Layered composite zinc-based material guided bone tissue regeneration membrane and preparation method thereof
Through the gradient distribution of layered composite zinc-based alloy materials, the problems of inertness and mechanical deficiencies of GBR membrane materials are solved, the antibacterial properties and bone-promoting properties are improved, and the treatment cost and failure rate are reduced.
Patent Information
- Application Number
- CN202410999764.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-10-29
AI Technical Summary
Existing GBR membrane materials have problems such as inert materials that cannot be degraded, insufficient mechanical support from polymers, and poor antibacterial properties, resulting in a high bone regeneration failure rate.
The antibacterial guided bone tissue regeneration membrane made of layered composite zinc-based alloy materials achieves uniform degradation and bone regeneration support by gradient distribution of antibacterial elements and bone-promoting elements in different layers of the membrane, combined with corrosion potential differences.
The membrane has good antibacterial and bone-promoting properties, uniform degradation and biocompatibility, avoids the defects of inert materials and polymer collagen membranes, and reduces treatment costs.
Smart Images

Figure CN118846261A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of medical devices, and in particular to an oral GBR membrane made of a layered composite zinc-based alloy material and a preparation method thereof, which can be applied in guided bone regeneration surgery. Technical Background
[0002] Tooth loss is usually caused by trauma, severe periodontitis, senile gingival atrophy, etc., which will have a significant impact on the patient's normal oral function and appearance. At present, oral implant surgery has become the main means of treating tooth loss. However, the success of such surgery requires that the patient has sufficient alveolar bone volume to ensure the firm implantation of the denture. Among patients with tooth loss, there is a common problem of insufficient bone quality and bone volume. In order to meet this challenge, guided bone regeneration (GBR) technology is usually used to restore the missing alveolar bone tissue before implant surgery.
[0003] In the bone defect area, osteoblasts grow at a slower rate, while surrounding soft tissues such as epithelial cells and connective tissue show a faster growth trend. In order to provide a more stable bone regeneration environment, GBR technology uses the physical barrier effect of implant materials to prevent soft tissue from occupying the space for osteoblast growth, ensuring that osteoblasts and other cells with slower proliferation rates grow effectively in the bone defect area, thereby achieving an effective increase in bone mass and quality. It should be noted that in this technology, the GBR membrane plays the role of a functional barrier membrane.
[0004] Although GBR technology can help patients restore alveolar bone, there are still patients who fail to reconstruct bone every year. The main reason is related to the material of the GBR membrane. According to the degradability, the GBR membranes currently used in clinical practice are mainly divided into two categories: non-degradable membranes and degradable membranes. The former are mostly inert materials such as polytetrafluoroethylene and titanium metal, which cannot be degraded and need to be removed through a secondary operation; they also have risks such as infection, wound dehiscence and membrane exposure. The latter is mainly made of high-molecular polymer materials, but it has the disadvantages of insufficient mechanical strength and too fast degradation rate. When the membrane degrades, it is easy to collapse, and it is difficult to maintain the space in the bone regeneration area in the later stage. In addition, the current two types of GBR membranes also have problems such as poor antibacterial properties and insufficient osteogenic function. Therefore, it is urgent to develop a new type of membrane that has both antibacterial and guided bone tissue regeneration. Summary of the invention
[0005] The purpose of the present invention is to provide a layered composite zinc-based alloy antibacterial guided bone tissue regeneration membrane to solve the problems that inert materials cannot be degraded, high molecular polymers cannot provide sufficient mechanical support, and the antibacterial and osteogenic properties of both are not ideal.
[0006] The present invention provides a layered composite zinc-based alloy antibacterial guided bone tissue regeneration membrane and describes in detail its preparation method. In order to achieve the above first objective, the present invention designs a layered composite zinc-based alloy antibacterial guided bone tissue regeneration membrane.
[0007] The structure of the regeneration membrane is as follows: the side in contact with the oral periodontal soft tissue serves as an antibacterial unit, which is a zinc-based material layer with a certain thickness of n layers (1≤n≤5) having antibacterial properties, and each layer is specifically marked as 1-n, and the smaller n is, the closer it is to the soft tissue side; the side in contact with the bone defect site serves as an osteogenic unit, which is a zinc-based material layer with a certain thickness of m layers (1≤m≤5) having osteogenic properties, and each layer is specifically marked as 2-m, and the smaller m is, the closer it is to the bone defect side; between the antibacterial unit and the osteogenic unit is a zinc-based material core layer with a certain thickness as a supporting unit; the GBR membrane is repeatedly bent ≥80 times without delamination.
[0008] Furthermore, the zinc-based material is pure zinc or a zinc alloy, and the mass percentage of a single alloying element in the zinc alloy is 0.001 to 10%.
[0009] Furthermore, the alloying elements in the antibacterial unit include one or more of copper, silver, cobalt, nickel, aluminum, molybdenum, lanthanum, zirconium, and gallium; the alloying elements in the osteogenic unit include one or more of lithium, strontium, calcium, phosphorus, magnesium, manganese, silicon, and barium; and the supporting unit is a zinc-based material with a higher corrosion potential than the adjacent 1-n and 2-m layers.
[0010] Furthermore, in the n-layer zinc-based material contained in the antibacterial unit, the content of alloying elements decreases gradually from 1-1 to 1-n, and the mass percentage of alloying elements between adjacent single layers differs by 0.1 to 9.999%; in the m-layer zinc-based material contained in the osteogenic unit, the content of alloying elements decreases gradually from 2-1 to 2-m, and the mass percentage of alloying elements between adjacent single layers differs by 0.1 to 9.999%.
[0011] Furthermore, the thickness of the regenerated film does not exceed 0.5 mm.
[0012] Furthermore, the regeneration membrane has conical holes with diameters ranging from 10 to 1000 μm. The holes on the side close to the soft tissue are larger to ensure the entry of nutrients; the holes on the side close to the bone defect are smaller to prevent soft tissue from growing into and occupying the bone defect space; the porosity is 5 to 90%.
[0013] The present invention discloses a cast zinc-based alloy composite GBR membrane with a layered structure and having antibacterial and osteogenic properties, comprising an antibacterial unit and an osteogenic unit located on the outer surfaces of both sides, and an internal support unit. The antibacterial unit comprises n layers of zinc-based alloys with different mass percentages of antibacterial elements (copper, silver, cobalt, nickel, aluminum, molybdenum, lanthanum, zirconium, gallium) added, which are marked as 1-1, 1-2...1-n layers from the outside to the inside. The mass percentage of alloying elements in the 1-1, 1-2...1-n layers shows a trend of gradually decreasing, and the mass percentage difference of alloying elements in two adjacent layers is 0.01-9.999%; while the osteogenic unit is composed of m layers of zinc-based alloy materials with different mass percentages of osteogenic elements (lithium, strontium, calcium, phosphorus, magnesium, manganese, silicon, barium, etc.) added, which are marked as 2-1, 2-2...2-m layers from the outside to the inside. The mass percentage of alloying elements in the 2-1, 2-2, ... 2-m layers shows a trend of gradually decreasing, and the mass percentage difference of alloying elements in two adjacent layers is 0.01-9.999%. The middle support unit uses a zinc-based material with a higher corrosion potential than the adjacent 1-n and 2-m layers. The thickness of each single layer in the antibacterial unit and osteogenic unit contained in the membrane is equal.
[0014] The functions of the various components in the layered composite zinc-based alloy antibacterial guided bone tissue regeneration membrane are as follows:
[0015] (1) The antibacterial unit has dual functions. On the one hand, as the GBR membrane degrades as a whole, the corresponding Cu, Ag, Co, Ni, Al, Mo, La, Zr, Ga and other ions are released, providing good antibacterial properties. At the same time, the alloying element content between adjacent monolayers (1-(n-1) and 1-n) in the antibacterial unit differs by 0.01 to 9.999 wt%, resulting in a corrosion potential difference between adjacent layers, which accelerates the degradation process and achieves better uniform degradation layer by layer.
[0016] (2) The osteogenic unit also has a dual function. The antibacterial elements release Li, Sr, Ca, P, Mg, Mn, Si, Ba and other ions during the gradual degradation of the GBR membrane system, promoting the growth of bone tissue. On the other hand, the alloying element content between adjacent monolayers (2-(m-1) and 2-m) in the osteogenic unit varies by 0.01 to 9.999 wt%, and the potential difference between adjacent monolayers achieves uniform degradation.
[0017] (3) The inner support unit is a zinc-based material with a higher corrosion potential than the adjacent 1-n and 2-m layers. This can ensure that the GBR membrane degrades uniformly layer by layer from the outside to the inside, providing sufficient time and space for bone tissue regeneration. In general, the degradation of the membrane system is orderly. In the early stage of degradation, before the growth of bone tissue cells and the healing of surrounding soft tissue wounds, the antibacterial units and osteogenic units located in the outer layer play a role. When the outer antibacterial units and osteogenic units are completely degraded, the support unit continues to play its supporting role; finally, the overall structure is completely degraded within 6 to 12 months after implantation.
[0018] The method for preparing the layered composite zinc-based alloy antibacterial guided bone tissue regeneration membrane as described above is characterized in that it includes the following four steps: 1) direct rolling composite in the cast state; 2) thinning; 3) membrane cutting; 4) laser drilling.
[0019] Furthermore, the specific process of each step includes 1) direct rolling composite in cast state: the billets are kept at 250-350°C for 30-60 min, and 1-3 rolling passes are performed according to the plastic deformation capacity of the zinc alloy, with a single-pass reduction (≥20%), and each rolling pass must be kept at the above temperature for 5-30 min again; 2) thinning: the composite plate obtained in step 1) is air-cooled to room temperature-350°C, and rolled, with a reduction of 5-40% per pass, until the composite plate is rolled to a thickness of ≤0.5 mm; 3) film cutting: using laser cutting technology, the composite plate obtained in step 2) is cut into a shape of 10-100 mm in length and 10-100 mm in width; 4) laser drilling: using laser cutting technology, a conical hole with a diameter range of 10-1000 μm and a width of 10-100 mm is punched on the GBR film obtained in the above step 3).
[0020] Furthermore, the as-cast direct rolling composite comprises the following steps:
[0021] (1a) Surface pretreatment: First, each zinc-based alloy contained in the antibacterial unit, the osteogenic unit and the supporting unit is cut into plates with a length of 10 to 200 mm, a width of 10 to 200 mm and a thickness of 1 to 10 mm, and the alloy plates are homogenized. The heat treatment process is to increase the temperature to 250°C at a rate of 5°C / min, keep the temperature for 2 h, continue to increase the temperature to 350°C at the same rate, keep the temperature for 2 h, and cool with the furnace; after the heat treatment, the surface of the metal plate is polished step by step with 600#, 1000# and 2000# sandpaper to remove the oxide scale and impurities on the metal surface, and then ultrasonically cleaned in acetone, anhydrous ethanol and water respectively, and blown dry with cold air to obtain a clean plate for use;
[0022] (2b) Assembling: Assemble the clean surface of the clean board in step (1a) in the order of antibacterial unit / support unit / osteogenic unit, and fix the four corners of the board with rivets;
[0023] (3c) Rolling bonding: In view of the different plastic deformation capabilities of different zinc alloys, different passes are selected to achieve rolling bonding. For zinc alloy materials with strong plastic deformation capabilities, such as Zn-Mn alloy, a single rolling pass is performed to achieve interlayer interface bonding, the rolling temperature is 250-350°C, and the rolling pass reduction is ≥50%; for zinc alloy materials with poor plastic deformation capabilities, such as Zn-Mg and Zn-Ca alloys, in order to prevent edge cracking and surface cracking, 2-3 rolling passes are performed to achieve metallurgical bonding of the interlayer interface, the rolling temperature is 200-350°C, and the rolling pass reduction is 20-50%.
[0024] The functions of each process in the preparation method are as follows: 1) The direct rolling composite step of the cast state applies downward pressure through the rolling mill to make the layers tightly bonded to achieve the successful composite of the antibacterial unit / support unit / bone-promoting unit. 2) The thinning process gradually reduces the thickness of the composite plate to a thickness of ≤0.5 mm suitable for surgical operation. 3) The cutting membrane is designed to prepare the corresponding shape according to the size and shape of different bone defects. 4) Laser drilling is to achieve the isolation function of the GBR membrane, which can prevent the surrounding soft tissue cells from entering the bone defect area and realize the smooth transportation of nutrients.
[0025] The present invention has the following advantages:
[0026] (1) The layered composite zinc-based alloy antibacterial GBR membrane of the present invention has good antibacterial and osteogenic properties. The antibacterial elements (Cu, Ag, Co, Ni, Al, Mo, La, Zr, Ga) released after implantation show anti-inflammatory, antimicrobial and anti-bacterial proliferation properties, and are widely used in the field of orthopedics. In addition, the released osteogenic elements (Li, Sr, Ca, P, Mg, Mn, Si, Ba ions) can promote bone tissue regeneration and improve the quality and speed of bone regeneration. Therefore, the antibacterial guided bone tissue regeneration membrane prepared by the present invention also exhibits excellent antibacterial properties.
[0027] (2) The layered composite zinc-based alloy antibacterial GBR film of the present invention has the characteristic of better degradation uniformity. The GBR film has the characteristics of gradient distribution of alloying elements, and due to the existence of galvanic corrosion between adjacent single layers, it will achieve more uniform degradation than a single-layer GBR film.
[0028] (3) The layered composite zinc-based alloy GBR membrane of the present invention has good biocompatibility. The overall thickness of the GBR membrane does not exceed 0.5 mm, and the thickness of each single layer in the antibacterial unit and the osteogenic unit is thinner (≤166 μm). The total amount of ions released during the degradation process is less than the maximum safe dose for the human body, ensuring good biocompatibility.
[0029] (4) This layered composite zinc-based alloy antibacterial guided bone tissue regeneration membrane solves the problem of rapid degradation of existing polymer collagen membranes, avoids the need for secondary surgery for inert materials such as titanium membranes, and overcomes the problem of hydrogen generation during the degradation of magnesium alloy barrier membranes.
[0030] (5) Zinc ranks fourth in global metal production and consumption. Its raw material price and the cost of preparing the subsequent GBR membrane are much lower than the cost of the existing GBR membrane in clinical practice, thus reducing production costs and final treatment costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is a schematic diagram of the structure of a layered zinc-based alloy antibacterial guided bone tissue regeneration membrane according to the first embodiment of the present invention;
[0032] Figure 2 for Figure 1 Sectional view along the central axis of the long side;
[0033] Figure 3 The preparation process of the layered zinc-based alloy antibacterial guided bone tissue regeneration membrane according to the second and third embodiments of the present invention;
[0034] Figure 4 This is a schematic diagram of the shape of the regeneration membrane for treating vertical alveolar bone defects according to the present invention;
[0035] Figure 5 A schematic diagram of treating a vertical alveolar bone defect according to the present invention;
[0036] Figure 6 A schematic diagram of the shape of the regeneration membrane for treating horizontal alveolar bone defects according to the present invention;
[0037] Figure 7 Schematic diagram of the present invention for treating horizontal alveolar bone defects. Specific implementation methods
[0039] The present invention is described in more detail below, with examples and drawings for illustration. However, it should be clearly pointed out that the embodiments of the present invention are only used to explain the present invention and are not used to limit the present invention. The present invention provides a layered composite zinc-based alloy antibacterial guided bone tissue regeneration membrane, which can be used after guided bone regeneration surgery and has antibacterial and bone regeneration-promoting properties. The percentages used in the following examples are all mass percentages unless otherwise specified.
[0040] Example 1: A layered composite zinc-based alloy antibacterial guided bone tissue regeneration membrane
[0041] This embodiment provides a layered composite zinc-based alloy antibacterial guided bone tissue regeneration membrane: Zn-3Cu / Zn-2Cu / Zn / Zn-0.2Sr / Zn-0.4Sr, namely, Example 1 in Table 1-1, hereinafter referred to as ZCS five-layer membrane. The three-dimensional shape and cross-sectional structure along the long side central axis of the ZCS five-layer membrane are shown in FIG. Figure 1 , 2 As shown in the figure, the ZCS five-layer membrane is composed of antibacterial units (single layers 1-1 and 1-2) and osteogenic units (single layers 2-1 and 2-2) on both sides and an inner support unit. Among them, 1-1 and 1-2 layers are zinc-copper alloy layers with a Cu mass percentage of 3% and 2%, respectively. 2-1 and 2-2 layers are zinc-strontium alloy layers with a Sr mass percentage of 0.4% and 0.2%, respectively. Among them, the thickness of single layers 1-1, 1-2, 2-1, 2-2 and the support unit layer is consistent, which is 0.02 mm. It is a rectangular shape with a side length of 30×20 mm. There are 1 base hole with a pore size of 4 mm for the dental implant base and 2 permeation holes for the transportation of nutrients on the ZCS five-layer membrane. The small pore size is a structure with one end wide and the other end narrow. The pore size on the side close to the bone tissue is as small as 10 μm, which plays an isolation role; the pore size on the side close to the soft tissue is as large as 800 μm, which is conducive to the transportation of nutrients. The obtained recycled film can be cut at any angle.
[0042] The above five-layer structure (see Figure 1 and Figure 2 ) is also applicable to other five-layer zinc-based GBR films, including but not limited to the following types, see Invention Example 2 in Table 1-1. Further, the above structure can be expanded to other layered structures, specifically as follows:
[0043] (1) In the structure of the five-layer ZCS membrane (see Figure 2 ), the antibacterial unit is 2 layers (i.e. Zn-3Cu / Zn-2Cu), the osteogenic unit is also 2 layers (i.e. Zn-0.4Sr / Zn-0.2Sr), and the supporting unit is 1 layer (i.e. pure Zn);
[0044] (2) In the three-layer membrane (see Figure 1 ), for example, in Inventive Example 3 in Table 1-1, the antibacterial unit is 1 layer (i.e., Zn-2Cu), the osteogenic unit is also 1 layer (i.e., Zn-0.4Sr-0.1Ca), and the supporting unit is 1 layer (i.e., Zn-0.8Li);
[0045] (3) In the four-layer membrane (see Figure 1), for example, in Inventive Example 5 in Table 1-1, the antibacterial unit is 2 layers (i.e., Zn-2Ag / Zn-1Ag), the osteogenic unit is 1 layer (i.e., Zn-1Mg-0.8Mn), and the supporting unit is 1 layer (i.e., Zn-0.1Ca);
[0046] (4) According to the above design concepts and specific examples, those skilled in the art can also design a zinc-based GBR film with more than 6 layers based on this embodiment.
[0047] Table 1-1
[0048]
[0049] Example 2: Three-pass rolling composite multilayer zinc-based GBR film
[0050] This embodiment provides a preparation method, that is, preparing a five-layer zinc-based alloy composite antibacterial guided bone tissue regeneration membrane: Zn-3Cu / Zn-2Cu / Zn / Zn-0.2Sr / Zn-0.4Sr, hereinafter referred to as ZCS five-layer membrane.
[0051] 1. Cast direct rolling composite
[0052] (1a) Surface pretreatment. To facilitate the test, the cast Zn-3Cu, Zn-2Cu, Zn-0.2Sr, Zn-0.4Sr, and pure Zn were first cut into 100×20×2 mm plates using a wire cutting machine. The above alloy plates were homogenized and the heat treatment process was as follows: heating to 250°C at a rate of 5°C / min and keeping the temperature for 2 hours, then heating to 350°C at the same rate and keeping the temperature for 2 hours, and then cooling with the furnace. After heat treatment, the surface of the metal plate will oxidize. Sandpaper (600#, 1000#, 2000#) was used to polish the plate step by step to remove the oxide scale and impurities on the metal surface. Then, the plate was ultrasonically cleaned in acetone, anhydrous ethanol and water for 10 min each, and dried with cold air for use.
[0053] (1b) Blanket assembly. In view of the requirements for the interface of rolling composite, during blank assembly, the clean surfaces of the surface-treated zinc-based alloy are first bonded together to form the above-mentioned Zn-3Cu / Zn-2Cu / Zn / Zn-0.2Sr / Zn-0.4Sr combination, which is then fixed at the four corners of the overall structure with rivets.
[0054] (1c) Rolling composite. Before rolling, the composite blank with a thickness of 10 mm was placed at a temperature of 320 ° C for 1 h, and then three rolling passes were performed. It was necessary to re-keep at 320 ° C for 5 min between each pass. The reduction of a single pass was 30%, and a composite plate with a thickness of 3.43 mm was obtained, which was then air-cooled to room temperature.
[0055] 2) Thinning
[0056] Then the composite billet was rolled 30 times, with a single-pass reduction of 0.1 mm, so that a zinc alloy composite plate with a thickness of 0.43 mm was finally obtained after rolling.
[0057] 3) Film cutting: The five-layer ZCS film obtained by the above process is laser cut to form a series of products with shapes such as 15×20 mm, 20×30 mm, and 30×40 mm.
[0058] 4) Laser drilling
[0059] Laser drilling was performed on a series of products obtained through the above process. The small aperture shape was a structure with one end wide and the other end narrow. The aperture on the side close to the soft tissue was 1000 μm; the aperture on the side close to the bone tissue was 10 μm.
[0060] Example 3: Single-pass rolling composite three-layer zinc-based GBR film
[0061] This embodiment provides a preparation method, that is, preparing a three-layer composite zinc-based GBR film: Zn-1Cu / Zn / Zn-0.2Mn, see Invention Example 4 in Table 1-1.
[0062] 1) Cast direct rolling composite
[0063] (1a) Surface pretreatment. First, a wire cutting machine was used to cut 50×20×5 mm plates from the ingots of Zn-0.2Mn, Zn-1Cu and pure Zn. The above zinc plates were subjected to homogenization heat treatment: the temperature was raised to 250°C at a rate of 5°C / min and kept at this temperature for 2 hours, then the temperature was raised to 350°C at the same rate and kept at this temperature for 2 hours, and then cooled with the furnace. After the above heat treatment, the surface of the metal plate was oxidized. The surface of the plate was polished step by step with sandpaper (600#, 1000#, 2000#) to remove the surface oxide scale, and then ultrasonically cleaned in acetone, anhydrous ethanol and water for 10 min each, and dried with cold air for use.
[0064] (1b) Assembly. First, the surface-pretreated zinc-based alloys were bonded together in the order of Zn-1Cu / Zn / Zn-0.2Mn with clean surfaces to form a composite slab with a thickness of 15 mm, and the composite slab was fixed at the four corners with aluminum rivets.
[0065] (1c) Rolling cladding. The composite slab was kept at 320°C for 1 h before rolling, and then single-pass rolling cladding was performed with a reduction of 70% to obtain a 4.5 mm thick composite plate, which was then quenched in water to room temperature. At this time, the interlayer interface of the composite plate achieved metallurgical bonding. Scanning electron microscopy (SEM) / EDS characterization showed that there was a 20 μm alloy element diffusion layer at the interface.
[0066] 2) Thinning
[0067] Then, the layered composite plate obtained above was rolled 20 times, with a single-pass reduction of 0.2 mm, so that a zinc alloy composite plate with a thickness of 0.5 mm was finally obtained after rolling.
[0068] 3) Membrane cutting. The Zn-1Cu / Zn / Zn-0.2Mn layered zinc-based alloy antibacterial guided bone tissue regeneration membrane obtained by the above process is laser cut to form a series of products with shapes of 15×20 mm, 20×30 mm, 30×40 mm, etc.
[0069] 4) Laser drilling
[0070] Laser drilling was performed on a series of products obtained through the above process. The small aperture shape was a structure with one end wide and the other end narrow. The aperture on the side close to the soft tissue was 500 μm; the aperture on the side close to the bone tissue was 10 μm.
[0071] Example 4: For treating vertical alveolar bone defects
[0072] When the height of the alveolar ridge is not reduced much, but the bone around the root is absorbed more, and the alveolar bone is defected vertically or at a certain angle to the root surface, it is a typical vertical alveolar bone defect. For vertical alveolar bone defects, the vertical alveolar bone regeneration membrane ( Figure 4 ) is enough.
[0073] like Figure 5 As shown in the figure, the goal is to reconstruct the bone defect. In the specific operation, the lesion site is first cleaned; then a mixture of autologous blood and bone replacement particles is placed at the defect site to fill the defect; a vertical alveolar bone regeneration membrane ( Figure 4 ) as a covering and isolating biomaterial. The base passes through the 1 base hole at one end of the GBR membrane, and the 3 main part of the membrane is bent and anastomosed according to the shape of the tissue after filling, and fixed with 4 fixing wings located on the side of the GBR membrane; finally, the flap is closed by the suturing technology of the flap.
[0074] Example 5: For treating horizontal alveolar bone defects
[0075] like Figure 7 As shown in the figure, when the alveolar bone top between the alveolar, labial or lingual sides is horizontally absorbed and the height of the alveolar ridge is reduced, a horizontal alveolar bone defect occurs, which is also the most common form of bone defect. At this time, guided bone regeneration surgery is required. For horizontal alveolar bone defects, horizontal alveolar bone regeneration membrane ( Figure 6 ) is enough.
[0076] In the specific operation, the lesion site is first cleaned; the bone defect is also filled with a mixture of autologous blood and bone replacement particles; then the horizontal alveolar bone regeneration membrane ( Figure 4 ) coverage; the 1 base hole in the center of the GBR membrane is used to fix the denture base, the 3 membrane main body on the GBR covers the top of the alveolar ridge, and the other part is bent to cover the bone defect on the labial and lingual sides, and finally the 4 fixing wings on the side are used to stabilize the GBR membrane; closure is achieved by suturing the skin flap.
[0077] Example 6: Antibacterial and osteogenic properties of the ZCS five-layer membrane (i.e., Invention Example 1 in Table 1-1)
[0078] This example further illustrates that the ZCS five-layer membrane prepared in Example 2 of the present invention has good antibacterial and osteogenic properties. The ZCS five-layer membrane was used as a test example, and the GBR membrane prepared with pure Zn (hereinafter referred to as pure Zn membrane) was used as a comparative example to conduct corresponding tests.
[0079] 1. Antibacterial test:
[0080] The inhibitory effect of the above GBR membrane on Staphylococcus aureus was evaluated by agar diffusion plate test to evaluate its antibacterial properties. Staphylococcus aureus was placed in 5 mL of culture medium and activated in a constant temperature oscillator for 24 hours, and then the bacterial solution was diluted to a concentration of 1×10 8 CFU / mL. Dissolve Luria-Bertani (LB) broth powder (10 g / L peptone, 5 g / L yeast extract powder, 10 g / L sodium chloride) in 950 mL distilled water, adjust the pH to 7.0-7.2 with 0.1 mol / L NaOH solution, and finally dilute to 1 L with distilled water. Add agar powder (1.5 g / 100 ml) to the above culture medium to obtain a solid culture medium solution. Then the above solid and liquid culture media and experimental samples were sterilized in an autoclave for 30 minutes. When the temperature cooled to 45°C, pour 20 mL of the culture medium solution into the culture dish and sterilize it with ultraviolet light for 30 minutes to obtain an agar culture medium plate. Use a pipette to evenly spread 500 μL of bacterial suspension on the surface of the agar culture medium, and place a 10 mm disc-shaped sample: ZCS five-layer film and pure Zn in the center of the plate. The experiment set up three sets of parallel samples, and the IZD value was determined after incubation at 37°C for 24 hours, and the antibacterial performance was calculated:
[0081] H=(Dd) / 2
[0082] Where H (unit: mm) represents the inhibition zone, D (unit: mm) represents the inhibition zone diameter, and d (unit: mm) represents the sample diameter. When H is greater than or equal to 1 mm, the antibacterial effect is excellent; when H is equal to 0 mm and the number of surrounding proliferating bacteria is large, there is no antibacterial effect.
[0083] The experimental results are as follows: ZCS (H = 3 ± 0.2) ≥ Zn (H = 0 ± 0.2), which indicates that the antibacterial activity of the ZCS five-layer film is significantly higher than that of the pure Zn film.
[0084] 2. In vitro osteogenesis experiment:
[0085] 0.5 mL of a 2×10 4 Mouse embryonic osteoblast precursor cells (MC3T3-E1) were seeded in 24-well plates at a concentration of 100 μg / mL and cultured in a cell culture incubator (37°C, 5% CO2, saturated humidity) until the bottom of the culture medium was covered. ZCS five-layer membrane and pure Zn membrane extract (diluted to 50% concentration) were added for co-culture. After 7 days of induction of differentiation, the ALP activity of MC3T3-E1 cells at this time was quantitatively analyzed using an ALP kit. The experimental results showed that the ALP activity value of MC3T3-E1 cells co-cultured with the ZCS five-layer membrane extract was 20% higher than that of the pure zinc group, indicating that the osteogenic effect of the ZCS five-layer membrane is higher than that of the pure Zn membrane.
[0086] In summary, the ZCS five-layer membrane prepared in Example 2 of the present invention has excellent comprehensive antibacterial and osteogenesis properties, which meets the performance requirements of guided bone regeneration membranes.
[0087] Example 7: Degradation uniformity of Zn-2Cu / Zn-0.8Li / Zn-0.4Sr-0.1Ca (hereinafter referred to as ZCLS) three-layer film
[0088] This example is to illustrate that the ZCLS three-layer membrane proposed in Invention Example 3 in Table 1-1 has good degradation uniformity. The ZCLS three-layer membrane is used as a test example, and the GBR membrane prepared by Zn-2Cu (hereinafter referred to as ZC membrane) is used as a comparative example to conduct an immersion experiment. According to the ASTM-G31-72 standard, the above ZCLS three-layer membrane and ZC membrane are immersed in a simulated body fluid (SBF) solution, and the ratio of SBF solution to sample surface area is 20 mL / cm 2 The SBF solution was changed every 2 days. After immersion in SBF at 37°C for 30 days, the corrosion products of the two groups of samples were removed and the corrosion morphology was observed by SEM.
[0089] The experimental results show that obvious corrosion pits were observed on the surface of the ZC membrane, and they penetrated the entire membrane along the thickness direction of the membrane. On the surface of the ZCLS three-layer membrane, degradation was observed only in the outermost antibacterial unit Zn-2Cu layer and the osteogenic unit Zn-0.4Sr-0.1Ca layer. The corrosion pits expanded laterally in the above layers and did not penetrate the supporting unit Zn-0.8Li layer along the thickness direction of the membrane. No obvious corrosion pits were formed in the supporting unit Zn-0.8Li layer, which indicates that the ZCLS three-layer membrane has better degradation uniformity than the single-layer ZC membrane.
Claims
1. A layered composite zinc-based alloy antibacterial guided bone tissue regeneration membrane, characterized in that: The structure of the regeneration membrane is as follows: the side in contact with the oral periodontal soft tissue serves as an antibacterial unit, which is a zinc-based material layer with antibacterial properties of a certain thickness of n layers (1≤n≤5), and each layer is specifically marked as 1-n, and the smaller n is, the closer it is to the soft tissue side; the side in contact with the bone defect site serves as an osteogenic unit, which is a zinc-based material layer with osteogenic properties of a certain thickness of m layers (1≤m≤5), and each layer is specifically marked as 2-m, and the smaller m is, the closer it is to the bone defect side; between the antibacterial unit and the osteogenic unit is a zinc-based material core layer of a certain thickness as a supporting unit; the GBR membrane is repeatedly bent ≥80 times without delamination.
2. The regenerated membrane according to claim 1, characterized in that: The zinc-based material is pure zinc or a zinc alloy, and the mass percentage of a single alloying element in the zinc alloy is 0.001-10%.
3. The regenerated membrane according to claim 1, characterized in that: The alloying elements in the antibacterial unit include one or more of copper, silver, cobalt, nickel, aluminum, molybdenum, lanthanum, zirconium, and gallium; the alloying elements in the osteogenic unit include one or more of lithium, strontium, calcium, phosphorus, magnesium, manganese, silicon, and barium; the supporting unit is a zinc-based material with a higher corrosion potential than the adjacent 1-n and 2-m layers.
4. The regenerated membrane according to claim 1, characterized in that: In the n-layer zinc-based material included in the antibacterial unit, the content of alloying elements decreases gradually from 1-1 to 1-n, and the mass percentage of alloying elements between adjacent single layers differs by 0.1 to 9.999%; in the m-layer zinc-based material included in the osteogenic unit, the content of alloying elements decreases gradually from 2-1 to 2-m, and the mass percentage of alloying elements between adjacent single layers differs by 0.1 to 9.999%.
5. The regenerated film according to claim 1, characterized in that The thickness of the regenerated film does not exceed 0.5 mm.
6. The regenerated film according to claim 1, characterized in that The regeneration membrane has conical holes with diameters ranging from 10 to 1000 μm. The hole diameter is larger on the side close to the soft tissue to ensure the entry of nutrients; the hole diameter is smaller on the side close to the bone defect to prevent the soft tissue from growing into and occupying the bone defect space; the porosity is 5 to 90%.
7. The method for preparing a regenerated membrane according to claim 1, characterized in that: The method comprises the following four steps: 1) direct rolling and compounding of the cast state; 2) thinning; 3) film cutting; and 4) laser drilling.
8. The method for preparing a regenerated membrane according to claim 7, characterized in that: The specific preparation process includes: 1) Cast direct rolling composite: keep the billets at 250-350℃ for 30-60 min, and carry out 1-3 passes of rolling according to the plastic deformation capacity of the zinc alloy, with a single pass reduction of ≥20%, and keep them at the above temperature for 5-30 min for each rolling pass; 2) Thinning: According to the thickness requirement of the final product, the composite plate obtained in step 1) is subjected to multiple rolling passes, the rolling temperature is room temperature to 350°C, and the rolling reduction is 5 to 40% until the thickness of the composite plate is ≤0.5 mm; 3) Film cutting: using laser cutting technology, the composite film obtained in step 2) is cut into a shape of 10 to 100 mm in length and 10 to 100 mm in width; 4) Laser drilling: using laser cutting technology, a conical hole with a diameter ranging from 10 to 1000 μm is punched on the GBR membrane obtained in step 3) above, which is wider on the antibacterial unit side and narrower on the osteogenic unit side.
9. The method for preparing a regenerated membrane according to claim 7 or 8, characterized in that: The as-cast direct rolling composite process comprises the following steps: (1a) Surface pretreatment: First, each zinc-based alloy contained in the antibacterial unit, the osteogenic unit and the supporting unit is cut into plates with a length of 10 to 200 mm, a width of 10 to 200 mm and a thickness of 1 to 10 mm, and the alloy plates are homogenized. The heat treatment process is to increase the temperature to 250°C at a rate of 5°C / min, keep the temperature for 2 h, continue to increase the temperature to 350°C at the same rate, keep the temperature for 2 h, and cool with the furnace; after the heat treatment, the surface of the metal plate is polished step by step with 600#, 1000# and 2000# sandpaper to remove the oxide scale and impurities on the metal surface, and then ultrasonically cleaned in acetone, anhydrous ethanol and water respectively, and blown dry with cold air to obtain a clean plate for use; (1b) Assembling: Assemble the clean surface of the clean board in step (1a) in the order of antibacterial unit / support unit / osteogenic unit, and fix the four corners of the board with rivets; (1c) Rolling bonding: In view of the different plastic deformation capabilities of different zinc alloys, different passes are selected to achieve rolling bonding; for zinc alloy materials with strong plastic deformation capabilities, a single rolling pass is performed to achieve interlayer interface bonding, the rolling temperature is 250-350°C, and the rolling pass reduction is ≥50%; for zinc alloy materials with poor plastic deformation capabilities, in order to prevent edge cracking and surface cracking, 2-3 rolling passes are performed to achieve metallurgical bonding at the interlayer interface, the rolling temperature is 200-350°C, and the rolling pass reduction is 20-50%.