Thin film photocatalyst as well as preparation method and application thereof
The 2D porous lamellar ZnIn2S4/TiO2 film photocatalyst was prepared by immersion pulling method and hydrothermal crystallization method, which solved the problems of low efficiency, high cost and poor selectivity of existing photocatalytic film materials, and achieved high efficiency and low cost. Degradation of organic pollutants, suitable for industrial applications.
Patent Information
- Application Number
- CN202411016460.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-27
- Publication Date
- 2024-10-29
AI Technical Summary
Existing photocatalytic film materials have low efficiency, high cost, and poor selectivity, and the powder catalyst has a short service life and is difficult to recycle, which limits its application in water purification.
A two-step method is used to prepare the thin film photocatalyst, which is the immersion pulling method and the hydrothermal crystallization method. Titanium dioxide nanosol and indium zinc sulfide are used to composite to form a 2D porous lamellar ZnIn2S4/TiO2 film, which is suitable for a variety of organic pollutants. degradation.
The photocatalytic degradation reaction rate is improved, a variety of organic pollutants are degraded, the cost is low, the application range is wide, and the film is reusable, and has the potential for industrial production.
Smart Images

Figure CN118847154A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a thin film photocatalyst, in particular to a thin film photocatalyst and a preparation method and application thereof. Background Art
[0002] Photocatalysis has made great breakthroughs in recent years as a safe, efficient and sustainable water purification method. The most promising of these are semiconductor-based photocatalysts, which have been widely studied due to their high efficiency in removing organic matter, good chemical stability and low cost. At present, powder photocatalysis has been widely studied, but powder catalysts have the disadvantages of short service life and difficulty in recycling.
[0003] Therefore, the preparation of high-performance photocatalytic thin film materials is of great scientific significance, but it is also a huge challenge. The defects of existing photocatalytic thin film preparation technology are: 1. Low efficiency. Many photocatalytic materials can only effectively utilize ultraviolet light, and the proportion of ultraviolet light in sunlight is small, which limits the photocatalytic efficiency of these materials. 2. High cost. High-efficiency photocatalytic thin film materials are often expensive, which limits their economic feasibility in large-scale applications. In addition, the preparation process may require complex equipment and technology, further increasing the cost. 3. Poor selectivity. Some photocatalytic films may show low selectivity in specific chemical reactions, affecting the quality of the final product.
[0004] In order to solve the above technical problems, the present invention provides a thin film photocatalyst and a preparation method and application thereof. Summary of the invention
[0005] The purpose of the present invention is to provide a thin film photocatalyst and its preparation method and application. The present invention has the characteristics of using a two-step method for preparation, namely an immersion pulling method and a hydrothermal crystallization method, a simple preparation process, and low-cost and readily available raw materials; the prepared thin film photocatalyst has a high catalytic degradation reaction rate, is reusable, can degrade a variety of organic pollutants, has a wide range of applications, is low in cost, and can be industrialized.
[0006] The technical solution of the present invention is: a thin film photocatalyst, which uses a glass slide, FTO glass, ITO glass, ceramic sheet or PAN board as a substrate, uses titanium dioxide nanosol to impregnate and pull a TiO2 film, hydrothermally crystallizes indium zinc sulfide and composites it on the TiO2 / substrate film, and indium zinc sulfide grows on the TiO2 / substrate film to form a 2D porous sheet indium zinc sulfide, thereby obtaining a 2D porous sheet ZnIn2S4 / TiO2 / substrate thin film photocatalyst.
[0007] In the aforementioned thin film photocatalyst, the thickness of the base plate is 50-200 mm.
[0008] In the aforementioned thin film photocatalyst, the TiO2 / substrate film is a titanium dioxide particle having 80-100 titanium dioxide particles spread on the substrate within an area of 100X100nm, the diameter of the titanium dioxide particles is 10-15nm, and the thickness of the TiO2 film is 50-200nm.
[0009] In the aforementioned thin film photocatalyst, the indium zinc sulfide grows vertically on the TiO2 / substrate film to form a 2D porous sheet of indium zinc sulfide. The 2D porous sheet of indium zinc sulfide is composed of arranged indium zinc sulfide holes and has a thickness of 700-800nm.
[0010] The method for preparing the thin film photocatalyst comprises the following steps:
[0011] (1) Add tetrabutyl titanate to anhydrous ethanol, then add glacial acetic acid, stir, and obtain product A;
[0012] (2) Add deionized water to anhydrous ethanol, then add nitric acid to adjust the pH value, stir, and obtain product B;
[0013] (3) Add product B to product A, stir, seal and age to obtain titanium dioxide nanosol, and obtain product C;
[0014] (4) Impregnating product C with a substrate, pulling a thin film, drying, and calcining to obtain a TiO2 / substrate film, product D;
[0015] (5) Indium chloride, zinc chloride, and thioacetamide are added to ethylene glycol and dissolved by ultrasonication to obtain an indium zinc sulfide precursor solution, which is product E;
[0016] (6) Product D and product E are placed in a reactor for hydrothermal crystallization reaction, cooled, and vacuum dried to obtain a 2D porous sheet ZnIn2S4 / TiO2 / substrate thin film photocatalyst.
[0017] In the above-mentioned method for preparing the thin film photocatalyst, in step (1), 5-15 mL of tetrabutyl titanate is added to 15-30 mL of anhydrous ethanol, and then 1-2 mL of glacial acetic acid is added, and stirred for 20-30 minutes to obtain product A.
[0018] In the aforementioned method for preparing the thin film photocatalyst, in step (2), 0.5-1.5 mL of deionized water is added to 10-20 mL of anhydrous ethanol, and then nitric acid is added to adjust the pH value to 1-4, and stirred for 5-15 minutes to obtain product B.
[0019] In the above-mentioned method for preparing thin film photocatalyst, in step (3), 15-25 mL of product B is added to 30-50 mL of product A, stirred for 1.5-3 h, sealed and aged for 5-60 h to obtain titanium dioxide nanosol, and product C is obtained.
[0020] In the aforementioned method for preparing thin film photocatalyst, in step (4), the substrate is immersed in product C for 5-15 seconds, then pulled upward at a speed of 0.1-0.5 mm / s, dried at 15-25°C for 10-20 minutes, then placed in a 40-80°C oven for drying for 10-50 minutes, and finally placed in a muffle furnace and heated to 400-550°C at a heating rate of 4-6°C / min and kept warm for 0.5-1.5 hours to obtain a TiO2 / substrate film, which is product D.
[0021] In the aforementioned method for preparing a thin film photocatalyst, in step (5), 0.3-0.5 g of indium chloride, 0.1-0.15 g of zinc chloride, and 0.2-0.4 g of thioacetamide are added to 30-50 mL of ethylene glycol and ultrasonically dissolved for 5-15 minutes to obtain an indium zinc sulfide precursor solution, which is product E.
[0022] In the aforementioned method for preparing thin film photocatalysts, in step (5), product D and product E are placed in a reactor, hydrothermally crystallized at 100-200°C for 3-12 hours, cooled, and placed in a vacuum oven at 50-70°C for vacuum drying for 18-24 hours to obtain a 2D porous sheet ZnIn2S4 / TiO2 / substrate plate thin film photocatalyst.
[0023] The application of the thin film photocatalyst, the 2D porous sheet ZnIn2S4 / TiO2 / substrate plate thin film photocatalyst is used for photocatalytic degradation of rhodamine B, methyl orange, methylene blue and tetracycline hydrochloride.
[0024] In the application of the aforementioned thin film photocatalyst, the 2D porous layer ZnIn2S4 / TiO2 / substrate plate thin film photocatalyst is used for photocatalytic degradation of rhodamine B at a wavelength of 500-600nm, photocatalytic degradation of methyl orange at a wavelength of 400-520nm, photocatalytic degradation of methylene blue at a wavelength of 600-700nm, and photocatalytic degradation of tetracycline hydrochloride at a wavelength of 250-400nm.
[0025] In the application of the aforementioned thin film photocatalyst, the 2D porous layer ZnIn2S4 / TiO2 / substrate plate thin film photocatalyst is used for photocatalytic degradation of rhodamine B at a wavelength of 554nm, photocatalytic degradation of methyl orange at a wavelength of 466nm, photocatalytic degradation of methylene blue at a wavelength of 664nm, and photocatalytic degradation of tetracycline hydrochloride at a wavelength of 357nm.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] 1. The present invention uses a glass slide, FTO glass, ITO glass, ceramic sheet or PAN board as a substrate. This material can be applied to a variety of substrates, and suitable substrate materials can be selected according to different sewage environments. The raw materials used in the present invention are all relatively low in price, and high-performance photocatalytic films can be prepared with cheap raw materials; titanium dioxide nanosol is used to impregnate and pull the TiO2 film. The present invention adopts an impregnation and pulling method to prepare a TiO2 / substrate film. This method is applicable to any sheet-like substrate, and the preparation process is simple. A film of the desired thickness can be prepared only by pulling the substrate up and down, which not only ensures that titanium dioxide will not fall off the substrate during the preparation process, but also ensures that a nano-scale and thickness-controllable film is prepared to the greatest extent. The nano-TiO2 / substrate film prepared by the present invention will play an indispensable fixing role during the hydrothermal crystallization of composite indium zinc sulfide. Indium zinc sulfide is hydrothermally crystallized and composited on a TiO2 / substrate film, and indium zinc sulfide grows on the TiO2 / substrate film to form a 2D porous sheet layer of indium zinc sulfide, thereby obtaining a 2D porous sheet layer ZnIn2S4 / TiO2 / substrate film photocatalyst. The present invention uses a hydrothermal crystallization method to grow a 2D porous sheet layer of indium zinc sulfide on a TiO2 / substrate film. This method is very commonly used in the fields of materials science and crystal engineering. Compared with traditional high-temperature melt growth, hydrothermal crystallization can be carried out at a relatively low temperature, which is helpful for synthesizing thermally unstable substances. And the hydrothermal crystallization method does not require expensive equipment, and can be mass-produced in smaller equipment, which makes it have a lower cost in industrial production. Including in the present invention, the cost of the raw materials used is very low, which can further reduce the cost and has the potential for industrial production.
[0028] 2. The thickness of the substrate used in the present invention is 0.5-2 mm. Using a substrate of appropriate thickness can improve mechanical stability. The appropriate substrate thickness can provide sufficient support for the film to ensure mechanical stability during preparation and subsequent processing. This is particularly important for preventing the film from being damaged, bent or cracked during processing or use.
[0029] 3. The TiO2 / substrate film of the present invention is a titanium dioxide particle with 80-100 titanium dioxide particles in an area of 100X100nm laid flat on the substrate, the diameter of the titanium dioxide particles is 10-15nm, and the thickness of the TiO2 film is 50-200nm. In the same area, the smaller the particle size of the titanium dioxide nanocrystal, the larger the surface area, the stronger the adsorption performance, the blue shift of the absorption band edge of its absorption spectrum, and the photocatalytic activity of titanium dioxide will be improved. At the same time, the quantum effect caused by the smaller particles will cause the band gap to widen and the energy band to blue shift. The widening of the band gap makes the electron / hole have a higher redox potential, so that the photocatalytic performance of the semiconductor is enhanced. The hydrothermal crystallization of indium zinc sulfide is compounded on the TiO2 / substrate film, and the morphology of the nanoparticles will enhance the wettability of the indium zinc sulfide precursor on the surface, thereby enhancing the adhesion to indium zinc sulfide.
[0030] 4. Indium zinc sulfide of the present invention grows vertically on the TiO2 / substrate film to form a 2D porous sheet indium zinc sulfide. The 2D porous sheet indium zinc sulfide is composed of arranged indium zinc sulfide holes and has a thickness of 700-800nm. The 2D porous sheet indium zinc sulfide has a porous structure and a large surface area, which can provide a large number of active sites and maximize the use of space, thereby improving the photocatalytic activity. At the same time, titanium dioxide and indium zinc sulfide form a Z-type heterojunction structure, which effectively increases the absorption of light. At the same time, the heterojunction promotes the separation of photogenerated charges, thereby achieving high carrier mobility and photocatalytic efficiency.
[0031] 5. In step (1) of the present invention, 5-15 mL of tetrabutyl titanate is added to 15-30 mL of anhydrous ethanol, and then 1-2 mL of glacial acetic acid is added, and stirred for 20-30 min to obtain product A. The effect of adding glacial acetic acid is to inhibit the hydrolysis of tetrabutyl titanate, and its mechanism is: acetate competes with water molecules in the reaction medium to be adsorbed on the surface of tetrabutyl titanate, hindering the approach and reaction of water molecules, and glacial acetic acid can adjust the pH value of the solution by releasing acetate ions. Lowering the pH value can control the hydrolysis rate, because under acidic conditions, the speed of the hydrolysis reaction will slow down. Its beneficial effect is to slow down the rate of hydrolysis and condensation reactions to prevent premature gel formation in the solution, thereby facilitating further operation and processing.
[0032] 6. In step (2) of the present invention, 0.5-1.5 mL of deionized water is added to 10-20 mL of anhydrous ethanol, and then nitric acid is added to adjust the pH value to 1-4, and stirred for 5-15 minutes to obtain product B. The purpose of adding nitric acid to adjust the pH value to acidic is to make the acidity and alkalinity of products A and B consistent, and to prevent unknown side reactions caused by different acidity and alkalinity from affecting the experimental results.
[0033] 7. In step (3) of the present invention, 15-25 mL of product B is added to 30-50 mL of product A, stirred for 1.5-3 hours, sealed and aged for 5-60 hours to obtain titanium dioxide nanosol and product C. During the aging process, the titanium dioxide in the sol will continue to polymerize and cross-link to form a larger polymer. This cross-linking effect makes the network structure stable and uniform. The aging process has the following beneficial effects: by extending the polymerization and maturation process in the sol, a more uniform material can be obtained, defects can be reduced, and the overall quality of the final product can be improved. And through aging, a material that is easy to process and shape can be obtained, which is helpful for subsequent processing.
[0034] 8. In step (4) of the present invention, after the substrate is immersed in product C for 5-15 seconds, it is pulled upward at a speed of 0.1-0.5 mm / s, dried at 15-25°C for 10-20 minutes, then placed in a 40-80°C oven for drying for 10-50 minutes, and finally placed in a muffle furnace and heated to 400-550°C at a heating rate of 4-6°C / min for 0.5-1.5 hours to obtain a TiO2 / substrate film, which is product D. The present invention adopts an immersion pulling method to prepare a TiO2 / substrate film. This method is applicable to the various substrates mentioned above. The preparation process is simple. A film of a desired thickness can be prepared by only pulling the substrate up and down, which not only ensures that titanium dioxide will not fall off the substrate during the preparation process, but also ensures that a TiO2 film with a nanometer thickness of 50-200 nm is prepared. The nano-TiO2 / substrate film prepared by the present invention will be used to fix indium zinc sulfide during hydrothermal crystallization of composite indium zinc sulfide.
[0035] 9. In step (5) of the present invention, 0.3-0.5g of indium chloride, 0.1-0.15g of zinc chloride, and 0.2-0.4g of thioacetamide are added to 30-50mL of ethylene glycol, and ultrasonically dissolved for 5-15min to obtain an indium zinc sulfide precursor solution, which is product E. The beneficial effect of preparing the material as a precursor solution first is that preparing the material as a precursor solution can ensure that the reactants are uniformly dispersed in the solution. This uniformity can achieve consistent reaction conditions, thereby resulting in uniform crystal growth and reduced defects. It can also promote the growth of complex morphologies, and the uniform reaction environment in the solution is conducive to the growth of crystals with complex or special morphologies.
[0036] 10. In step (5) of the present invention, product D and product E are placed in a reactor, hydrothermally crystallized at 100-200°C for 3-12 hours, cooled, and placed in a vacuum oven at 50-70°C for vacuum drying for 18-24 hours to obtain a 2D porous sheet ZnIn2S4 / TiO2 / substrate thin film photocatalyst. The present invention vertically constructs a 2D porous sheet indium zinc sulfide on the TiO2 / substrate thin film. The unique porous structure of the 2D sheet indium zinc sulfide provides more active sites for photocatalytic degradation. Compared with the 2D porous sheet ZnIn2S4 / TiO2 / substrate thin film photocatalyst, the TiO2 / substrate thin film has no pores inside, so that only the active sites on the outer surface of the TiO2 / substrate thin film can be used during degradation. At the same time, titanium dioxide can only absorb ultraviolet light, so the degradation performance of the TiO2 / substrate thin film is poor. The reason why the 2D porous sheet ZnIn2S4 / TiO2 / substrate thin film photocatalyst has a high surface area is mainly attributed to the composite 2D sheet indium zinc sulfide, and the high surface area of indium zinc sulfide mainly depends on the holes formed by the material itself during hydrothermal crystallization rather than the voids, so the 2D porous sheet ZnIn2S4 / TiO2 / substrate thin film photocatalyst can provide more active sites. At the same time, titanium dioxide and indium zinc sulfide form a Z-type heterojunction for efficient degradation of organic matter, paving the way for the industrialization of thin film photocatalysis.
[0037] 11. The 2D porous sheet ZnIn2S4 / TiO2 / substrate thin film photocatalyst of the present invention is used for photocatalytic degradation of rhodamine B, methylene blue, methyl orange and tetracycline hydrochloride. The film prepared by the present invention exhibits excellent photocatalytic degradation of organic matter performance, and can completely degrade 100ml, 50mg / L rhodamine B solution in 80min, degrade 20mg / L, 100ml methylene blue in 40min, and degrade 20mg / L, 100ml methyl orange in 80min. The degradation rate can reach more than 80%, and the degradation rate of 50mg / L, 100ml tetracycline hydrochloride in 80min is 79%. This 2D porous sheet ZnIn2S4 / TiO2 / substrate thin film photocatalyst has convenient recycling performance and stability, and can maintain highly stable photocatalytic activity and film stability.
[0038] 12. The 2D porous sheet ZnIn2S4 / TiO2 / substrate thin film photocatalyst of the present invention is used for photocatalytic degradation of rhodamine B at a wavelength of 500-600nm, photocatalytic degradation of methyl orange at a wavelength of 400-520nm, photocatalytic degradation of methylene blue at a wavelength of 600-700nm, and photocatalytic degradation of tetracycline hydrochloride at a wavelength of 250-400nm. The excellent performance of the film prepared by the present invention is due to the excellent stability of the TiO2 / substrate film, and the grown 2D porous sheet indium zinc sulfide broadens the light response range, strengthens the surface area, and enhances light absorption. The 2D porous sheet ZnIn2S4 / TiO2 / substrate thin film photocatalyst prepared by the present invention has a high catalytic degradation reaction rate and can be reused. After being reused for 4 times, it still maintains a removal rate of more than 95%, and has good stability. In addition, the construction of the titanium dioxide and indium zinc sulfide heterojunction forms a built-in electric field, which effectively promotes the transfer of photogenerated charges and ultimately achieves the improvement of photodegradation performance.
[0039] 13. The 2D porous sheet ZnIn2S4 / TiO2 / substrate thin film photocatalyst of the present invention is used for photocatalytic degradation of rhodamine B at a wavelength of 554nm, photocatalytic degradation of methyl orange at a wavelength of 466nm, photocatalytic degradation of methylene blue at a wavelength of 664nm, and photocatalytic degradation of tetracycline hydrochloride at a wavelength of 357nm. The 2D porous sheet ZnIn2S4 / TiO2 / substrate thin film photocatalyst prepared by the present invention can degrade rhodamine B, methyl orange, methylene blue and tetracycline hydrochloride at different concentrations, has a wide range of applications, and can adapt to different dyes and pollutants of different concentrations.
[0040] In summary, the present invention has a two-step preparation method, namely, an immersion pulling method and a hydrothermal crystallization method. The preparation process is simple and the raw materials are inexpensive and easily available. The prepared thin film photocatalyst has a high catalytic degradation reaction rate and is reusable. It can degrade a variety of organic pollutants, has a wide range of applications, is low in cost, and can be industrialized. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 It is a graph of degradation of RhB solution (50 mg / L, 100 ml) by 2D porous sheet ZnIn2S4 / TiO2 / substrate thin film photocatalyst prepared in Examples 1-5 of the present invention;
[0042] Figure 2 is a SEM surface and cross-sectional view of the TiO2 / substrate film prepared in Example 3 of the present invention, wherein Figure 2 a is the surface map, Figure 2 b is a cross-sectional view;
[0043] Figure 3 The SEM surface and cross-sectional images of the 2D porous sheet ZnIn2S4 / TiO2 / substrate thin film photocatalyst prepared in Example 3 of the present invention are shown in FIG. Figure 3 a is the surface map, Figure 3 b is a cross-sectional view;
[0044] Figure 4 TEM and mapping images of the 2D porous sheet ZnIn2S4 / TiO2 / substrate thin film photocatalyst prepared in Example 3 of the present invention, wherein Figure 4 a is the TEM image of 2D porous ZnIn2S4 / TiO2 / substrate thin film photocatalyst. Figure 4 bf are elemental mappings of Zn, In, S, Ti and O in the 2D porous sheet ZnIn2S4 / TiO2 / substrate thin film photocatalyst;
[0045] Figure 5 It is the XRD spectrum of the TiO2 / substrate thin film and the 2D porous sheet ZnIn2S4 / TiO2 / substrate thin film photocatalyst prepared in Example 3 of the present invention;
[0046] Figure 6 FTIR spectra of the TiO2 / substrate film and the 2D porous sheet ZnIn2S4 / TiO2 / substrate film photocatalyst prepared in Example 3 of the present invention;
[0047] Figure 7 The adsorption curve of RhB solution (50 mg / L, 100 ml) of the TiO2 / substrate film and the 2D porous sheet ZnIn2S4 / TiO2 / substrate film photocatalyst prepared in Example 3 of the present invention;
[0048] Figure 8 The degradation curve of RhB solution (50 mg / L, 100 ml) of the TiO2 / substrate film and the 2D porous sheet ZnIn2S4 / TiO2 / substrate film photocatalyst prepared in Example 3 of the present invention;
[0049] Fig. 9 It is the degradation curve of RhB solution of different concentrations of the 2D porous sheet ZnIn2S4 / TiO2 / substrate plate thin film photocatalyst prepared in Example 3 of the present invention;
[0050] Fig.10 The degradation curve of MB solution (20 mg / L, 100 ml) of the TiO2 / substrate film and the 2D porous sheet ZnIn2S4 / TiO2 / substrate film photocatalyst prepared in Example 3 of the present invention;
[0051] Fig.11 The degradation curve of MO solution (20 mg / L, 100 ml) of the TiO2 / substrate film and the 2D porous sheet ZnIn2S4 / TiO2 / substrate film photocatalyst prepared in Example 3 of the present invention;
[0052] Fig.12 This is the degradation curve of TC solution (50 mg / L, 100 ml) of the TiO2 / substrate thin film and 2D porous sheet ZnIn2S4 / TiO2 / substrate thin film photocatalyst prepared in Example 3 of the present invention. DETAILED DESCRIPTION
[0053] The present invention is further described below in conjunction with the accompanying drawings and embodiments, but they are not intended to limit the present invention.
[0054] Embodiment 1: A method for preparing a thin film photocatalyst comprises the following steps:
[0055] In step (1), 5 mL of tetrabutyl titanate was added to 15 mL of anhydrous ethanol, and then 1 mL of glacial acetic acid was added, and stirred for 20 min to obtain product A;
[0056] In step (2), 0.5 mL of deionized water was added to 10 mL of anhydrous ethanol, and nitric acid was added to adjust the pH value to 1, and stirred for 5 min to obtain product B;
[0057] In step (3), 15 mL of product B was added to 30 mL of product A, stirred for 1.5 h, sealed and aged for 5 h to obtain titanium dioxide nanosol, product C;
[0058] In step (4), FTO glass is used as a substrate, and the thickness of the substrate is 50-200 mm. After the substrate is immersed in product C for 5 seconds, it is pulled upward at a speed of 0.1 mm / s, dried at 15°C for 10 minutes, and then placed in a 40°C oven for drying for 10 minutes. Finally, it is placed in a muffle furnace and heated to 400°C at a heating rate of 4°C / min and kept warm for 0.5 hours to obtain a TiO2 / substrate film, which is product D.
[0059] In step (5), 0.3 g of indium chloride, 0.1 g of zinc chloride, and 0.2 g of thioacetamide were added to 30 mL of ethylene glycol and dissolved by ultrasonication for 5 min to obtain an indium zinc sulfide precursor solution, which is product E;
[0060] In step (6), product D and product E are placed in a reaction kettle, hydrothermally crystallized at 100°C for 3 hours, cooled, and placed in a vacuum oven at 50°C for vacuum drying for 18 hours to obtain a 2D porous sheet ZnIn2S4 / TiO2 / substrate plate thin film photocatalyst.
[0061] Embodiment 2: A method for preparing a thin film photocatalyst comprises the following steps:
[0062] In step (1), 8 mL of tetrabutyl titanate was added to 20 mL of anhydrous ethanol, and then 1.5 mL of glacial acetic acid was added, and stirred for 20 min to obtain product A;
[0063] In step (2), 0.8 mL of deionized water was added to 12 mL of anhydrous ethanol, and nitric acid was added to adjust the pH value to 1-4, and stirred for 5-15 min to obtain product B;
[0064] In step (3), 18 mL of product B was added to 35 mL of product A, stirred for 2 h, sealed and aged for 10 h to obtain titanium dioxide nanosol, product C;
[0065] In step (4), ITO glass is used as a substrate plate, and the thickness of the substrate plate is 50-200 mm. After the substrate plate is immersed in product C for 8 seconds, it is pulled upward at a speed of 0.2 mm / s, dried at 18°C for 15 minutes, and then placed in a 50°C oven for drying for 20 minutes. Finally, it is placed in a muffle furnace and heated to 450°C at a heating rate of 4°C / min and kept warm for 0.5 hours to obtain a TiO2 / substrate plate film, which is product D.
[0066] In step (5), 0.35 g of indium chloride, 0.1 g of zinc chloride, and 0.25 g of thioacetamide were added to 35 mL of ethylene glycol and dissolved by ultrasonication for 8 min to obtain an indium zinc sulfide precursor solution, which was product E.
[0067] In step (6), product D and product E are placed in a reaction kettle, hydrothermally crystallized at 120°C for 6 hours, cooled, and placed in a vacuum oven at 55°C for vacuum drying for 20 hours to obtain a 2D porous sheet ZnIn2S4 / TiO2 / substrate thin film photocatalyst.
[0068] Embodiment 3: A method for preparing a thin film photocatalyst comprises the following steps:
[0069] In step (1), 10 mL of tetrabutyl titanate was added to 25 mL of anhydrous ethanol, and then 1.5 mL of glacial acetic acid was added, and stirred for 25 min to obtain product A;
[0070] In step (2), 1 mL of deionized water was added to 15 mL of anhydrous ethanol, and nitric acid was added to adjust the pH value to 3, and stirred for 10 min to obtain product B;
[0071] In step (3), 20 mL of product B was added to 40 mL of product A, stirred for 2 h, sealed and aged for 36 h to obtain titanium dioxide nanosol, product C;
[0072] In step (4), a glass slide is used as a substrate, the thickness of the substrate is 50-200 mm, the substrate is immersed in product C for 10 seconds, pulled upward at a speed of 0.3 mm / s, dried at 20°C for 15 minutes, then placed in a 60°C oven for 30 minutes, and finally placed in a muffle furnace and heated to 500°C at a heating rate of 5°C / min for 1 hour to obtain a TiO2 / substrate film, which is product D;
[0073] In step (5), 0.4 g of indium chloride, 0.13 g of zinc chloride, and 0.3 g of thioacetamide were added to 40 mL of ethylene glycol and dissolved by ultrasonication for 10 min to obtain an indium zinc sulfide precursor solution, which was product E.
[0074] In step (6), product D and product E are placed in a reaction kettle, hydrothermally crystallized at 160°C for 6 hours, cooled, and placed in a vacuum oven at 60°C for vacuum drying for 20 hours to obtain a 2D porous sheet ZnIn2S4 / TiO2 / substrate thin film photocatalyst.
[0075] Embodiment 4: A method for preparing a thin film photocatalyst comprises the following steps:
[0076] In step (1), 12 mL of tetrabutyl titanate was added to 28 mL of anhydrous ethanol, and then 1.8 mL of glacial acetic acid was added, and stirred for 25 min to obtain product A;
[0077] In step (2), 1.5 mL of deionized water was added to 18 mL of anhydrous ethanol, and nitric acid was added to adjust the pH value to 4, and stirred for 15 min to obtain product B;
[0078] In step (3), 22 mL of product B was added to 45 mL of product A, stirred for 1.5-3 h, sealed and aged for 48 h to obtain titanium dioxide nanosol, product C;
[0079] In step (4), a ceramic sheet is used as a substrate, and the thickness of the substrate is 50-200 mm. After the substrate is immersed in product C for 12 seconds, it is pulled upward at a speed of 0.4 mm / s, dried at 25°C for 18 minutes, and then placed in a 70°C oven for drying for 40 minutes. Finally, it is placed in a muffle furnace and heated to 500°C at a heating rate of 5°C / min and kept warm for 1 hour to obtain a TiO2 / substrate film, which is product D.
[0080] In step (5), 0.45 g of indium chloride, 0.14 g of zinc chloride, and 0.35 g of thioacetamide were added to 45 mL of ethylene glycol and dissolved by ultrasonication for 12 min to obtain an indium zinc sulfide precursor solution, which was product E.
[0081] In step (6), product D and product E are placed in a reaction kettle, hydrothermally crystallized at 180°C for 9 hours, cooled, and placed in a vacuum oven at 60°C for vacuum drying for 20 hours to obtain a 2D porous sheet ZnIn2S4 / TiO2 / substrate thin film photocatalyst.
[0082] Embodiment 5: A method for preparing a thin film photocatalyst comprises the following steps:
[0083] In step (1), 15 mL of tetrabutyl titanate was added to 30 mL of anhydrous ethanol, and then 2 mL of glacial acetic acid was added, and stirred for 30 min to obtain product A;
[0084] In step (2), 1.5 mL of deionized water was added to 20 mL of anhydrous ethanol, and nitric acid was added to adjust the pH value to 4, and stirred for 15 min to obtain product B;
[0085] In step (3), 25 mL of product B was added to 50 mL of product A, stirred for 3 h, sealed and aged for 60 h to obtain titanium dioxide nanosol, product C;
[0086] In step (4), a PAN board is used as a substrate board, and the thickness of the substrate board is 50-200 mm. After the substrate board is immersed in product C for 15 seconds, it is pulled upward at a speed of 0.5 mm / s, dried at 25°C for 20 minutes, and then placed in an 80°C oven for drying for 50 minutes. Finally, it is placed in a muffle furnace and heated to 550°C at a heating rate of 6°C / min for 1.5 hours to obtain a TiO2 / substrate board film, which is product D.
[0087] In step (5), 0.5 g of indium chloride, 0.15 g of zinc chloride, and 0.4 g of thioacetamide were added to 50 mL of ethylene glycol and dissolved by ultrasonication for 15 min to obtain an indium zinc sulfide precursor solution, which was product E.
[0088] In step (6), product D and product E are placed in a reaction kettle, hydrothermally crystallized at 200°C for 12 hours, cooled, and placed in a vacuum oven at 70°C for vacuum drying for 24 hours to obtain a 2D porous sheet ZnIn2S4 / TiO2 / substrate plate thin film photocatalyst.
[0089] Application examples:
[0090] The application of the thin film photocatalyst, the 2D porous sheet ZnIn2S4 / TiO2 / substrate plate thin film photocatalyst is used for photocatalytic degradation of rhodamine B, methyl orange, methylene blue and tetracycline hydrochloride.
[0091] In the application of the aforementioned thin film photocatalyst, the 2D porous layer ZnIn2S4 / TiO2 / substrate plate thin film photocatalyst is used for photocatalytic degradation of rhodamine B at a wavelength of 500-600nm, photocatalytic degradation of methyl orange at a wavelength of 400-520nm, photocatalytic degradation of methylene blue at a wavelength of 600-700nm, and photocatalytic degradation of tetracycline hydrochloride at a wavelength of 250-400nm.
[0092] In the application of the aforementioned thin film photocatalyst, the 2D porous layer ZnIn2S4 / TiO2 / substrate plate thin film photocatalyst is used for photocatalytic degradation of rhodamine B at a wavelength of 554nm, photocatalytic degradation of methyl orange at a wavelength of 466nm, photocatalytic degradation of methylene blue at a wavelength of 664nm, and photocatalytic degradation of tetracycline hydrochloride at a wavelength of 357nm.
[0093] 1. The present invention applies the 2D porous sheet ZnIn2S4 / TiO2 / substrate plate thin film photocatalyst prepared in Examples 1-5 to the degradation of Rhodamine B solution, and uses an ultraviolet-visible spectrophotometer (UV-vis) to detect the absorbance and draw a degradation curve: a piece of film is placed in a jacketed beaker, the film size is controlled at 2.5cmX2.5cm, the temperature of the system is controlled at 25°C using a condensed water circulation system, 100ml of 50mg / L Rhodamine B solution is added, a dark reaction is carried out for 60min to achieve adsorption-desorption equilibrium, and then a 300W xenon lamp is used for illumination, 3ml of the solution is taken out from the solution every 10min to measure the absorbance at 554nm, and the relationship between the degradation rate and time is calculated.
[0094] The 2D porous sheet ZnIn2S4 / TiO2 / substrate thin film photocatalyst prepared by the preparation method of Examples 1-5 was tested for degradation of Rhodamine B solution to evaluate the degradation performance. Figure 1 is a graph of the degradation of RhB solution (50 mg / L, 100 ml) by the 2D porous sheet ZnIn2S4 / TiO2 / substrate thin film photocatalyst prepared in Examples 1-5 of the present invention; Figure 1 As shown, the degradation rates of the 2D porous sheet ZnIn2S4 / TiO2 / substrate plate thin film photocatalysts prepared by the preparation method of Examples 1-5 for Rhodamine B solution at 70 min were 81.1%, 92.6%, 96.9%, 95.4% and 78.1%, respectively. It can be seen that the photocatalytic degradation performance of the TiO2 / substrate plate thin film and the 2D porous sheet ZnIn2S4 / TiO2 / substrate plate thin film photocatalysts prepared by the preparation method of Example 3 are better than those of the thin film photocatalysts in other examples.
[0095] The TiO2 / substrate thin film and 2D porous sheet ZnIn2S4 / TiO2 / substrate thin film photocatalyst prepared by the preparation method of Example 3 were subjected to subsequent experiments and characterizations, as shown below:
[0096] 1. The present invention applies the 2D porous sheet ZnIn2S4 / TiO2 / substrate plate thin film photocatalyst prepared in the embodiment to adsorb Rhodamine B solution, and uses an ultraviolet-visible spectrophotometer (UV-vis) to detect the absorbance and draw an adsorption curve: a piece of film is placed in a jacketed beaker, the film size is controlled at 2.5cmX2.5cm, the temperature of the system is controlled at 25°C using a condensed water circulation system, 100ml of 50mg / L Rhodamine B solution is added, 3ml of the solution is taken out from the solution every 10min to measure the absorbance at 554nm, and the relationship between the adsorption rate and time is calculated.
[0097] 2. The present invention applies the TiO2 / substrate plate film and 2D porous sheet ZnIn2S4 / TiO2 / substrate plate film photocatalyst prepared in Example 3 to the degradation of methylene blue solution, and uses an ultraviolet-visible spectrophotometer (UV-vis) to detect the absorbance and draw a degradation curve: a piece of film is placed in a jacketed beaker, the film size is controlled at 2.5cmX2.5cm, the temperature of the system is controlled at 25°C using a condensed water circulation system, 100ml of 20mg / L methylene blue solution is added, a dark reaction is carried out for 60min to make it reach adsorption-desorption equilibrium, and then a 300W xenon lamp is used for illumination, 3ml of the solution is taken out from the solution every 10min to measure the absorbance at 664nm, and the relationship between the degradation rate and time is calculated.
[0098] 3. The present invention applies the TiO2 / substrate plate film and 2D porous sheet ZnIn2S4 / TiO2 / substrate plate film photocatalyst prepared in Example 3 to the degradation of methyl orange solution, and uses an ultraviolet-visible spectrophotometer (UV-vis) to detect the absorbance and draw a degradation curve: a piece of film is placed in a jacketed beaker, the film size is controlled at 2.5cmX2.5cm, the temperature of the system is controlled at 25°C using a condensed water circulation system, 100ml of 20mg / L methyl orange solution is added, and a dark reaction is carried out for 60min to reach adsorption-desorption equilibrium, then a 300W xenon lamp is used for illumination, 3ml of the solution is taken out from the solution every 10min to measure the absorbance at 466nm, and the relationship between the degradation rate and time is calculated.
[0099] 4. The present invention applies the TiO2 / substrate plate film and 2D porous sheet ZnIn2S4 / TiO2 / substrate plate film photocatalyst prepared in Example 3 to the degradation of tetracycline hydrochloride solution, and uses an ultraviolet-visible spectrophotometer (UV-vis) to detect the absorbance and draw a degradation curve: a piece of film is placed in a jacketed beaker, the film size is controlled at 2.5cmX2.5cm, the temperature of the system is controlled at 25°C using a condensed water circulation system, 100ml of 50mg / L tetracycline hydrochloride solution is added, and a dark reaction is carried out for 60min to reach adsorption-desorption equilibrium, then a 300W xenon lamp is used for illumination, 3ml of the solution is taken out from the solution every 10min, the absorbance at 357nm is measured, and the relationship between the degradation rate and time is calculated.
[0100] Experimental data:
[0101] Figure 2 is a SEM surface and cross-sectional view of the TiO2 / substrate film prepared in Example 3 of the present invention, wherein Figure 2 a is the surface map, Figure 2 b is a cross-sectional view; Figure 2As can be seen in a, titanium dioxide exists in the form of nanoparticles and is densely packed on the surface to form a dense and uniform film. There are 80-100 titanium dioxide particles in an area of 100X100nm spread on the substrate, and the diameter of the titanium dioxide particles is 10-15nm; Figure 2 b shows that the thickness of the TiO2 film is 50-200nm, and the SEM image of the TiO2 / substrate film produced by immersion pulling shows that the surface is relatively smooth, without cracks, and the thickness is 72nm. This indicates that the titanium dioxide prepared by the immersion pulling method can be well attached to the glass surface, with low stress and no breakage.
[0102] Figure 3 The SEM surface and cross-sectional images of the 2D porous sheet ZnIn2S4 / TiO2 / substrate thin film photocatalyst prepared in Example 3 of the present invention are shown in FIG. Figure 3 a is the surface map, Figure 3 b is a cross-sectional view; Figure 3 a As can be seen from the composite growth of indium zinc sulfide, a 2D porous sheet of indium zinc sulfide grows on the surface of the TiO2 / substrate film. The porous structure provides more active sites, which is beneficial to the improvement of its photocatalytic performance. Figure 3 b The layered structure of the film can be clearly seen. The bottom layer is the base plate, the middle layer is the TiO2 film, and the top layer is the 2D porous sheet indium zinc sulfide. It can be obtained that the thickness of the TiO2 film is 70nm, and the thickness of the 2D porous sheet indium zinc sulfide is 798nm. The thickness of the 2D porous sheet indium zinc sulfide is much higher than that of the TiO2 film, indicating that the TiO2 film can hold indium zinc sulfide very well, showing the importance of the TiO2 film.
[0103] Figure 4 TEM and mapping images of the 2D porous sheet ZnIn2S4 / TiO2 / substrate thin film photocatalyst prepared in Example 3 of the present invention, wherein Figure 4 a is the TEM image of 2D porous ZnIn2S4 / TiO2 / substrate thin film photocatalyst. Figure 4 bf are the element mapping diagrams of Zn, In, S, Ti and O of the 2D porous sheet ZnIn2S4 / TiO2 / substrate thin film photocatalyst; in order to see the heterojunction structure clearly, the film was scraped off for testing, and no ultrasonic treatment was performed during the test to avoid damaging the heterojunction. TEM images are shown in Figure 4 As shown in a, we can see that there are two parts in the figure, dark and light. After analysis, we can find that the darker part is indium zinc sulfide and the lighter part is titanium dioxide. Figure 4 A mapping test can be performed on the area of a Figure 4 bf, Figure 4bf are element mapping diagrams of Ti, O, Zn, In, and S, respectively. Figure 4 b and c can prove Figure 4 The lighter part in a is composed of Ti and O elements, indicating that this area is the scraped TiO2 / substrate film. Figure 4 As shown in df, the part that overlaps with titanium dioxide is composed of Zn, In, and S elements, indicating that this area is indium zinc sulfide. TEM and element mapping confirm the successful construction of the Z-type heterojunction of titanium dioxide and indium zinc sulfide. The heterojunction enables a strong coupling relationship between titanium dioxide and indium zinc sulfide. The band gap between the two materials can achieve energy complementarity, allowing the photogenerated carriers to be efficiently separated and transmitted at the interface, thereby improving the efficiency of the photocatalytic reaction.
[0104] Figure 5 It is the XRD spectrum of the TiO2 / substrate film and the 2D porous sheet ZnIn2S4 / TiO2 / substrate film photocatalyst prepared in Example 3 of the present invention; it can be found that using the thin film for testing will test the substrate, resulting in the measurement of a large area of amorphous phase peaks, which will have a serious impact on observation and analysis, but in the figure, the curve of the TiO2 / substrate film can still see the subtle characteristic peaks of rutile titanium dioxide (A-TiO2), and the curve of the 2D porous sheet ZnIn2S4 / TiO2 / substrate film photocatalyst can see the subtle characteristic peaks of rutile titanium dioxide (A-TiO2) and indium zinc sulfide (ZnIn2S4), however, the characteristic peak of indium zinc sulfide is not found on the curve of the TiO2 / substrate film, which proves the successful compounding of indium zinc sulfide and titanium dioxide in the 2D porous sheet ZnIn2S4 / TiO2 / substrate film photocatalyst.
[0105] Figure 6 The FTIR spectra of the TiO2 / substrate film and the 2D porous ZnIn2S4 / TiO2 / substrate film photocatalyst prepared in Example 3 of the present invention are shown in FIG. 3. The curve of the TiO2 / substrate film in the figure shows that 3420 cm -1 The peak at 1625 cm is related to the stretching vibration of the -OH group of the adsorbed water molecule, while the peak at 1625 cm -1 The peak at 923 cm -1 With 767cm -1 The peak at 554 cm is the characteristic peak of the glass substrate, and the peak at 554 cm -1 The peak is the stretching vibration peak of Ti-O. After the growth of 2D porous indium zinc sulfide sheets, a new peak of indium zinc sulfide appeared, 1424cm -1 The peak at is the peak of ZnIn2S4, which indicates that indium zinc sulfide is successfully grown on the TiO2 / substrate film, and these results are consistent with the XRD detection results.
[0106] Figure 7 This is the adsorption curve of RhB solution (50 mg / L, 100 ml) of the TiO2 / substrate film and 2D porous sheet ZnIn2S4 / TiO2 / substrate film photocatalyst prepared in Example 3 of the present invention. It can be seen that all films reach equilibrium after 60 minutes of adsorption. The adsorption rate of the TiO2 / substrate film is low, and the adsorption rate at 60 minutes is only 1.6%. The main reason is that the TiO2 / substrate film is very flat and has low roughness, and cannot provide more adsorption sites. The adsorption rate of the composite 2D porous sheet ZnIn2S4 / TiO2 / substrate film photocatalyst is greatly improved on the basis of the TiO2 / substrate film, and the 60-minute adsorption rate is 46.6%. This is mainly attributed to the 2D porous sheet indium zinc sulfide structure, indicating that the introduction of indium zinc sulfide has greatly improved the adsorption performance of the film.
[0107] Figure 8 The degradation curve of RhB solution (50mg / L, 100ml) of TiO2 / substrate film and 2D porous sheet ZnIn2S4 / TiO2 / substrate film photocatalyst prepared in Example 3 of the present invention is shown; it can be seen that the 2D porous sheet ZnIn2S4 / TiO2 / substrate film photocatalyst exhibits excellent photocatalytic performance. From the data, at 20 minutes, the degradation rate of TiO2 / substrate film is 6.2%, while the degradation rate of the composite 2D porous sheet ZnIn2S4 / TiO2 / substrate film photocatalyst is 69.1%. The degradation rate of RhB solution of 2D porous sheet ZnIn2S4 / TiO2 / substrate film photocatalyst at 70 minutes is 96.9%, while the degradation rate of TiO2 / substrate film at 70 minutes is only 15.7%, which further illustrates that indium zinc sulfide and titanium dioxide are successfully composited, and the photocatalytic performance is greatly improved.
[0108] Fig. 9This is the degradation curve of RhB solution of different concentrations of 2D porous sheet ZnIn2S4 / TiO2 / substrate thin film photocatalyst prepared in Example 3 of the present invention. The concentrations of RhB solution are 10mg / L, 20mg / L, 30mg / L, 40mg / L, and 50mg / L, respectively. As shown in the figure, after dark reaction and illumination for 20 minutes, the degradation rates of RhB solutions with concentrations of 10mg / L, 20mg / L, 30mg / L, 40mg / L, and 50mg / L are 99.4%, 94%, 84.9%, 77.5%, and 69.1%, respectively. After illumination for 70 minutes, the degradation rates of RhB solutions with concentrations of 10mg / L, 20mg / L, 30mg / L, 40mg / L, and 50mg / L are more than 99.9%, more than 99.9%, more than 99.9%, 98.9%, and 96.9%, respectively. When the concentration of RhB solution is low, it can be quickly removed by adsorption as well as degradation. For high concentration RhB solution, the removal rate by adsorption is relatively low, so the remaining RhB is only removed by photocatalytic degradation.
[0109] Fig.10 This is the degradation curve of MB solution (20mg / L, 100ml) of TiO2 / substrate film and 2D porous sheet ZnIn2S4 / TiO2 / substrate film photocatalyst prepared in Example 3 of the present invention. It can be seen that after 20 minutes of illumination, the degradation rate of TiO2 / substrate film is only 4.8%, while the degradation rate of 2D porous sheet ZnIn2S4 / TiO2 / substrate film photocatalyst is 88.9%. And using 2D porous sheet ZnIn2S4 / TiO2 / substrate film photocatalyst for degradation, after 80 minutes of illumination, the removal rate of MB by 2D porous sheet ZnIn2S4 / TiO2 / substrate film photocatalyst can reach more than 99.9%, while the removal rate of TiO2 / substrate film is only 18.9%, and the removal rate of 2D porous sheet ZnIn2S4 / TiO2 / substrate film photocatalyst is much higher than that of TiO2 / substrate film.
[0110] Fig.11This is the degradation curve of MO solution (20mg / L, 100ml) of TiO2 / substrate film and 2D porous sheet ZnIn2S4 / TiO2 / substrate film photocatalyst prepared in Example 3 of the present invention. It can be seen that after 20 minutes of illumination, the degradation rate of TiO2 / substrate film is only 2.4%, while the degradation rate of 2D porous sheet ZnIn2S4 / TiO2 / substrate film photocatalyst is 42.9%. And when using 2D porous sheet ZnIn2S4 / TiO2 / substrate film photocatalyst for degradation, at 80 minutes of illumination, the removal rate of MO is 80.1%, and the removal rate of TiO2 / substrate film is 8.4%. The removal rate of degradation using 2D porous sheet ZnIn2S4 / TiO2 / substrate film photocatalyst is much higher than that of TiO2 / substrate film.
[0111] Fig.12 The degradation curve of TC solution (50mg / L, 100ml) of TiO2 / substrate film and 2D porous sheet ZnIn2S4 / TiO2 / substrate film photocatalyst prepared in Example 3 of the present invention is shown. It can be seen that after 20 minutes of illumination, the degradation rate of TiO2 / substrate film is only 2.1%, while the degradation rate of 2D porous sheet ZnIn2S4 / TiO2 / substrate film photocatalyst is 41.8%. And when using 2D porous sheet ZnIn2S4 / TiO2 / substrate film photocatalyst for degradation, the removal rate of TC is 76.7% when the illumination is 80 minutes, and when using TiO2 / substrate film for degradation, the removal rate is only 6.9%, and the removal rate of 2D porous sheet ZnIn2S4 / TiO2 / substrate film photocatalyst is significantly improved compared with TiO2 / substrate film. According to the above results, it can be seen that the prepared composite film has excellent degradation performance for various organic pollutants.
[0112] The applicant also conducted the above-mentioned experiments on TiO2 / substrate thin films and 2D porous ZnIn2S4 / TiO2 / substrate thin film photocatalysts prepared in other embodiments and thin films prepared using different substrates. Figure 2-12 The experimental tests and analyses described herein yielded results comparable to those of the tests and analyses described above.
Claims
1. A thin film photocatalyst, characterized in that: A glass slide, FTO glass, ITO glass, ceramic sheet or PAN board is used as a substrate, and a TiO2 film is impregnated and pulled using titanium dioxide nanosol to obtain a TiO2 / substrate film. Indium zinc sulfide is hydrothermally crystallized and composited on the TiO2 / substrate film. Indium zinc sulfide grows on the TiO2 / substrate film to form a 2D porous sheet of indium zinc sulfide, thereby obtaining a 2D porous sheet ZnIn2S4 / TiO2 / substrate film photocatalyst.
2. The thin film photocatalyst according to claim 1, characterized in that: The thickness of the substrate is 50-200mm; the TiO2 / substrate film is titanium dioxide particles with 80-100 titanium dioxide particles spread on the substrate within an area of 100X100nm, the diameter of the titanium dioxide particles is 10-15nm, and the thickness of the TiO2 film is 50-200nm.
3. The thin film photocatalyst according to claim 1, characterized in that: The indium zinc sulfide grows vertically on the TiO2 / substrate film to form a 2D porous sheet indium zinc sulfide. The 2D porous sheet indium zinc sulfide is composed of arranged indium zinc sulfide holes and has a thickness of 700-800nm.
4. The method for preparing a thin film photocatalyst according to claim 1, characterized in that: The following steps are involved: (1) Add tetrabutyl titanate to anhydrous ethanol, then add glacial acetic acid, stir, and obtain product A; (2) Add deionized water to anhydrous ethanol, then add nitric acid to adjust the pH value, stir, and obtain product B; (3) Add product B to product A, stir, seal and age to obtain titanium dioxide nanosol, and obtain product C; (4) Impregnating product C with a substrate, pulling a thin film, drying, and calcining to obtain a TiO2 / substrate film, product D; (5) Indium chloride, zinc chloride, and thioacetamide are added to ethylene glycol and dissolved by ultrasonication to obtain an indium zinc sulfide precursor solution, which is product E; (6) Product D and product E are placed in a reactor for hydrothermal crystallization reaction, cooled, and vacuum dried to obtain a 2D porous sheet ZnIn2S4 / TiO2 / substrate thin film photocatalyst.
5. The method for preparing a thin film photocatalyst according to claim 4, characterized in that: In the step (1), 5-15 mL of tetrabutyl titanate is added to 15-30 mL of anhydrous ethanol, and then 1-2 mL of glacial acetic acid is added, and stirred for 20-30 minutes to obtain product A.
6. The method for preparing a thin film photocatalyst according to claim 4, characterized in that: In the step (2), 0.5-1.5 mL of deionized water is added to 10-20 mL of anhydrous ethanol, and then nitric acid is added to adjust the pH value to 1-4, and stirred for 5-15 minutes to obtain product B; in the step (3), 15-25 mL of product B is added to 30-50 mL of product A, stirred for 1.5-3 hours, sealed and aged for 5-60 hours to obtain titanium dioxide nanosol, and product C is obtained.
7. The method for preparing a thin film photocatalyst according to claim 4, characterized in that: In the step (4), the substrate is immersed in product C for 5-15 seconds, pulled upward at a speed of 0.1-0.5 mm / s, dried at 15-25°C for 10-20 minutes, then placed in a 40-80°C oven for drying for 10-50 minutes, and finally placed in a muffle furnace and heated to 400-550°C at a heating rate of 4-6°C / min and kept warm for 0.5-1.5 hours to obtain a TiO2 / substrate film, which is product D.
8. The method for preparing a thin film photocatalyst according to claim 4, characterized in that: In the step (5), 0.3-0.5 g of indium chloride, 0.1-0.15 g of zinc chloride, and 0.2-0.4 g of thioacetamide are added to 30-50 mL of ethylene glycol, and ultrasonically dissolved for 5-15 minutes to obtain an indium zinc sulfide precursor solution, which is product E.
9. The method for preparing a thin film photocatalyst according to claim 4, characterized in that: In the step (6), product D and product E are placed in a reaction kettle, hydrothermally crystallized at 100-200°C for 3-12 hours, cooled, and placed in a vacuum oven at 50-70°C for vacuum drying for 18-24 hours to obtain a 2D porous sheet ZnIn2S4 / TiO2 / substrate plate thin film photocatalyst.
10. The use of the thin film photocatalyst according to any one of claims 1 to 9, characterized in that: The 2D porous sheet ZnIn2S4 / TiO2 / substrate thin film photocatalyst is used for photocatalytic degradation of rhodamine B, methyl orange, methylene blue and tetracycline hydrochloride.
Citation Information
Patent Citations
Preparation method for nano-titanium dioxide film photocatalyst
CN101367035A
Method for preparing titanium dioxide nano-semiconductor photocatalysis film
CN105771949A
Preparation method of zinc indium sulfide nanosheet array film
CN109052988A