A TPU fiber membrane for removing bisphenols from water and preparation method thereof
By using electrospinning method and a specific solvent combination in TPU fiber membranes, combined with functional modifiers, the problem of low adsorption efficiency of existing polymer membrane materials when removing bisphenols in water is solved, and high efficiency and economicality are achieved Bisphenol A removal effect.
Patent Information
- Application Number
- CN202411320113.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-23
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-23
AI Technical Summary
The adsorption efficiency of existing polymer film materials is not high when removing bisphenols from water, the preparation process is complex and costly, and the adsorption efficiency of bisphenols still needs to be improved.
The TPU fiber membrane was prepared by electrospinning method, and pore-generating using a mixed solvent of ethanol and nonafluoroisobutyl methyl ether was used to form pores. Combined with 2-aminoterephthalic acid-modified β-cyclodextrin and chitosan loading, using a gradient The heating program and vacuum suction filtration technology optimize the physical and chemical properties of membrane materials to improve adsorption performance.
The efficient removal rate of bisphenol A (≥99.5%) and short-term adsorption (≤30min) are achieved, the preparation process is simplified, the cost is reduced, and efficient, economical and environmentally friendly solutions are provided for drinking water purification.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the field of polymer fiber membrane preparation, in particular to a TPU fiber membrane for removing bisphenol substances in water and a preparation method thereof. Background Art
[0002] Bisphenol compounds, especially endocrine disruptors represented by bisphenol A (BPA), have become the focus of global environmental pollution. Bisphenol endocrine disruptors can simulate or block the normal effects of hormones, interfere with the endocrine system of organisms, and cause a series of ecological and health problems such as reproductive disorders, decreased immune function, and abnormal development of the nervous system. At present, bisphenol endocrine disruptors enter the natural water environment through various channels such as industrial production and daily life emissions, and are even enriched in drinking water used in daily life.
[0003] In order to remove bisphenol endocrine disruptors in daily drinking water, various polymer membrane materials have been developed in the prior art for adsorption and removal of bisphenol substances in water. However, although the current polymer membrane materials have their own characteristics, they also have certain limitations.
[0004] Cellulose-based membrane: It has the advantages of abundant raw materials, renewability and good biocompatibility, but its chemical resistance is poor and it is easy to lose stability in complex water environments, affecting the adsorption effect.
[0005] Synthetic polymer membranes: such as polysulfone and PVDF (polyvinylidene fluoride), have high mechanical strength and chemical stability, and can overcome the defects of cellulose-based membranes to a certain extent. However, these materials often involve complex chemical reactions in the preparation process, are costly, and the adsorption efficiency of bisphenols still needs to be improved.
[0006] Functional polymer membrane: By introducing specific functional groups into the membrane material, such as ion exchange groups, affinity groups, etc., the adsorption performance of bisphenols can be significantly improved. However, the preparation process of such materials is complicated, and the introduction of functional groups may affect the overall performance of the membrane material, such as mechanical strength and chemical stability.
[0007] Therefore, in view of the problems existing in the prior art, it is urgent to develop a polymer membrane material and a preparation method thereof having a high adsorption removal rate and good adsorption efficiency for bisphenol endocrine disruptors. Summary of the invention
[0008] In view of the defects of the above-mentioned prior art, an object of the present invention is to provide a TPU fiber membrane for removing bisphenols from water and a preparation method thereof. Based on its unique physical and chemical properties, the TPU fiber membrane material aims to solve the technical problems of insufficient adsorption removal rate and poor adsorption efficiency of bisphenols by the existing polymer membranes that adsorb bisphenols in water through optimized preparation process and functional modification. At the same time, the present invention is also committed to simplifying the preparation process, reducing costs, and providing an efficient, economical and environmentally friendly solution for the field of drinking water purification.
[0009] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0010] A method for preparing a TPU fiber membrane for removing bisphenols from water, wherein the TPU fiber membrane specifically comprises the following preparation steps:
[0011] S1, dissolving TPU in a mixed solvent of ethanol and nonafluoroisobutyl methyl ether, stirring at room temperature for a certain period of time until uniform to obtain a TPU solution, preparing a TPU film by an electrospinning method, and then drying the solvent by a gradient heating program to obtain a TPU porous fiber membrane;
[0012] S2, using 2-aminoterephthalic acid to modify β-cyclodextrin and chitosan respectively to obtain amino-modified β-cyclodextrin and amino-modified chitosan;
[0013] S3, filtering the mixed dispersion of amino-modified β-cyclodextrin and amino-modified chitosan to the TPU porous fiber membrane in step S1 by suction filtration, and drying to obtain the TPU fiber membrane for removing bisphenols in water.
[0014] Preferably, the volume ratio of ethanol and nonafluoroisobutyl methyl ether in the mixed solvent of step S1 is (2-3): 1;
[0015] Preferably, the mass concentration of the TPU in the mixed solvent is 15-25wt%;
[0016] Preferably, the stirring time is 12-24h;
[0017] Preferably, the electrospinning method comprises the following specific steps: electrospinning is performed using an electrospinning device, the TPU solution is first injected into a plastic syringe, and the spinning conditions are: voltage 15 kV, injection speed 0.5 mL / h-1 mL / h, receiving distance 10 cm-20 cm, continuous spinning for 1-3 h, that is, a TPU film is obtained on a collecting roller;
[0018] Preferably, the gradient temperature rising program is to maintain at 60-70°C for 0.5-3h, and then maintain at 80-90°C for 0.5-3h. More preferably, the gradient temperature rising program is to dry at 60°C for 1h, and then dry at 80°C for 1h.
[0019] Preferably, the method for modifying β-cyclodextrin with 2-aminoterephthalic acid in step S2 is: adding 2-aminoterephthalic acid to an organic solvent containing β-cyclodextrin, adding a certain amount of dehydrating agent, stirring evenly, reacting at 35-45° C. for 12-24 hours, and then centrifugally filtering, washing with water and drying to obtain amino-modified β-cyclodextrin;
[0020] Preferably, the method for modifying chitosan with 2-aminoterephthalic acid is: adding 2-aminoterephthalic acid to an organic solvent containing chitosan, adding a certain amount of dehydrating agent, stirring evenly, reacting at 35-45° C. for 12-24 hours, then centrifugally filtering, washing with water and drying to obtain amino-modified chitosan;
[0021] Preferably, the organic solvent is selected from dimethylformamide, dimethyl sulfoxide or dichloromethane;
[0022] Preferably, the dehydrating agent is selected from DDC or EDC·HCl;
[0023] Preferably, the mass ratio of 2-aminoterephthalic acid to β-cyclodextrin or chitosan is 1:(3-5);
[0024] Preferably, the mass concentration of the organic solvent containing β-cyclodextrin or the organic solvent containing chitosan is 15-25%;
[0025] Preferably, the mass ratio of the dehydrating agent to 2-aminoterephthalic acid is 10%.
[0026] Preferably, the amino-modified β-cyclodextrin and amino-modified chitosan mixed dispersion in step S3 is obtained by adding the amino-modified β-cyclodextrin and amino-modified chitosan obtained in step S2 to tetrahydrofuran;
[0027] Preferably, the mass ratio of the amino-modified β-cyclodextrin to the amino-modified chitosan is (2-3): 1;
[0028] Preferably, the total mass of the amino-modified β-cyclodextrin and the amino-modified chitosan is 15-25% of the mass of the TPU porous fiber membrane;
[0029] Preferably, the filtration is vacuum filtration;
[0030] Preferably, the drying is carried out at 50-60° C. for 8-12 hours.
[0031] The second object of the present invention is to provide a TPU fiber membrane for removing bisphenols in water, which is prepared by the above-mentioned preparation method.
[0032] The TPU fiber membrane for removing bisphenols from water has an adsorption removal rate of 99.5% or more for bisphenols, and a shortest adsorption time of 30 minutes or less.
[0033] The third object of the present invention is to provide an application of a TPU fiber membrane prepared by the aforementioned method for preparing a TPU fiber membrane for removing bisphenols from water, wherein the application is to remove bisphenols from water.
[0034] Compared with the prior art, the present invention has the following advantages:
[0035] (1) The present invention creatively adopts a mixed solvent of ethanol and nonafluoroisobutyl methyl ether in a specific ratio as a porogen of the TPU fiber membrane in the preparation step of the TPU porous fiber membrane in the method for preparing the TPU fiber membrane for removing bisphenols in water, and adopts a gradient temperature rising program to dry the solvent. By utilizing the difference in boiling points and volatility of the two solvents, the two solvents play a synergistic role, so that the finally obtained TPU fiber membrane has an excellent adsorption effect on bisphenols.
[0036] (2) The present invention creatively adopts a specific ratio of 2-aminoterephthalic acid-modified β-cyclodextrin and chitosan to load on the TPU fiber membrane. Through the different adsorption effects of the two on bisphenols, and the different loading levels of the two on the surface of the previously obtained TPU porous fiber membrane, the special structure of the TPU porous fiber membrane is used to synergize the effect, so that the finally obtained TPU fiber membrane has excellent adsorption effect on bisphenols.
[0037] (3) The present invention creatively selects 2-aminoterephthalic acid to perform surface treatment on β-cyclodextrin or chitosan, and utilizes the active end group and aromatic structure of 2-aminoterephthalic acid to achieve better adsorption of bisphenols.
[0038] (4) The TPU fiber membrane for removing bisphenols from water obtained by the present invention can achieve an excellent bisphenol A adsorption removal rate (≥99.5%) and a high adsorption efficiency (shortest adsorption time ≤30 min). Among them, the TPU fiber membrane of Example 1 has the best performance and can achieve a bisphenol A adsorption removal rate of 99.9% in 20 min. DETAILED DESCRIPTION
[0039] The raw materials and equipment used in the present invention, unless otherwise specified, are all commonly used raw materials and equipment in the art; the methods used in the present invention, unless otherwise specified, are all conventional methods in the art.
[0040] Unless otherwise specified, the meanings of the terms in this specification are the same as those generally understood by those skilled in the art. However, if there is any conflict, the definitions in this specification shall prevail.
[0041] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.
[0042] The raw materials are selected as follows:
[0043] TPU: BASF, Konz 208 / F;
[0044] β-Cyclodextrin: Shanghai Aladdin Biochemical Technology Co., Ltd., C104384;
[0045] Chitosan: Shanghai Aladdin Biochemical Technology Co., Ltd., C434547.
[0046] Amino-modified β-cyclodextrin:
[0047] Preparation Example 1a
[0048] 2-aminoterephthalic acid was added to dimethylformamide containing β-cyclodextrin at a mass concentration of 15%, and a certain amount of DDC was added. After stirring evenly, the mixture was reacted at 45°C for 12 hours, and then centrifuged, filtered, washed with water, and dried to obtain amino-modified β-cyclodextrin, referred to as N-β-CDs1.
[0049] The mass ratio of 2-aminoterephthalic acid to β-cyclodextrin is 1:3; and the mass ratio of the dehydrating agent to 2-aminoterephthalic acid is 10%.
[0050] Preparation Example 2a
[0051] 2-aminoterephthalic acid was added to dimethylformamide containing β-cyclodextrin at a mass concentration of 15%, and a certain amount of DDC was added. After stirring evenly, the mixture was reacted at 45°C for 12 hours, and then centrifuged, filtered, washed with water, and dried to obtain amino-modified β-cyclodextrin, referred to as N-β-CDs2.
[0052] The mass ratio of 2-aminoterephthalic acid to β-cyclodextrin is 1:5; and the mass ratio of the dehydrating agent to 2-aminoterephthalic acid is 10%.
[0053] Comparative Preparation Example 1a
[0054] 2-aminoterephthalic acid was added to dimethylformamide containing β-cyclodextrin at a mass concentration of 15%, and a certain amount of DDC was added. After stirring evenly, the mixture was reacted at 45°C for 12 hours, and then centrifuged, filtered, washed with water, and dried to obtain amino-modified β-cyclodextrin, referred to as N-β-CDs-c1.
[0055] The mass ratio of 2-aminoterephthalic acid to β-cyclodextrin is 1:2; and the mass ratio of the dehydrating agent to 2-aminoterephthalic acid is 10%.
[0056] Comparative Preparation Example 2a
[0057] 2-aminopropionic acid was added to dimethylformamide containing β-cyclodextrin at a mass concentration of 15%, and a certain amount of DDC was added. After stirring evenly, the mixture was reacted at 45°C for 12 hours, and then centrifuged, filtered, washed with water, and dried to obtain amino-modified β-cyclodextrin, referred to as N-β-CDs-c2.
[0058] The mass ratio of 2-aminopropionic acid to β-cyclodextrin is 1:3; and the mass ratio of the dehydrating agent to 2-aminoterephthalic acid is 10%.
[0059] Amino-modified chitosan:
[0060] Preparation Example 1b
[0061] 2-aminoterephthalic acid was added to dimethylformamide containing chitosan at a mass concentration of 15%, and a certain amount of DDC was added. After stirring evenly, the mixture was reacted at 45°C for 12 hours, and then centrifuged, filtered, washed and dried to obtain amino-modified chitosan, referred to as N-K1.
[0062] The mass ratio of 2-aminoterephthalic acid to chitosan is 1:3; and the mass ratio of DDC to 2-aminoterephthalic acid is 10%.
[0063] Preparation Example 2b
[0064] 2-aminoterephthalic acid was added to dimethylformamide containing chitosan with a mass concentration of 15%, and a certain amount of DDC was added. After stirring evenly, the mixture was reacted at 45°C for 12 hours, and then centrifuged, filtered, washed and dried to obtain amino-modified chitosan, referred to as N-K2.
[0065] The mass ratio of 2-aminoterephthalic acid to chitosan is 1:5; and the mass ratio of DDC to 2-aminoterephthalic acid is 10%.
[0066] Comparative Preparation Example 1b
[0067] 2-aminoterephthalic acid was added to dimethylformamide containing chitosan with a mass concentration of 15%, and a certain amount of DDC was added. After stirring evenly, the mixture was reacted at 45°C for 12 hours, and then centrifuged, filtered, washed and dried to obtain amino-modified chitosan, referred to as NK-c1.
[0068] The mass ratio of 2-aminoterephthalic acid to chitosan is 1:2; and the mass ratio of DDC to 2-aminoterephthalic acid is 10%.
[0069] Comparative Preparation Example 2b
[0070] 2-aminopropionic acid was added to dimethylformamide containing chitosan at a mass concentration of 15%, and a certain amount of DDC was added. After stirring evenly, the mixture was reacted at 45°C for 12 hours, and then centrifuged, filtered, washed and dried to obtain amino-modified β-cyclodextrin, referred to as NK-c2.
[0071] The mass ratio of 2-aminopropionic acid to chitosan is 1:3; the mass ratio of DDC to 2-aminoterephthalic acid is 10%.
[0072] Example 1
[0073] A TPU fiber membrane for removing bisphenols in water, wherein the TPU fiber membrane is obtained by the following preparation method, which specifically comprises the following preparation steps:
[0074] S1, TPU was dissolved in a mixed solvent of ethanol and nonafluoroisobutyl methyl ether in a volume ratio of 2:1, the mass concentration of TPU in the mixed solvent was configured to be 20wt%, and the TPU solution was obtained after stirring at room temperature for 18h until it was uniform, and the TPU porous fiber membrane was prepared by electrospinning;
[0075] The electrospinning method comprises the following specific steps: electrospinning is performed using an electrospinning device, firstly a TPU solution is injected into a plastic syringe, and the spinning conditions are: voltage 15 kV, injection speed 0.8 mL / h, receiving distance 10 cm, and continuous spinning for 3 h, so that a TPU film is obtained on a collecting roller, and then the TPU film is dried at 60° C. for 1 h and then at 80° C. for 1 h, so that the solvent is fully volatilized, and thus a TPU porous fiber film is obtained;
[0076] S2, prepare N-β-CDs1 and N-K1, and set aside;
[0077] S3. The mixed dispersion of N-β-CDs1 and N-K1 was filtered to the TPU porous fiber membrane in step S1 by vacuum filtration, and dried at 60° C. for 12 h to obtain the TPU fiber membrane for removing bisphenols in water.
[0078] The N-β-CDs1 and N-K1 mixed dispersion is obtained by adding N-β-CDs1 and N-K1 into tetrahydrofuran;
[0079] The mass ratio of N-β-CDs1 to N-K1 in the N-β-CDs1 and N-K1 mixed dispersion is 2:1;
[0080] The total mass of the N-β-CDs1 and N-K1 is 20% of the mass of the TPU porous fiber membrane.
[0081] Example 2
[0082] A TPU fiber membrane for removing bisphenols in water, wherein the TPU fiber membrane is obtained by the following preparation method, which specifically comprises the following preparation steps:
[0083] S1, TPU was dissolved in a mixed solvent of ethanol and nonafluoroisobutyl methyl ether in a volume ratio of 3:1, the mass concentration of TPU in the mixed solvent was configured to be 20wt%, and the TPU solution was obtained after stirring at room temperature for 18h until it was uniform, and the TPU porous fiber membrane was prepared by electrospinning;
[0084] The electrospinning method comprises the following specific steps: electrospinning is performed using an electrospinning device, firstly a TPU solution is injected into a plastic syringe, and the spinning conditions are: voltage 15 kV, injection speed 0.8 mL / h, receiving distance 10 cm, and continuous spinning for 3 h, so that a TPU film is obtained on a collecting roller, and then the TPU film is dried at 60° C. for 1 h and then at 80° C. for 1 h, so that the solvent is fully volatilized, and thus a TPU porous fiber film is obtained;
[0085] S2, prepare N-β-CDs1 and N-K1, and set aside;
[0086] S3. The mixed dispersion of N-β-CDs1 and N-K1 was filtered to the TPU porous fiber membrane in step S1 by vacuum filtration, and dried at 60° C. for 12 h to obtain the TPU fiber membrane for removing bisphenols in water.
[0087] The N-β-CDs1 and N-K1 mixed dispersion is obtained by adding N-β-CDs1 and N-K1 into tetrahydrofuran;
[0088] The mass ratio of N-β-CDs1 to N-K1 in the N-β-CDs1 and N-K1 mixed dispersion is 2:1;
[0089] The total mass of the N-β-CDs1 and N-K1 is 20% of the mass of the TPU porous fiber membrane.
[0090] Example 3
[0091] A TPU fiber membrane for removing bisphenols in water, wherein the TPU fiber membrane is obtained by the following preparation method, which specifically comprises the following preparation steps:
[0092] S1, TPU was dissolved in a mixed solvent of ethanol and nonafluoroisobutyl methyl ether in a volume ratio of 2:1, the mass concentration of TPU in the mixed solvent was configured to be 20wt%, and the TPU solution was obtained after stirring at room temperature for 18h until it was uniform, and the TPU porous fiber membrane was prepared by electrospinning;
[0093] The electrospinning method comprises the following specific steps: electrospinning is performed using an electrospinning device, firstly a TPU solution is injected into a plastic syringe, and the spinning conditions are: voltage 15 kV, injection speed 0.8 mL / h, receiving distance 10 cm, and continuous spinning for 3 h, so that a TPU film is obtained on a collecting roller, and then the TPU film is dried at 60° C. for 1 h and then at 80° C. for 1 h, so that the solvent is fully volatilized, and thus a TPU porous fiber film is obtained;
[0094] S2, prepare N-β-CDs1 and N-K1, and set aside;
[0095] S3. The mixed dispersion of N-β-CDs1 and N-K1 was filtered to the TPU porous fiber membrane in step S1 by vacuum filtration, and dried at 60° C. for 12 h to obtain the TPU fiber membrane for removing bisphenols in water.
[0096] The N-β-CDs1 and N-K1 mixed dispersion is obtained by adding N-β-CDs1 and N-K1 into tetrahydrofuran;
[0097] The mass ratio of N-β-CDs1 to N-K1 in the N-β-CDs1 and N-K1 mixed dispersion is 3:1;
[0098] The total mass of the N-β-CDs1 and N-K1 is 20% of the mass of the TPU porous fiber membrane.
[0099] Example 4
[0100] A TPU fiber membrane for removing bisphenols in water, wherein the TPU fiber membrane is obtained by the following preparation method, which specifically comprises the following preparation steps:
[0101] S1, TPU was dissolved in a mixed solvent of ethanol and nonafluoroisobutyl methyl ether in a volume ratio of 2:1, the mass concentration of TPU in the mixed solvent was configured to be 20wt%, and the TPU solution was obtained after stirring at room temperature for 18h until it was uniform, and the TPU porous fiber membrane was prepared by electrospinning;
[0102] The electrospinning method comprises the following specific steps: electrospinning is performed using an electrospinning device, firstly a TPU solution is injected into a plastic syringe, and the spinning conditions are: voltage 15 kV, injection speed 0.8 mL / h, receiving distance 10 cm, and continuous spinning for 3 h, so that a TPU film is obtained on a collecting roller, and then the TPU film is dried at 60° C. for 1 h and then at 80° C. for 1 h, so that the solvent is fully volatilized, and thus a TPU porous fiber film is obtained;
[0103] S2, prepare N-β-CDs2 and N-K2, and set aside;
[0104] S3. The mixed dispersion of N-β-CDs2 and N-K2 is filtered to the TPU porous fiber membrane in step S1 by vacuum filtration, and dried at 60° C. for 12 h to obtain the TPU fiber membrane for removing bisphenols in water.
[0105] The N-β-CDs2 and N-K2 mixed dispersion is obtained by adding N-β-CDs2 and N-K2 into tetrahydrofuran;
[0106] The mass ratio of N-β-CDs2 to N-K2 in the N-β-CDs2 and N-K2 mixed dispersion is 2:1;
[0107] The total mass of the N-β-CDs2 and N-K2 is 20% of the mass of the TPU porous fiber membrane.
[0108] Example 5
[0109] A TPU fiber membrane for removing bisphenols in water, wherein the TPU fiber membrane is obtained by the following preparation method, which specifically comprises the following preparation steps:
[0110] S1, TPU was dissolved in a mixed solvent of ethanol and nonafluoroisobutyl methyl ether in a volume ratio of 2:1, the mass concentration of TPU in the mixed solvent was configured to be 20wt%, and the TPU solution was obtained after stirring at room temperature for 18h until it was uniform, and the TPU porous fiber membrane was prepared by electrospinning;
[0111] The electrospinning method comprises the following specific steps: electrospinning is performed using an electrospinning device, firstly a TPU solution is injected into a plastic syringe, and the spinning conditions are: voltage 15 kV, injection speed 0.8 mL / h, receiving distance 10 cm, and continuous spinning for 3 h, so that a TPU film is obtained on a collecting roller, and then the TPU film is dried at 60° C. for 1 h and then at 80° C. for 1 h, so that the solvent is fully volatilized, and thus a TPU porous fiber film is obtained;
[0112] S2, prepare N-β-CDs1 and N-K2, and set aside;
[0113] S3. The mixed dispersion of N-β-CDs1 and N-K2 was filtered to the TPU porous fiber membrane in step S1 by vacuum filtration, and dried at 60° C. for 12 h to obtain the TPU fiber membrane for removing bisphenols in water.
[0114] The N-β-CDs1 and N-K2 mixed dispersion is obtained by adding N-β-CDs1 and N-K2 into tetrahydrofuran;
[0115] The mass ratio of N-β-CDs1 to N-K2 in the N-β-CDs1 and N-K2 mixed dispersion is 2:1;
[0116] The total mass of the N-β-CDs1 and N-K2 is 20% of the mass of the TPU porous fiber membrane.
[0117] Example 6
[0118] A TPU fiber membrane for removing bisphenols in water, wherein the TPU fiber membrane is obtained by the following preparation method, which specifically comprises the following preparation steps:
[0119] S1, TPU was dissolved in a mixed solvent of ethanol and nonafluoroisobutyl methyl ether in a volume ratio of 2:1, the mass concentration of TPU in the mixed solvent was configured to be 20wt%, and the TPU solution was obtained after stirring at room temperature for 18h until it was uniform, and the TPU porous fiber membrane was prepared by electrospinning;
[0120] The electrospinning method comprises the following specific steps: electrospinning is performed using an electrospinning device, firstly a TPU solution is injected into a plastic syringe, and the spinning conditions are: voltage 15 kV, injection speed 0.8 mL / h, receiving distance 10 cm, and continuous spinning for 3 h, so that a TPU film is obtained on a collecting roller, and then the TPU film is dried at 60° C. for 1 h and then at 80° C. for 1 h, so that the solvent is fully volatilized, and thus a TPU porous fiber film is obtained;
[0121] S2, prepare N-β-CDs2 and N-K1, and set aside;
[0122] S3. The mixed dispersion of N-β-CDs2 and N-K1 was filtered to the TPU porous fiber membrane in step S1 by vacuum filtration, and dried at 60° C. for 12 h to obtain the TPU fiber membrane for removing bisphenols in water.
[0123] The N-β-CDs2 and N-K1 mixed dispersion is obtained by adding N-β-CDs2 and N-K1 into tetrahydrofuran;
[0124] The mass ratio of N-β-CDs2 to N-K1 in the N-β-CDs2 and N-K1 mixed dispersion is 2:1;
[0125] The total mass of the N-β-CDs2 and N-K1 is 20% of the mass of the TPU porous fiber membrane.
[0126] Comparative Example 1
[0127] A TPU fiber membrane for removing bisphenols in water, wherein the TPU fiber membrane is obtained by the following preparation method, which specifically comprises the following preparation steps:
[0128] S1, TPU was dissolved in a mixed solvent of ethanol and nonafluoroisobutyl methyl ether in a volume ratio of 1:1, the mass concentration of TPU in the mixed solvent was configured to be 20wt%, and the TPU solution was obtained by stirring at room temperature for 18h until it was uniform, and the TPU porous fiber membrane was prepared by electrospinning;
[0129] The electrospinning method comprises the following specific steps: electrospinning is performed using an electrospinning device, firstly a TPU solution is injected into a plastic syringe, and the spinning conditions are: voltage 15 kV, injection speed 0.8 mL / h, receiving distance 10 cm, and continuous spinning for 3 h, so that a TPU film is obtained on a collecting roller, and then the TPU film is dried at 60° C. for 1 h and then at 80° C. for 1 h, so that the solvent is fully volatilized, and thus a TPU porous fiber film is obtained;
[0130] S2, prepare N-β-CDs1 and N-K1, and set aside;
[0131] S3. The mixed dispersion of N-β-CDs1 and N-K1 was filtered to the TPU porous fiber membrane in step S1 by vacuum filtration, and dried at 60° C. for 12 h to obtain the TPU fiber membrane for removing bisphenols in water.
[0132] The N-β-CDs1 and N-K1 mixed dispersion is obtained by adding N-β-CDs1 and N-K1 into tetrahydrofuran;
[0133] The mass ratio of N-β-CDs1 to N-K1 in the N-β-CDs1 and N-K1 mixed dispersion is 2:1;
[0134] The total mass of the N-β-CDs1 and N-K1 is 20% of the mass of the TPU porous fiber membrane.
[0135] Comparative Example 2
[0136] A TPU fiber membrane for removing bisphenols in water, wherein the TPU fiber membrane is obtained by the following preparation method, which specifically comprises the following preparation steps:
[0137] S1, TPU was dissolved in a mixed solvent of ethanol and nonafluoroisobutyl methyl ether in a volume ratio of 4:1, the mass concentration of TPU in the mixed solvent was configured to be 20wt%, and the TPU solution was obtained after stirring at room temperature for 18h until it was uniform, and the TPU porous fiber membrane was prepared by electrospinning;
[0138] The electrospinning method comprises the following specific steps: electrospinning is performed using an electrospinning device, firstly a TPU solution is injected into a plastic syringe, and the spinning conditions are: voltage 15 kV, injection speed 0.8 mL / h, receiving distance 10 cm, and continuous spinning for 3 h, so that a TPU film is obtained on a collecting roller, and then the TPU film is dried at 60° C. for 1 h and then at 80° C. for 1 h, so that the solvent is fully volatilized, and thus a TPU porous fiber film is obtained;
[0139] S2, prepare N-β-CDs1 and N-K1, and set aside;
[0140] S3. The mixed dispersion of N-β-CDs1 and N-K1 was filtered to the TPU porous fiber membrane in step S1 by vacuum filtration, and dried at 60° C. for 12 h to obtain the TPU fiber membrane for removing bisphenols in water.
[0141] The N-β-CDs1 and N-K1 mixed dispersion is obtained by adding N-β-CDs1 and N-K1 into tetrahydrofuran;
[0142] The mass ratio of N-β-CDs1 to N-K1 in the N-β-CDs1 and N-K1 mixed dispersion is 2:1;
[0143] The total mass of the N-β-CDs1 and N-K1 is 20% of the mass of the TPU porous fiber membrane.
[0144] Comparative Example 3
[0145] A TPU fiber membrane for removing bisphenols in water, wherein the TPU fiber membrane is obtained by the following preparation method, which specifically comprises the following preparation steps:
[0146] S1, TPU was dissolved in a mixed solvent of ethanol and nonafluoroisobutyl methyl ether in a volume ratio of 2:1, the mass concentration of TPU in the mixed solvent was configured to be 20wt%, and the TPU solution was obtained after stirring at room temperature for 18h until it was uniform, and the TPU porous fiber membrane was prepared by electrospinning;
[0147] The electrospinning method comprises the following specific steps: electrospinning is performed using an electrospinning device, firstly a TPU solution is injected into a plastic syringe, and the spinning conditions are: voltage 15 kV, injection speed 0.8 mL / h, receiving distance 10 cm, and continuous spinning for 3 h, so that a TPU film is obtained on a collecting roller, and then the TPU film is dried at 60° C. for 1 h and then at 80° C. for 1 h, so that the solvent is fully volatilized, and thus a TPU porous fiber film is obtained;
[0148] S2, prepare N-β-CDs1 and N-K1, and set aside;
[0149] S3. The mixed dispersion of N-β-CDs1 and N-K1 was filtered to the TPU porous fiber membrane in step S1 by vacuum filtration, and dried at 60° C. for 12 h to obtain the TPU fiber membrane for removing bisphenols in water.
[0150] The N-β-CDs1 and N-K1 mixed dispersion is obtained by adding N-β-CDs1 and N-K1 into tetrahydrofuran;
[0151] The mass ratio of N-β-CDs1 to N-K1 in the N-β-CDs1 and N-K1 mixed dispersion is 1:1;
[0152] The total mass of the N-β-CDs1 and N-K1 is 20% of the mass of the TPU porous fiber membrane.
[0153] Comparative Example 4
[0154] A TPU fiber membrane for removing bisphenols in water, wherein the TPU fiber membrane is obtained by the following preparation method, which specifically comprises the following preparation steps:
[0155] S1, TPU was dissolved in a mixed solvent of ethanol and nonafluoroisobutyl methyl ether in a volume ratio of 2:1, the mass concentration of TPU in the mixed solvent was configured to be 20wt%, and the TPU solution was obtained after stirring at room temperature for 18h until it was uniform, and the TPU porous fiber membrane was prepared by electrospinning;
[0156] The electrospinning method comprises the following specific steps: electrospinning is performed using an electrospinning device, firstly a TPU solution is injected into a plastic syringe, and the spinning conditions are: voltage 15 kV, injection speed 0.8 mL / h, receiving distance 10 cm, and continuous spinning for 3 h, so that a TPU film is obtained on a collecting roller, and then the TPU film is dried at 60° C. for 1 h and then at 80° C. for 1 h, so that the solvent is fully volatilized, and thus a TPU porous fiber film is obtained;
[0157] S2, prepare N-β-CDs1 and N-K1, and set aside;
[0158] S3. The mixed dispersion of N-β-CDs1 and N-K1 was filtered to the TPU porous fiber membrane in step S1 by vacuum filtration, and dried at 60° C. for 12 h to obtain the TPU fiber membrane for removing bisphenols in water.
[0159] The N-β-CDs1 and N-K1 mixed dispersion is obtained by adding N-β-CDs1 and N-K1 into tetrahydrofuran;
[0160] The mass ratio of N-β-CDs1 to N-K1 in the N-β-CDs1 and N-K1 mixed dispersion is 4:1;
[0161] The total mass of the N-β-CDs1 and N-K1 is 20% of the mass of the TPU porous fiber membrane.
[0162] Comparative Example 5
[0163] A TPU fiber membrane for removing bisphenols in water, wherein the TPU fiber membrane is obtained by the following preparation method, which specifically comprises the following preparation steps:
[0164] S1, TPU was dissolved in a mixed solvent of ethanol and nonafluoroisobutyl methyl ether in a volume ratio of 2:1, the mass concentration of TPU in the mixed solvent was configured to be 20wt%, and the TPU solution was obtained after stirring at room temperature for 18h until it was uniform, and the TPU porous fiber membrane was prepared by electrospinning;
[0165] The electrospinning method comprises the following specific steps: electrospinning is performed using an electrospinning device, firstly a TPU solution is injected into a plastic syringe, and the spinning conditions are: voltage 15 kV, injection speed 0.8 mL / h, receiving distance 10 cm, and continuous spinning for 3 h, so that a TPU film is obtained on a collecting roller, and then the TPU film is dried at 60° C. for 1 h and then at 80° C. for 1 h, so that the solvent is fully volatilized, and thus a TPU porous fiber film is obtained;
[0166] S2, prepare N-β-CDs-c1 and NK-c1, and set aside;
[0167] S3. The mixed dispersion of N-β-CDs-c1 and NK-c1 was filtered into the TPU porous fiber membrane of step S1 by vacuum filtration, and dried at 60° C. for 12 h to obtain the TPU fiber membrane for removing bisphenols in water.
[0168] The N-β-CDs-c1 and NK-c1 mixed dispersion is obtained by adding N-β-CDs-c1 and NK-c1 into tetrahydrofuran;
[0169] The mass ratio of N-β-CDs-c1 to NK-c1 in the N-β-CDs-c1 and NK-c1 mixed dispersion is 2:1;
[0170] The total mass of the N-β-CD-c1 and NK-c1 is 20% of the mass of the TPU porous fiber membrane.
[0171] Comparative Example 6
[0172] A TPU fiber membrane for removing bisphenols in water, wherein the TPU fiber membrane is obtained by the following preparation method, which specifically comprises the following preparation steps:
[0173] S1, TPU was dissolved in a mixed solvent of ethanol and nonafluoroisobutyl methyl ether in a volume ratio of 2:1, the mass concentration of TPU in the mixed solvent was configured to be 20wt%, and the TPU solution was obtained after stirring at room temperature for 18h until it was uniform, and the TPU porous fiber membrane was prepared by electrospinning;
[0174] The electrospinning method comprises the following specific steps: electrospinning is performed using an electrospinning device, firstly a TPU solution is injected into a plastic syringe, and the spinning conditions are: voltage 15 kV, injection speed 0.8 mL / h, receiving distance 10 cm, and continuous spinning for 3 h, so that a TPU film is obtained on a collecting roller, and then the TPU film is dried at 60° C. for 1 h and then at 80° C. for 1 h, so that the solvent is fully volatilized, and thus a TPU porous fiber film is obtained;
[0175] S2, prepare N-β-CDs-c2 and NK-c2 for later use;
[0176] S3. The mixed dispersion of N-β-CDs-c2 and NK-c2 was filtered into the TPU porous fiber membrane of step S1 by vacuum filtration, and dried at 60° C. for 12 h to obtain the TPU fiber membrane for removing bisphenols in water.
[0177] The N-β-CDs-c2 and NK-c2 mixed dispersion is obtained by adding N-β-CDs-c2 and NK-c2 into tetrahydrofuran;
[0178] The mass ratio of N-β-CDs-c2 to NK-c2 in the N-β-CDs-c2 and NK-c2 mixed dispersion is 2:1;
[0179] The total mass of the N-β-CD-c2 and NK-c2 is 20% of the mass of the TPU porous fiber membrane.
[0180] Comparative Example 7
[0181] A TPU fiber membrane for removing bisphenols in water, wherein the TPU fiber membrane is obtained by the following preparation method, which specifically comprises the following preparation steps:
[0182] S1, TPU was dissolved in a mixed solvent of ethanol and nonafluoroisobutyl methyl ether in a volume ratio of 2:1, the mass concentration of TPU in the mixed solvent was configured to be 20wt%, and the TPU solution was obtained after stirring at room temperature for 18h until it was uniform, and the TPU porous fiber membrane was prepared by electrospinning;
[0183] The specific steps of the electrospinning method are as follows: electrospinning is performed using an electrospinning device, firstly the TPU solution is injected into a plastic syringe, the spinning conditions are: voltage 15 kV, injection speed 0.8 mL / h, receiving distance 10 cm, continuous spinning for 3 hours, that is, a TPU film is obtained on a collecting roller, and then the TPU film is dried at 80° C. for 2 hours to fully volatilize the solvent, and then a TPU porous fiber membrane is obtained;
[0184] S2, prepare N-β-CDs1 and N-K1, and set aside;
[0185] S3. The mixed dispersion of N-β-CDs1 and N-K1 was filtered to the TPU porous fiber membrane in step S1 by vacuum filtration, and dried at 60° C. for 12 h to obtain the TPU fiber membrane for removing bisphenols in water.
[0186] The N-β-CDs1 and N-K1 mixed dispersion is obtained by adding N-β-CDs1 and N-K1 into tetrahydrofuran;
[0187] The mass ratio of N-β-CDs1 to N-K1 in the N-β-CDs1 and N-K1 mixed dispersion is 2:1;
[0188] The total mass of the N-β-CDs1 and N-K1 is 20% of the mass of the TPU porous fiber membrane.
[0189] Comparative Example 8
[0190] A TPU fiber membrane for removing bisphenols in water, wherein the TPU fiber membrane is obtained by the following preparation method, which specifically comprises the following preparation steps:
[0191] S1, the TPU was dissolved in ethanol, the mass concentration of TPU in the solvent was configured to be 20wt%, and the TPU solution was obtained by stirring at room temperature for 18h until uniform, and the TPU porous fiber membrane was prepared by electrospinning;
[0192] The electrospinning method comprises the following specific steps: electrospinning is performed using an electrospinning device, firstly a TPU solution is injected into a plastic syringe, and the spinning conditions are: voltage 15 kV, injection speed 0.8 mL / h, receiving distance 10 cm, and continuous spinning for 3 h, so that a TPU film is obtained on a collecting roller, and then the TPU film is dried at 60° C. for 1 h and then at 80° C. for 1 h, so that the solvent is fully volatilized, and thus a TPU porous fiber film is obtained;
[0193] S2, prepare N-β-CDs1 and N-K1, and set aside;
[0194] S3. The mixed dispersion of N-β-CDs1 and N-K1 was filtered to the TPU porous fiber membrane in step S1 by vacuum filtration, and dried at 60° C. for 12 h to obtain the TPU fiber membrane for removing bisphenols in water.
[0195] The N-β-CDs1 and N-K1 mixed dispersion is obtained by adding N-β-CDs1 and N-K1 into tetrahydrofuran;
[0196] The mass ratio of N-β-CDs1 to N-K1 in the N-β-CDs1 and N-K1 mixed dispersion is 2:1;
[0197] The total mass of the N-β-CDs1 and N-K1 is 20% of the mass of the TPU porous fiber membrane.
[0198] Comparative Example 9
[0199] A TPU fiber membrane for removing bisphenols in water, wherein the TPU fiber membrane is obtained by the following preparation method, which specifically comprises the following preparation steps:
[0200] S1, the TPU was dissolved in nonafluoroisobutyl methyl ether, the mass concentration of TPU in the solvent was configured to be 20wt%, and the TPU solution was obtained by stirring at room temperature for 18h until uniform, and the TPU porous fiber membrane was prepared by electrospinning;
[0201] The electrospinning method comprises the following specific steps: electrospinning is performed using an electrospinning device, firstly a TPU solution is injected into a plastic syringe, and the spinning conditions are: voltage 15 kV, injection speed 0.8 mL / h, receiving distance 10 cm, and continuous spinning for 3 h, so that a TPU film is obtained on a collecting roller, and then the TPU film is dried at 60° C. for 1 h and then at 80° C. for 1 h, so that the solvent is fully volatilized, and thus a TPU porous fiber film is obtained;
[0202] S2, prepare N-β-CDs1 and N-K1, and set aside;
[0203] S3. The mixed dispersion of N-β-CDs1 and N-K1 was filtered to the TPU porous fiber membrane in step S1 by vacuum filtration, and dried at 60° C. for 12 h to obtain the TPU fiber membrane for removing bisphenols in water.
[0204] The N-β-CDs1 and N-K1 mixed dispersion is obtained by adding N-β-CDs1 and N-K1 into tetrahydrofuran;
[0205] The mass ratio of N-β-CDs1 to N-K1 in the N-β-CDs1 and N-K1 mixed dispersion is 2:1;
[0206] The total mass of the N-β-CDs1 and N-K1 is 20% of the mass of the TPU porous fiber membrane.
[0207] Performance Test:
[0208] Adsorption removal rate and adsorption efficiency:
[0209] The TPU fiber membranes for removing bisphenols in water of Examples 1-6 and Comparative Examples 1-7 were respectively placed in 50 mL of 20 mg / L bisphenol A aqueous solution, and samples were taken at 10 min, 20 min, 25 min, 30 min, 35 min, 40 min, 50 min, 60 min, 70 min, 80 min, 90 min, and 100 min, respectively, and the concentration of the bisphenol A aqueous solution was tested by HPLC. When the concentration of the bisphenol A aqueous solution remained unchanged, the adsorption removal rate of bisphenol A was calculated, and the time was counted as the shortest adsorption time, which represented the adsorption efficiency value.
[0210] The test results are shown in Table 1 below:
[0211] Table 1
[0212]
[0213] By comparing Examples 1-6 and Comparative Examples 1-7 in Table 1, it can be seen that the TPU fiber membrane preparation method for removing bisphenols in water of the present invention adopts a mixed solvent of ethanol and nonafluoroisobutyl methyl ether in a specific proportion as a porogen of the TPU fiber membrane in the preparation step of the TPU porous fiber membrane, and simultaneously adopts a specific proportion of 2-aminoterephthalic acid-modified β-cyclodextrin and chitosan to load on the TPU fiber membrane, so that the final TPU fiber membrane has excellent bisphenol A adsorption removal rate (≥99.5%) and high adsorption efficiency (shortest adsorption time ≤30min). Among them, the TPU fiber membrane of Example 1 has the best performance in various aspects, and can achieve a bisphenol A adsorption removal rate of 99.9% in 20min.
[0214] By comparing Examples 1-6 with Comparative Examples 1-2 and 8-9 in Table 1, it can be seen that in the preparation process of TPU porous fiber membrane, when a mixed solvent of ethanol and nonafluoroisobutyl methyl ether in different proportions is used, when the content of nonafluoroisobutyl methyl ether in the mixed solvent is too low or too high, or only a single solvent is contained, it has an adverse effect on the adsorption removal rate and adsorption efficiency of the final TPU fiber membrane. It can be seen that the mixed solvent of ethanol and nonafluoroisobutyl methyl ether plays a synergistic role in the preparation process of TPU fiber membrane. This may be because ethanol and nonafluoroisobutyl methyl ether have different boiling points and volatilization rates, which bring different porosities and pore uniformity to the TPU porous fiber membrane.
[0215] By comparing Examples 1-6 with Comparative Example 7 in Table 1, it can be seen that in the preparation process of the TPU porous fiber membrane, when the gradient heating program is not adopted, the final adsorption effect is adversely affected. This is because the boiling points and saturated vapor pressures of the two solvents are different. The gradient heating can ensure uniform volatilization of the solvent, which has a positive effect on the porosity and uniformity of the TPU porous fiber membrane.
[0216] By comparing Examples 1-6 with Comparative Examples 3-4 in Table 1, it can be seen that when the content ratio of amino-modified β-cyclodextrin and amino-modified chitosan is not within the specified ratio range of the present invention, the adsorption removal rate and adsorption efficiency of bisphenol A of the finally obtained TPU fiber membrane are significantly inferior to those of Example 1, indicating that amino-modified β-cyclodextrin and amino-modified chitosan play a synergistic role in the system, which is caused by the different adsorption properties of the two for bisphenol A.
[0217] By comparing Examples 1-6 with Comparative Examples 5-6 in Table 1, it can be seen that when the surface treatment concentrations of amino-modified β-cyclodextrin and amino-modified chitosan are different, or when 2-aminoterephthalic acid is not used but aminopropionic acid is used for treatment, the adsorption removal rate and adsorption efficiency of the final TPU fiber membrane are adversely affected. This may be because the aromatic surface treatment agent will bring about a favorable effect of Π-Π stacking when adsorbing bisphenol A, and different surface treatment concentrations will affect the adsorption effect.
[0218] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the embodiments of the present invention rather than to limit them. Although the embodiments of the present invention have been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the embodiments of the present invention can still be modified or replaced by equivalents, and these modifications or equivalent replacements cannot cause the modified technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a TPU fiber membrane for removing bisphenols in water, characterized in that: The TPU fiber membrane specifically includes the following preparation steps: S1, dissolving TPU in a mixed solvent of ethanol and nonafluoroisobutyl methyl ether, stirring at room temperature for a certain period of time until uniform to obtain a TPU solution, preparing a TPU film by an electrospinning method, and then drying the solvent by a gradient heating program to obtain a TPU porous fiber membrane; The volume ratio of ethanol and nonafluoroisobutyl methyl ether in the mixed solvent of step S1 is (2-3): 1; The gradient temperature program is drying at 60°C for 1 hour, and then drying at 80°C for 1 hour; S2, using 2-aminoterephthalic acid to modify β-cyclodextrin and chitosan to obtain amino-modified β-cyclodextrin and amino-modified chitosan respectively; The mass ratio of 2-aminoterephthalic acid to β-cyclodextrin or chitosan is 1:(3-5); S3, filtering the mixed dispersion of amino-modified β-cyclodextrin and amino-modified chitosan to the TPU porous fiber membrane of step S1 by suction filtration, and drying to obtain the TPU fiber membrane for removing bisphenols in water; The mass ratio of the amino-modified β-cyclodextrin to the amino-modified chitosan is (2-3):
1.
2. The method for preparing a TPU fiber membrane for removing bisphenols in water according to claim 1, characterized in that: The mass concentration of TPU in the mixed solvent in step S1 is 15-25wt%; The stirring time is 12-24h; The specific steps of the electrospinning method are: electrospinning is performed using an electrospinning device, the TPU solution is first injected into a plastic syringe, and the spinning conditions are: voltage 15 kV, injection speed 0.5 mL / h-1 mL / h, receiving distance 10 cm-20 cm, continuous spinning 1-3 hours, and a TPU film is obtained on a collecting roller.
3. The method for preparing a TPU fiber membrane for removing bisphenols in water according to claim 1, characterized in that: The method for modifying β-cyclodextrin with 2-aminoterephthalic acid in step S2 is: adding 2-aminoterephthalic acid to an organic solvent containing β-cyclodextrin, adding a certain amount of dehydrating agent, stirring evenly, reacting at 35-45° C. for 12-24 hours, and then centrifugally filtering, washing with water and drying to obtain amino-modified β-cyclodextrin; The method for modifying chitosan with 2-aminoterephthalic acid is as follows: adding 2-aminoterephthalic acid to an organic solvent containing chitosan, adding a certain amount of a dehydrating agent, stirring evenly, reacting at 35-45° C. for 12-24 hours, and then centrifugally filtering, washing with water and drying to obtain amino-modified chitosan.
4. The method for preparing a TPU fiber membrane for removing bisphenols in water according to claim 3, characterized in that: The organic solvent is selected from dimethylformamide, dimethyl sulfoxide or dichloromethane; The dehydrating agent is selected from DDC or EDC·HCl; The mass concentration of the organic solvent containing β-cyclodextrin or the organic solvent containing chitosan is 15-25%; The mass ratio of the dehydrating agent to 2-aminoterephthalic acid is 10%.
5. The method for preparing a TPU fiber membrane for removing bisphenols in water according to claim 1, characterized in that: The mixed dispersion of amino-modified β-cyclodextrin and amino-modified chitosan in step S3 is obtained by adding the amino-modified β-cyclodextrin and amino-modified chitosan obtained in step S2 into tetrahydrofuran; The total mass of the amino-modified β-cyclodextrin and the amino-modified chitosan is 15-25% of the mass of the TPU porous fiber membrane; The filtration is vacuum filtration; The drying is performed at 50-60° C. for 8-12 hours.
6. A TPU fiber membrane for removing bisphenols from water, characterized in that: The TPU fiber membrane is prepared by the preparation method described in any one of claims 1-5.
7. The TPU fiber membrane for removing bisphenols in water according to claim 6, characterized in that: The TPU fiber membrane for removing bisphenols from water has an adsorption removal rate of 99.5% or more for bisphenols, and a shortest adsorption time of 30 minutes or less.
8. An application of the TPU fiber membrane prepared by the method for preparing a TPU fiber membrane for removing bisphenols in water according to any one of claims 1 to 5, wherein the application is to remove bisphenols in water.