at a speed of 200 r / min at room temperature until it is completely dissolved and the liquid is clear and transparent. Under ice bath conditions, 1 ml of methacrylic anhydride is added dropwise to the solution, and a 5 mol / L NaOH solution is used at the same time to keep the solution pH at 8.5. Protect from light and continue to fully react under ice bath conditions for 24 hours. After the reaction is completed, the reaction product is loaded into a dialysis bag with a molecular weight cutoff of 14,000 and dialyzed in deionized water at room temperature for 4 days. During this period, the deionized water is replaced every 4 hours. The dialyzate is then transferred to an ultra-low temperature refrigerator at -80°C and frozen overnight. The next day, it is placed in a freeze dryer and freeze-dried until completely dehydrated (about 3-4 days, the smaller the thickness of the filtrate frozen block, the easier it is to freeze-dry), to obtain a white flocculent substance. Finally, the freeze-dried MeHA (methacryloyl hyaluronic acid) is placed in a brown bottle and refrigerated for storage for later use.

[0061] Step (3): Preparation of methacrylylated silk fibroin:

[0062] Degumming: 150g of raw silk (SF) was placed in 6L of 0.05wt% NaCO3 aqueous solution and boiled at 100℃ for 30min to remove sericin, and repeated three times. After being fully washed and stretched, it was dried in an oven at 60℃ overnight to obtain refined silk, which was stretched for later use.

[0063] Dissolution of silk fibroin: Prepare 100 ml of LiBr (9M) solution.

[0064] The required weight of LiBr g = (86.844 g / mol) (9 mol / l) (the volume of LiBr solution required / 1000 ml)

[0065] It is calculated that 78.2 g of anhydrous lithium bromide is needed to prepare 100 ml of LiBr (9M) solution. First, dissolve 78.2 g of anhydrous lithium bromide in 50 ml of pure water, gently stir with a glass rod until completely dissolved, and then add pure water to make up the volume to 100 ml to prepare 9M LiBr. Note that before making the solution reach the final required volume, ensure that the lithium bromide is completely dissolved.

[0066] 20 g of extracted refined silk was dissolved in 100 ml of lithium bromide (BrLi, 9 M) aqueous solution to prepare 20% (weight / volume) RSF. The beaker was first covered with plastic wrap and then with aluminum foil, and then the beaker was transferred to a flow oven and incubated at 60 °C for 1 hour. The beaker in the oven was gently shaken every 20 minutes to promote complete dissolution of SF.

[0067] Silk fibroin methylation modification: Filter the above 100 ml solution into a beaker with 12 layers of gauze, and cover the beaker with plastic wrap and aluminum foil to minimize air absorption in the solution. Heat in a 60°C water bath and stir at 300 rpm for 10 minutes. Then increase the stirring rate to 800 rpm, slowly drip 6 ml of glycidyl methacrylate (GMA) to obtain a mixed solution with a GMA concentration of 424 mM, and continue to stir at 300 rpm for 6 hours at 60°C to allow GMA and SF molecules to fully react. The timing of the reaction between GMA and RSF is very critical. After dissolving SF in LiBr, GMA reacts immediately with RSF solution to produce a better RSF-GMA reactant than using freeze-dried RSF, and its mechanism is unknown. The prepared methacrylylated silk fibroin (Sil-MA) solution was dialyzed in distilled water for 4 days, frozen at -40°C for 12 hours, and then freeze-dried for 36 hours to obtain a white sponge, which was stored at -80°C in the dark until use.

[0068] 150 mg of the GelMA obtained in step (1) and 1 mg of the photoinitiator LAP were dissolved in 1 ml of PBS to obtain a photocurable GelMA solution A;

[0069] Take 50 mg of the GelMA obtained in step (1) and 1 mg of the photoinitiator LAP and dissolve them in 1 ml of PBS to obtain a photocurable GelMA solution B;

[0070] Take 150 mg of GelMA obtained in step (1), 10 mg of HAMA obtained in step (2), 10 mg of Sil-MA obtained in step (3) and 1 mg of photoinitiator LAP and dissolve them in 1 ml of PBS to obtain a photocurable GelMA / HAMA / Sil-MA mixed solution.

[0071] The photocurable GelMA solution A obtained above was cured in a 1 ml syringe using a visible blue light curing lamp for 30 seconds to obtain GelMA gel 1, and the photocurable GelMA solution B was cured in a 1 ml syringe using a visible blue light curing lamp for 30 seconds to obtain GelMA gel 2; the photocurable GelMA / HAMA / Sil-MA mixed solution was cured in a 1 ml syringe using a visible blue light curing lamp for 30 seconds to obtain GelMA / HAMA / Sil-MA gel. Take the prepared dentin fragment, first inject 20% of GelMA gel 1 into the root apex; close to GelMA gel 1, inject 60% of GelMA gel 2 into the root canal; close to GelMA gel 2, inject 20% of GelMA / HAMA / Sil-MA gel into the crown of the root canal to seal the crown.

[0072] Example 3

[0073] This embodiment shows a method for preparing a locally injectable light-cured three-stage integrated osteogenic hydrogel composite material, which comprises the following steps:

[0074] Step (1): Preparation of methacrylic acid acylated gelatin: 5g of type A gelatin is soaked in 50ml of deionized water and stirred thoroughly in a magnetic stirrer until completely dissolved. While stirring, the mixture is heated in a water bath to 60°C (and maintained at this temperature). After 3 hours, the gelatin is completely dissolved and the solution is a light yellow transparent liquid. The temperature of the water bath is adjusted to 50°C, and 4ml of methacrylic anhydride is added dropwise while stirring. The mixture is incubated for 3 hours to promote the modification of methacrylic anhydride on the gelatin. After the reaction is completed, 250ml of PBS is added to terminate the reaction. The diluted solution is then transferred to a dialysis bag with a molecular weight cutoff of 12,000, protected from light, and dialyzed with a large amount of deionized water in a constant temperature box at 40°C for 1 week. During this period, the deionized water is replaced every 4 hours. After the dialysis is completed, the dialysate is centrifuged at 10,000r / min for 5 minutes and then filtered with a cell filter with a diameter of 70um to remove the unreacted white methacrylic anhydride precipitate. The filtrate was then transferred to a -80°C ultra-low temperature freezer and frozen overnight. The next day, it was placed in a freeze dryer and freeze-dried until completely dehydrated (about 3-4 days. The thinner the thickness of the filtrate frozen block, the easier it is to freeze-dry) to obtain a white sponge. Finally, the freeze-dried GelMA (methacrylylated gelatin) was placed in a brown bottle and refrigerated for storage.

[0075] Step (2): Preparation of methacryloyl hyaluronic acid: 1 g of hyaluronic acid is gradually added in batches to 100 ml of deionized water under uniform stirring. During the addition of hyaluronic acid, it is necessary to avoid the hyaluronic acid from forming lumps. Hyaluronic acid with a hydrophobic layer on the surface is difficult to dissolve. Stir at a speed of 200 r / min at room temperature until it is completely dissolved and the liquid is clear and transparent. Under ice bath conditions, 1 ml of methacrylic anhydride is added dropwise to the solution, and a 5 mol / L NaOH solution is used at the same time to keep the solution pH at 8.5. Protect from light and continue to fully react under ice bath conditions for 24 hours. After the reaction is completed, the reaction product is loaded into a dialysis bag with a molecular weight cutoff of 14,000 and dialyzed in deionized water at room temperature for 4 days. During this period, the deionized water is replaced every 4 hours. The dialyzate is then transferred to an ultra-low temperature refrigerator at -80°C and frozen overnight. The next day, it is placed in a freeze dryer and freeze-dried until completely dehydrated (about 3-4 days, the smaller the thickness of the filtrate frozen block, the easier it is to freeze-dry), to obtain a white flocculent substance. Finally, the freeze-dried MeHA (methacryloyl hyaluronic acid) is placed in a brown bottle and refrigerated for storage for later use.

[0076] Step (3): Preparation of methacrylylated silk fibroin:

[0077] Degumming: 150g of raw silk (SF) was placed in 6L of 0.05wt% NaCO3 aqueous solution and boiled at 100℃ for 30min to remove sericin, and repeated three times. After being fully washed and stretched, it was dried in an oven at 60℃ overnight to obtain refined silk, which was stretched for later use.

[0078] Dissolution of silk fibroin: Prepare 100 ml of LiBr (9M) solution.

[0079] The required weight of LiBr g = (86.844 g / mol) (9 mol / l) (the volume of LiBr solution required / 1000 ml)

[0080] It is calculated that 78.2 g of anhydrous lithium bromide is needed to prepare 100 ml of LiBr (9M) solution. First, dissolve 78.2 g of anhydrous lithium bromide in 50 ml of pure water, gently stir with a glass rod until completely dissolved, and then add pure water to make up the volume to 100 ml to prepare 9M LiBr. Note that before making the solution reach the final required volume, ensure that the lithium bromide is completely dissolved.

[0081] 20 g of extracted refined silk was dissolved in 100 ml of lithium bromide (BrLi, 9 M) aqueous solution to prepare 20% (weight / volume) RSF. The beaker was first covered with plastic wrap and then with aluminum foil, and then the beaker was transferred to a flow oven and incubated at 60 °C for 1 hour. The beaker in the oven was gently shaken every 20 minutes to promote complete dissolution of SF.

[0082] Silk fibroin methylation modification: Filter the above 100 ml solution into a beaker with 12 layers of gauze, and cover the beaker with plastic wrap and aluminum foil to minimize air absorption in the solution. Heat in a 60°C water bath and stir at 300 rpm for 10 minutes. Then increase the stirring rate to 800 rpm, slowly drip 6 ml of glycidyl methacrylate (GMA) to obtain a mixed solution with a GMA concentration of 424 mM, and continue to stir at 300 rpm for 6 hours at 60°C to allow GMA and SF molecules to fully react. The timing of the reaction between GMA and RSF is very critical. After dissolving SF in LiBr, GMA reacts immediately with RSF solution to produce a better RSF-GMA reactant than using freeze-dried RSF, and its mechanism is unknown. The prepared methacrylylated silk fibroin (Sil-MA) solution was dialyzed in distilled water for 4 days, frozen at -40°C for 12 hours, and then freeze-dried for 36 hours to obtain a white sponge, which was stored at -80°C in the dark until use.

[0083] 40 mg of the GelMA obtained in step (1) and 1 mg of the photoinitiator LAP were dissolved in 1 ml of PBS to obtain a photocurable GelMA solution A;

[0084] Take 50 mg of the GelMA obtained in step (1) and 1 mg of the photoinitiator LAP and dissolve them in 1 ml of PBS to obtain a photocurable GelMA solution B;

[0085] Take 50 mg of GelMA obtained in step (1), 10 mg of HAMA obtained in step (2), 10 mg of Sil-MA obtained in step (3) and 1 mg of photoinitiator LAP and dissolve them in 1 ml of PBS to obtain a photocurable GelMA / HAMA / Sil-MA mixed solution.

[0086] The photocurable GelMA solution A obtained above was cured in a 1 ml syringe using a visible blue light curing lamp for 20 seconds to obtain GelMA gel 1, and the photocurable GelMA solution B was cured in a 1 ml syringe using a visible blue light curing lamp for 30 seconds to obtain GelMA gel 2; the photocurable GelMA / HAMA / Sil-MA mixed solution was cured in a 1 ml syringe using a visible blue light curing lamp for 30 seconds to obtain GelMA / HAMA / Sil-MA gel. Take the prepared dentin fragment, first inject 10% of GelMA gel 1 into the root apex, and slightly overfill the root apex by 2 mm; close to GelMA gel 1, inject 80% of GelMA gel 2 into the root canal; close to GelMA gel 2, inject 10% of GelMA / HAMA / Sil-MA gel into the crown of the root canal to seal the crown.

[0087] Comparative Example 1

[0088] A method for preparing a locally injectable hydrogel material is shown below, which comprises the following steps:

[0089] Preparation of methacrylic acid acylated gelatin: Soak 5g of type A gelatin in 50ml of deionized water and stir thoroughly in a magnetic stirrer until completely dissolved. While stirring, heat the mixture in a water bath to 60°C (and keep it at this temperature). After 3h, the gelatin is completely dissolved and the solution is a light yellow transparent liquid. Adjust the temperature of the water bath to 50°C, add 4ml of methacrylic anhydride dropwise while stirring, and incubate for 3h to promote the modification of methacrylic anhydride on gelatin. After the reaction is completed, add 250ml of PBS to terminate the reaction. Then transfer the diluted solution to a dialysis bag with a molecular weight cutoff of 12000, protect it from light, and dialyze it with a large amount of deionized water in a constant temperature box at 40°C for 1 week. During this period, the deionized water was replaced every 4h. After the dialysis is completed, the dialysate is centrifuged at 10000r / min for 5min, and then filtered with a cell filter with a diameter of 70um to remove the unreacted white precipitate of methacrylic anhydride. The filtrate was then transferred to a -80°C ultra-low temperature freezer and frozen overnight. The next day, it was placed in a freeze dryer and freeze-dried until completely dehydrated (about 3-4 days. The thinner the thickness of the filtrate frozen block, the easier it is to freeze-dry) to obtain a white sponge. Finally, the freeze-dried GelMA (methacrylylated gelatin) was placed in a brown bottle and refrigerated for storage.

[0090] Take 50 mg of the GelMA obtained in step (1) and 1 mg of the photoinitiator LAP and dissolve them in 1 ml of PBS to obtain a photocurable GelMA solution;

[0091] Through the above steps, a GelMA hydrogel in a solution state is obtained, the main component of which is a GelMA solution with a concentration of 50 mg / mL.

[0092] The photocurable GelMA solution obtained above was cured in a 1 ml syringe using a visible blue light curing lamp for 30 seconds to obtain a GelMA gel, and the prepared dentin fragment was taken to fill the entire root. Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention, rather than to limit it; although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the field should understand that they can still modify the technical solutions recorded in the above embodiments, or replace some of the technical features therein by equivalents. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A composite hydrogel with a "three-stage" hardness gradient, It is characterized in that A three-stage integrated hydrogel with a three-layer structure: (1) a loose lower layer containing a modified gelatin hydrogel; (2) forming a middle layer containing a relatively high concentration of modified gelatin hydrogel on the basis of the loose lower layer of step (1), the mechanical properties of which match those of the physiological dental pulp; (3) forming a dense upper layer hydrogel containing modified silk fibroin (SilMA), modified hyaluronic acid (HAMA) and modified gelatin by covalent cross-linking and solidification on the basis of the middle layer in step (2); The modified gelatin, modified silk fibroin and modified hyaluronic acid all contain photosensitive groups; The loose lower layer accounts for 10-20% of the volume fraction of the three-stage integrated hydrogel, the middle layer matching the physiological pulp mechanical properties accounts for 60-80% of the volume fraction of the three-stage integrated hydrogel, and the dense upper layer accounts for 10-20% of the volume fraction of the three-stage integrated hydrogel.

2. A method for preparing a composite hydrogel having a "three-stage" hardness gradient as described in claim 1, It is characterized in that First, photosensitive groups were introduced into gelatin, silk fibroin, and hyaluronic acid by acylation reaction, and then they were mixed with PBS and LAP to obtain a hydrogel in a sol state. Finally, the material was photocured to undergo a sol-gel transition, and a hydrogel with a three-stage integrated structure was obtained. The following steps are involved: (1) subjecting gelatin, silk fibroin and hyaluronic acid to acylation reaction respectively, to obtain gelatin GelMA containing a photosensitive group, silk fibroin Sil-MA containing a photosensitive group and hyaluronic acid HAMA containing a photosensitive group; (2) preparing the gelatin containing the photosensitive group into gelatin sols with two mechanical properties in the loose lower layer and the middle layer respectively; The silk fibroin containing the photosensitive group, the hyaluronic acid containing the photosensitive group and the gelatin containing the photosensitive group are mixed in the upper layer to prepare the silk fibroin-hyaluronic acid-gelatin sol; (3) The gelatin sol and silk fibroin-hyaluronic acid-gelatin sol with the two mechanical properties are light-cured respectively to form a three-section integrated hydrogel having a loose and soft upper layer, a middle layer matching the physiological mechanical properties of dental pulp, and a dense upper layer.

3. The method according to claim 2, It is characterized in that The concentration of gelatin in the gelatin sol is 3-15% wv; the concentration of silk fibroin in the silk fibroin-hyaluronic acid-gelatin sol is 1% wv, the concentration of hyaluronic acid is 4% wv, and the concentration of gelatin is 4-10% wv.

4. The method according to claim 2, It is characterized in that The three layers are physically joined together to form a three-section integrated structure.

5. The method according to claim 2, It is characterized in that The light curing time is 20-30s.

6. The method according to claim 2, It is characterized in that The method comprises the steps of filling the root apex region with the loose lower layer and having a small amount of gel overfilling the root apex region by 2 mm, and the dense upper layer being close to the coronal hard tissue.

7. The method according to claim 2, It is characterized in that The step (2) is specifically: Take 30-150 mg of gelatin GelMA containing photosensitive groups and photoinitiator LAP and dissolve them in PBS to obtain photocurable GelMA solution A; Take 50 mg of gelatin GelMA containing photosensitive groups and photoinitiator LAP and dissolve them in PBS to obtain photocurable GelMA solution B; Take 30-150 mg of gelatin GelMAGelMA containing photosensitive groups, 10 mg of hyaluronic acid HAMA containing photosensitive groups, 10 mg of silk fibroin Sil-MA containing photosensitive groups and photoinitiator LAP and dissolve them in PBS to obtain a photocurable GelMA / HAMA / Sil-MA mixed solution.

8. Use of a composite hydrogel with a "three-stage" hardness gradient according to claim 1, It is characterized in that Application in the preparation of materials promoting pulp regeneration or filling and repairing materials for irregular root canal inflammation.