Preparation method of spinous spherical nano nickel powder
By configuring nickel salt and sodium hydroxide solutions under low temperature conditions, and adding surfactants and reducing agents, nanoscale spiny spherical nickel powder is prepared, which solves the problems of uneven particle size and high equipment requirements in the existing technology, and achieves Efficient and low-cost preparation of nano-nickel powder is achieved, which is suitable for applications in many fields.
Patent Information
- Application Number
- CN202411248740.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-09-06
AI Technical Summary
It is difficult to prepare nano-scale spiny spherical nickel powder with the existing technology. The particle size distribution is uneven, and the nickel carbonyl used is a highly toxic substance. It requires high equipment and is difficult to control, and cannot meet the needs of industrial production.
By configuring nickel aqueous salt solution and sodium hydroxide aqueous solution, adding surfactant and reducing agent, and performing preheating and heating reactions, spinous spherical nano-nickel powder with a large specific surface area is prepared, with a particle size between 100-300 nm, using Simple equipment and low temperature conditions.
It achieves the preparation of nanoscale spiny spherical nickel powder with high purity, uniform particle size and large specific surface area, overcomes the problem of low efficiency in high temperature and high pressure environments, is suitable for industrial mass production, and is suitable for antistatic and electromagnetic shielding materials.
Smart Images

Figure CN118847985A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nano material preparation, and in particular to a method for preparing thorn-shaped spherical nano nickel powder. Background Art
[0002] Nano nickel powder has small size and large specific surface area. It has performance advantages such as efficient photocatalysis, high conductivity and magnetic properties. Nano nickel particles also have excellent conductivity, good stability, low sintering temperature and other characteristics. It plays an important role in many fields such as electronics, chemical industry, environmental protection and energy, and can be used for electromagnetic shielding materials, wave absorbing materials and multilayer ceramic capacitors. The application field of nano nickel powder is closely related to its morphology. Studies have found that nano nickel powder used as a catalyst requires a regular spherical structure so that it can fully contact with the material, thus having excellent catalytic performance. However, spherical nano nickel powder has a smooth particle surface and a small specific surface area. The specific surface area of spherical nano nickel powder used in multilayer ceramic capacitors (MLCC) currently required by the industry is about 3.1-4.35 m² / g, and there are still restrictions on nano nickel powders with larger specific surface areas.
[0003] Although nano nickel powders with other morphologies have been less studied, they also have many uses. For example, nano nickel powders with branched structures can provide more reaction sites on amorphous surfaces and are more suitable for use as electrode materials for alkaline fuel cells. Petal-shaped nano nickel powders are thin but have excellent wave absorbing properties and can be used in small and efficient absorbers. Han Baozhong's team studied the variation of the resistivity of silicone rubber composites filled with nickel powders of different dosages and shapes with tensile strain and found that silicone rubber composites doped with thorn-shaped spherical nickel powders have significant tensile sensitivity. Therefore, the development of nano nickel powders with different morphologies can expand the application areas of nano nickel powders.
[0004] Chinese invention patent CN 1817527A discloses a method for preparing thorn-shaped spherical nickel powder, which uses carbonyl nickel thermal decomposition method to form a mixed gas with carbonyl nickel vapor and carbon monoxide gas, and passes the mixed gas through six different temperature zones. When heated, it decomposes to generate metallic nickel. The surface of the nickel powder prepared by the invention is covered with needle thorns and the particle size is 0.5-12 μm.
[0005] However, the above-mentioned prior art can only produce micron-level thorn-shaped spherical nickel powder, and the particle size distribution is uneven. At the same time, carbonyl nickel is a highly toxic substance, and the equipment requirements are high and the control is difficult. Therefore, it is still a technical problem to be solved to prepare nano-level thorn-shaped spherical nickel powder by a preparation method that is simple to operate, has low equipment requirements and controllable morphology. Summary of the invention
[0006] In order to overcome the above disadvantages, the present invention aims to provide a method for preparing thorn-shaped spherical nano-nickel powder, which is simple in preparation method, has low equipment requirements, and can produce thorn-shaped spherical nano-nickel powder with larger specific surface area. In order to achieve the above object, the technical solution adopted by the present invention is: a method for preparing thorn-shaped spherical nano nickel powder, comprising the following steps: S1, preparing a nickel salt aqueous solution, adding a surfactant to the nickel salt aqueous solution, stirring and mixing, to obtain a solution A; S2, prepare a sodium hydroxide aqueous solution, add a reducing agent to the sodium hydroxide aqueous solution, stir and mix, and obtain a solution B; S3, preheating solution A and solution B respectively, adding solution B into solution A after reaching the preheating temperature, heating for reaction, and post-processing to obtain thorn-like spherical nano nickel powder.
[0007] Further, in S1, the nickel salt aqueous solution is a nickel chloride aqueous solution, and the concentration of the nickel salt aqueous solution is 0.1-0.4 mol / L. Exemplarily, the concentration of the nickel salt aqueous solution is 0.1 mol / L, 0.2 mol / L, 0.3 mol / L, 0.4 mol / L or a range consisting of any two thereof.
[0008] Furthermore, in S1, the surfactant is polyvinyl pyrrolidone.
[0009] Further, in S1, the mass ratio of the added amount of the surfactant to the nickel salt is 1:(2.5-8.1). Exemplarily, the mass ratio of the added amount of the surfactant to the nickel salt is 1:2.5, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:8.1 or a range consisting of any two of them.
[0010] Further, in S2, the concentration of the sodium hydroxide aqueous solution is 0.6-1.4 mol / L. Exemplarily, the concentration of the sodium hydroxide aqueous solution is 0.6 mol / L, 0.8 mol / L, 1.0 mol / L, 1.2 mol / L, 1.4 mol / L or a range consisting of any two thereof.
[0011] Furthermore, in S2, the reducing agent is hydrazine hydrate, and the mass percentage concentration of the reducing agent is 80%.
[0012] Further, in S2, the reducing agent concentration in the configured solution B is 0.5-1.97 mol / L. Exemplarily, the reducing agent concentration in the configured solution B is 0.5 mol / L, 1 mol / L, 1.5 mol / L, 1.97 mol / L, or a range consisting of any two thereof.
[0013] Furthermore, in S3, the preheating temperature is 70-90°C, the heating temperature is 70-90°C, and the heating time is 2-4 h.
[0014] Furthermore, in S3, the post-treatment step includes: pouring off the supernatant, washing the crude product with water until the conductivity drops below 5 μs / cm, then washing with ethanol, and drying in a vacuum drying oven.
[0015] Furthermore, in S3, the obtained thorn-like spherical nano nickel powder has a particle size of 100-300 nm.
[0016] The beneficial effects of the present invention are: 1) The preparation method of the present invention prepares nano-grade nickel powder at normal pressure and relatively low temperature by separately preparing a nickel salt solution and a reducing solution, and preheating them separately, and then mixing and heating them. The equipment requirements are low, the operation steps are simple, and the operability is strong.
[0017] 2) This preparation method does not add a complexing agent, but through the screening and concentration control of nickel salt solution, alkali solution, reducing agent and other materials, a thorn-shaped nano nickel powder with a large specific surface area is prepared under a simple preparation method. It overcomes the problems of high temperature and high pressure environment, high energy consumption, low efficiency and unsuitability for large-scale industrial production in the current commonly used technology.
[0018] 3) The thorn-like spherical nickel nanoparticles prepared by the method of the present invention have the characteristics of small size, narrow particle size distribution range, high purity and large specific surface area. They provide conductive fillers for optimizing the performance of antistatic materials and electromagnetic shielding materials and are widely used in aerospace, construction, medical food and other fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] The drawings constituting a part of this application are used to provide a further understanding of the present invention. The illustrative embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0020] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0021] Figure 1 SEM image of the thorn-like spherical nickel nanopowder prepared in Example 1 (*40000); Figure 2 SEM image of the thorn-like spherical nickel nanopowder prepared in Example 1 (*8000); Figure 3SEM image of the thorn-like spherical nickel nanopowder prepared in Example 2 (*40000); Figure 4 SEM image of the thorn-like spherical nickel nanopowder prepared in Example 2 (*8000); Figure 5 SEM image of the thorn-like spherical nickel nanopowder prepared in Example 3 (*40000); Figure 6 SEM image of the thorn-like spherical nickel nanopowder prepared in Example 3 (*8000); Figure 7 SEM image of the thorn-like spherical nickel nanopowder prepared in Comparative Example 1 (*40000); Figure 8 SEM image of the thorn-like spherical nickel nanopowder prepared in Comparative Example 1 (*8000); Fig. 9 SEM image of the thorn-like spherical nickel nanopowder prepared in Comparative Example 2 (*50000); Fig.10 SEM image of the thorn-like spherical nickel nanopowder prepared in Comparative Example 2 (*8000); Fig.11 SEM image of the thorn-like spherical nickel nanopowder prepared in Comparative Example 3 (*100000); Fig.12 SEM image of the thorn-like spherical nickel nanopowder prepared in Comparative Example 3 (*8000); Fig.13 SEM image of the thorn-like spherical nickel nanopowder prepared in Comparative Example 4 (*40000); Fig.14 SEM image of the thorn-like spherical nickel nanopowder prepared in Comparative Example 4 (*8000). DETAILED DESCRIPTION
[0022] In order to make the above-mentioned purpose, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below.
[0023] Except as shown in the operating examples or otherwise indicated, all numbers used in the specification and claims to indicate the amount of ingredients, physicochemical properties, etc. are understood to be adjusted by the term "about" in all cases. Therefore, unless otherwise indicated, the numerical parameters listed in the above specification and the attached claims are approximate values, and those skilled in the art can use the teachings disclosed herein to seek to obtain the desired properties and appropriately change these approximate values. The use of numerical ranges expressed as endpoints includes all numbers within the range and any range within the range, for example, 1 to 5 includes 1, 1.1, 1.3, 1.5, 2, 2.75, 3, 3.80, 4 and 5, etc.
[0024] The applicant found that the existing technology can only produce micron-level thorn-shaped spherical nickel powder, and the particle size distribution is uneven. At the same time, the carbonyl nickel used is a highly toxic substance, which requires high equipment and is difficult to control. The production of nano-level thorn-shaped nickel powder still requires a preparation method that is simple to operate, has low equipment requirements and can control the morphology. Therefore, it is of great significance to explore the industrial production of nano-level nickel powder products with high purity, dispersion, uniform particle size distribution and thorn-shaped spherical structure. An embodiment of the present invention provides a method for preparing thorn-shaped spherical nano nickel powder to solve the above problem, which specifically comprises the following steps: S1. Prepare a nickel chloride aqueous solution with a concentration of 0.1-0.4 mol / L, add a surfactant polyvinyl pyrrolidone to the nickel chloride aqueous solution, stir and mix, and obtain solution A; wherein the mass ratio of the added amount of the surfactant to the nickel salt is 1:(2.5-8.1).
[0025] S2. Prepare a sodium hydroxide aqueous solution with a concentration of 0.6-1.4 mol / L, add a reducing agent hydrazine hydrate with a mass percentage concentration of 80% to the sodium hydroxide aqueous solution, stir and mix, and obtain a solution B; the reducing agent concentration in the prepared solution B is 0.5-1.97 mol / L.
[0026] S3, preheating solution A and solution B respectively, the preheating temperature is 70-90°C, and after reaching the preheating temperature, solution B is added to solution A, and heated to react, the heating temperature is 70-90°C, and the heating time is 2-4 hours. Post-treatment obtains thorn-shaped spherical nano-nickel powder, and the particle size of the thorn-shaped spherical nano-nickel powder is 100-300 nm.
[0027] The post-treatment steps include: pouring off the supernatant, washing the crude product with water until the conductivity drops below 5 μs / cm, then washing with ethanol, and drying in a vacuum drying oven.
[0028] Example The following examples describe the disclosure of the present invention in more detail, and these examples are intended for illustrative purposes only, as various modifications and variations within the scope of the disclosure of the present invention will be apparent to those skilled in the art. Unless otherwise stated, all parts, percentages, and ratios reported in the following examples are by weight, and all reagents used in the examples are commercially available or synthesized according to conventional methods and can be used directly without further processing, and the instruments used in the examples are commercially available.
[0029] Example 1 A method for preparing thorn-shaped spherical nickel nanoparticles comprises the following steps: S1. Dissolve 0.4 mol NiCl2·6H2O (237.7*0.4=95.08 g) in 1000 g water and mix evenly, then add 17.6 g polyvinylpyrrolidone PVP and stir evenly to obtain solution A; wherein the mass ratio of the added amount of the surfactant to the nickel salt is 17.6:95.08=1:5.4.
[0030] S2. Dissolve 0.6 mol NaOH in 1000 g water and mix evenly, then add 0.9 mol hydrazine hydrate with a mass fraction of 80% and stir evenly to obtain solution B.
[0031] S3, preheating solution A and solution B in a water bath, and after reaching the preheating temperature of 80°C, using a peristaltic pump to pump solution B into solution A at a pumping speed of 40 mL / min, and mixing and stirring for 3 h using a stirring paddle, while maintaining the temperature at 80°C, to obtain solution C, and placing solution C in a water bath at 80°C for heating and reaction for 3 h, and cooling to room temperature (25°C) after the reaction is completed; The supernatant was discarded, and the crude product was first washed with water until the conductivity dropped below 5μs / cm, then washed twice with ethanol, and dried in a vacuum drying oven at 60°C for 12 h to obtain thorn-shaped spherical nano-nickel powder with a particle size of about 100-300 nm. Figure 1 and attached Figure 2 As shown, it can be seen that the prepared nickel powder has uniform particle size and good dispersibility.
[0032] Example 2 A method for preparing thorn-shaped spherical nickel nanoparticles comprises the following steps: S1. Dissolve 0.6 mol of NiCl2·6H2O (237.7*0.6=142.62 g) in 1000 g of water and mix evenly, then add 52.8 g of PVP and stir evenly to obtain solution A; wherein the mass ratio of the added amount of the surfactant to the nickel salt is 52.8:142.62=1:2.7.
[0033] S2, 1.2 mol of NaOH was dissolved in 1000 g of water and mixed evenly, and then 1.35 mol of 80% mass fraction of hydrazine hydrate was added and stirred to obtain solution B; S3, preheating solution A and solution B in a water bath, respectively, and after reaching the preheating temperature of 80°C, using a peristaltic pump to pump solution B into solution A at a pumping speed of 40 mL / min, using a stirring paddle to mix and stir for 3 h, maintaining the temperature at 80°C during stirring, to obtain solution C, placing solution C in a water bath at 80°C for heating reaction for 3 h, and cooling to room temperature (25°C) after the reaction is completed; The supernatant was discarded, and the crude product was first washed with water until the conductivity dropped below 5μs / cm, then washed twice with ethanol, and dried in a vacuum drying oven at 60°C for 12 h to obtain thorn-shaped spherical nano-nickel powder with a particle size of about 200-300 nm. Figure 3 and attached Figure 4 As shown, it can be seen that the prepared nickel powder has uniform particle size and good dispersibility.
[0034] Example 3 A method for preparing thorn-shaped spherical nickel nanoparticles comprises the following steps: S1. Dissolve 0.8 mol NiCl2·6H2O (237.7*0.8=190.16 g) in 1000 g water and mix evenly, then add 35.2 g PVP and stir evenly to obtain solution A; wherein the mass ratio of the added amount of the surfactant to the nickel salt is 35.2:190.16=1:5.4.
[0035] S2, 1.2 mol NaOH was dissolved in 1000 g of water and mixed evenly, and then 1.8 mol of 80% mass fraction of hydrazine hydrate was added and stirred to obtain solution B; S3, preheating solution A and solution B in a water bath, and after reaching the preheating temperature of 80°C, using a peristaltic pump to pump solution B into solution A at a pumping speed of 40 mL / min, and mixing and stirring for 3 h using a stirring paddle, while maintaining the temperature at 80°C, to obtain solution C, and placing solution C in a water bath at 80°C for heating and reaction for 3 h, and cooling to room temperature (25°C) after the reaction is completed; The supernatant was discarded, and the crude product was first washed with water until the conductivity dropped below 5 μs / cm, then washed twice with ethanol, and dried in a vacuum drying oven at 60°C for 12 h to obtain thorny spherical nano-nickel powder with a particle size of about 100-200 nm.
[0036] From the attached Figure 5 and attached Figure 6As shown in the figure, it can be seen that the prepared nickel powder has uniform particle size and good dispersibility. The BET measured by the specific surface area tester is 12.87 m² / g.
[0037] Comparative Example 1 S1. Dissolve 0.5 mol NiCl2·6H2O (237.7*0.5=118.85 g) in 1000 g water and mix evenly. Then add 20 g PVP and stir evenly to obtain solution A. S2, 1.5 mol NaOH was dissolved in 1000 g of water and mixed evenly, and then 2 mol mass fraction of 80% hydrazine hydrate was added and stirred to obtain solution B; S3, preheating solution A and solution B in a water bath, and after reaching the preheating temperature of 80°C, using a peristaltic pump to pump solution B into solution A at a pumping speed of 40 mL / min, and mixing and stirring for 3 h using a stirring paddle, while maintaining the temperature at 80°C, to obtain solution C, and placing solution C in a water bath at 80°C for heating and reaction for 3 h, and cooling to room temperature (25°C) after the reaction is completed; The supernatant was discarded, and the crude product was first washed with water until the conductivity dropped below 5 μs / cm, then washed twice with ethanol, and dried in a vacuum drying oven at 60°C for 12 h to obtain nano nickel powder.
[0038] See attached Figure 7 and attached Figure 8 As shown, in Comparative Example 1, the concentration of the nickel salt aqueous solution used is 0.5 mol / L, the concentration of the sodium hydroxide aqueous solution is 1.5 mol / L, and the prepared nickel powder is a large-particle-size nearly spherical nano nickel powder with a particle size of about 500-700 nm, and the particles are severely agglomerated. Therefore, when the concentration of the nickel salt aqueous solution is controlled at 0.4 mol / L or less, and the concentration of the sodium hydroxide aqueous solution is controlled at 1.4 mol / L or less, the prepared nickel powder is a nano-scale thorn-shaped spherical nickel powder.
[0039] Comparative Example 2 S1. Dissolve 0.05 mol NiCl2·6H2O in 1000 g water and mix evenly, then add 4 g PVP and stir evenly to obtain solution A; S2, 0.7 mol NaOH was dissolved in 1000 g of water and mixed evenly, and then 0.5 mol mass fraction of 80% hydrazine hydrate was added and stirred to obtain solution B; S3, preheating solution A and solution B in a water bath, and after reaching the preheating temperature of 80°C, using a peristaltic pump to pump solution B into solution A at a pumping speed of 40 mL / min, and mixing and stirring for 3 h using a stirring paddle, while maintaining the temperature at 80°C, to obtain solution C, and placing solution C in a water bath at 80°C for heating and reaction for 3 h, and cooling to room temperature (25°C) after the reaction is completed; The supernatant was discarded, and the crude product was first washed with water until the conductivity dropped below 5 μs / cm, then washed twice with ethanol, and dried in a vacuum drying oven at 60°C for 12 h. This resulted in inferior nano-nickel powder.
[0040] See attached Fig. 9 and attached Fig.10 As shown, in Comparative Example 2, the concentration of the nickel salt aqueous solution used is 0.05 mol / L, and a poor nano nickel powder is obtained, and the particles are seriously agglomerated. It may be that the nickel salt concentration is low, the reducing agent is high relative to the nickel salt concentration, the reaction is too fast, and a large amount of nickel powder crystals are generated at the same time, which are easy to grow together and agglomerate. Therefore, it is appropriate to control the concentration of the nickel salt aqueous solution in this scheme to be 0.1 mol / L-0.4 mol / L.
[0041] Comparison 3 S1. Dissolve 0.2 mol NiCl2·6H2O (0.2*237.7=47.54 g) in 1000 g water and mix evenly. Then add 8 g PVP and stir evenly to obtain solution A. S2, 0.3 mol NaOH was dissolved in 1000 g of water and mixed evenly, and then 0.5 mol mass fraction of 80% hydrazine hydrate was added and stirred to obtain solution B; S3, preheating solution A and solution B in a water bath, and after reaching the preheating temperature of 80°C, using a peristaltic pump to pump solution B into solution A at a pumping speed of 40 mL / min, and mixing and stirring for 3 h using a stirring paddle, while maintaining the temperature at 80°C, to obtain solution C, and placing solution C in a water bath at 80°C for heating and reaction for 3 h, and cooling to room temperature (25°C) after the reaction is completed; The supernatant was discarded and the crude product was washed with water until the conductivity dropped below 5 μs / cm, then washed twice with ethanol and dried in a vacuum drying oven at 60°C for 12 h to obtain inferior nickel powder with a particle size of about 100~500nm and severe agglomeration.
[0042] See attached Fig.11 and attached Fig.12As shown, in Comparative Example 3, the concentration of the NaOH solution used was 0.3 mol / L, and poor nano nickel powder was obtained, and the particles were seriously agglomerated. It may be that the concentration of the NaOH solution is low, the reducing agent is relatively high, the reaction is too fast, a large number of nickel powder crystals are generated at the same time, and they are easy to grow together and agglomerate. Therefore, the concentration of the sodium hydroxide aqueous solution in this scheme is preferably controlled at 0.6 mol / L-1.4 mol / L.
[0043] Comparative Example 4 A method for preparing thorn-shaped spherical nickel nanoparticles comprises the following steps: S1. Dissolve 0.4 mol NiCl2·6H2O (237.7*0.4=95.08 g) in 1000 g water and mix evenly, then add 17.6 g polyvinylpyrrolidone PVP and stir evenly to obtain solution A; wherein the mass ratio of the added amount of the surfactant to the nickel salt is 17.6:95.08=1:5.4.
[0044] S2. Dissolve 0.6 mol NaOH in 1000 g water and mix evenly, then add 0.9 mol hydrazine hydrate with a mass fraction of 80% and stir evenly to obtain solution B.
[0045] S3, using a peristaltic pump to pump solution B into solution A at a pumping speed of 40 mL / min, mixing and stirring with a stirring paddle at 80°C for 3 h to obtain solution C, placing solution C in an 80°C water bath for heating and reaction for 3 h, and cooling to room temperature (25°C) after the reaction; The supernatant was discarded, and the crude product was first washed with water until the conductivity dropped below 5 μs / cm, then washed twice with ethanol, and dried in a vacuum drying oven at 60°C for 12 h to obtain a spherical shape with less obvious thorns on the surface, rather than a spherical shape with a rough surface (see Appendix Fig.13 and attached Fig.14 As shown). Therefore, in the process of preparing the thorn-like spherical nickel nanoparticles, solution A and solution B need to be preheated and then mixed.
[0046] The above implementation modes are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the content of the present invention and implement it, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing thorn-shaped spherical nano nickel powder, characterized in that: The steps include: S1, preparing a nickel salt aqueous solution, adding a surfactant to the nickel salt aqueous solution, stirring and mixing, to obtain a solution A; S2, prepare a sodium hydroxide aqueous solution, add a reducing agent to the sodium hydroxide aqueous solution, stir and mix, and obtain a solution B; S3, preheating solution A and solution B respectively, adding solution B into solution A after reaching the preheating temperature, heating for reaction, and post-processing to obtain thorn-like spherical nano nickel powder.
2. The method for preparing the thorny spherical nickel nanopowder according to claim 1, characterized in that: In S1, the nickel salt aqueous solution is a nickel chloride aqueous solution, and the concentration of the nickel salt aqueous solution is 0.1-0.4 mol / L.
3. The method for preparing the thorn-like spherical nickel nanopowder according to claim 1, characterized in that: In S1, the surfactant is polyvinyl pyrrolidone.
4. The method for preparing the thorny spherical nickel nanopowder according to claim 1, characterized in that: In S1, the mass ratio of the added amount of the surfactant to the nickel salt is 1:(2.5~8.1).
5. The method for preparing the thorn-like spherical nickel nanopowder according to claim 1, characterized in that: In S2, the concentration of the sodium hydroxide aqueous solution is 0.6-1.4 mol / L.
6. The method for preparing the thorn-like spherical nickel nanopowder according to claim 1, characterized in that: In S2, the reducing agent is hydrazine hydrate, and the mass percentage concentration of the reducing agent is 80%.
7. The method for preparing the thorn-like spherical nickel nanopowder according to claim 1, characterized in that: In S2, the reducing agent concentration in the prepared solution B is 0.5-1.97 mol / L.
8. The method for preparing the thorn-like spherical nickel nanopowder according to claim 1, characterized in that: In S3, the preheating temperature is 70-90°C, the heating temperature is 70-90°C, and the heating time is 2-4 h.
9. The method for preparing the thorn-like spherical nickel nanopowder according to claim 1, characterized in that: In S3, the post-treatment step includes: pouring off the supernatant, washing the crude product with water until the conductivity drops below 5 μs / cm, then washing with ethanol, and drying in a vacuum drying oven.
10. The method for preparing the thorn-like spherical nickel nanopowder according to claim 1, characterized in that: In S3, the particle size of the thorn-like spherical nickel nanopowder is 100-300 nm.
Citation Information
Patent Citations
Method for preparing spherical submicron nickel powder with controllable particle size
CN102554259A
Method for preparing superfine nickel powder through liquid phase reduction
CN110976905A
Method of preparing nano metal nickel powder
CN1426865A
Nano structure nickel powde and its preparing method
CN1586773A
Production for nanometer nickel powder
CN1644282A