Preparation method of tungsten-silicon target material

Through the compaction molding and static pressure treatment of tungsten-silicon alloy raw materials, the oxygen content and uniformity problems in the existing technology are solved, the preparation of tungsten-silicon targets with high density and low oxygen content is achieved, and impurities and agglomeration are avoided.

CN118847993APending Publication Date: 2024-10-29KONFOONG MATERIALS INTERNATIONAL CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410934629.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

The existing tungsten-silicon target preparation method cannot effectively control the oxygen content and microstructure uniformity, and is easy to introduce impurities and alloy phases or elemental silicon agglomeration, and cannot meet the requirements of high density and low gas content.

Method used

Tungsten-silicon alloy raw materials are used to tamp the mold, cold isostatic pressing and hot isostatic pressing. The molding process is controlled through multiple pressure boosting and pressure holding steps to avoid delamination and cracking, improve the density, and use hot isostatic pressing. Pressure treatment controls the size of alloy phase grains and elemental silicon to ensure the uniformity of the target material.

Benefits of technology

It achieves low oxygen content (≤300ppm), high density (≥98%) and uniform microstructure of the target material, avoids the agglomeration of alloy phase and elemental silicon, and improves the performance of the target material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004940913990000111
    Figure BDA0004940913990000111
  • Figure BDA0004940913990000121
    Figure BDA0004940913990000121
Patent Text Reader

Abstract

The invention relates to a preparation method of a tungsten-silicon target material, which comprises the following steps: (1) sequentially carrying out tamping and die filling, cold isostatic pressing treatment and machining on a tungsten-silicon alloy raw material to obtain an ingot material; the cold isostatic pressing treatment comprises first pressure boosting, first pressure maintaining, second pressure boosting, second pressure maintaining, third pressure boosting and third pressure maintaining which are carried out in sequence; (2) sequentially carrying out sheath assembly, welding, degassing and hot isostatic pressing treatment on the ingot material obtained in the step (1) to obtain a tungsten-silicon target material; the hot isostatic pressing treatment comprises first heating, second heating and first heat preservation which are sequentially carried out. According to the preparation method provided by the invention, introduction of metal and nonmetal impurities can be avoided, the oxygen content of the target material is reduced, the microstructure uniformity and compactness of the target material are improved, and monatomic silicon agglomeration is avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of target material preparation, and in particular to a method for preparing a tungsten silicon target material. Background Art

[0002] Tungsten silicon thin films are usually used as gate contact layers, barrier layers or adhesion layers in integrated circuits, especially in the storage field. At present, the commonly used thin film preparation methods mainly include physical vapor deposition (magnetron sputtering) and chemical vapor deposition (CVD). Among them, the main method for obtaining tungsten silicon thin films in the semiconductor field is magnetron sputtering, which can be divided into three methods according to the different sputtering sources: (1) single target sputtering, that is, using a high-purity tungsten target as a sputtering source to obtain a tungsten film on a silicon substrate, and then obtaining a tungsten silicon film by heat treatment; (2) dual target sputtering, that is, by alternately or simultaneously sputtering a single tungsten target and a single silicon target and then combining a heat treatment process to obtain a tungsten silicon film; (3) alloy target sputtering, that is, using an alloy target as a sputtering source to obtain a tungsten silicon film. Compared with the other two sputtering methods, the alloy target sputtering method has a more controllable film, a higher gradient coverage, and fewer sputtered particles. It is currently the mainstream method for obtaining tungsten silicon thin films. However, this method has high requirements on the physical and chemical properties of the target material, requiring the target material to have high density (≥99.5%), high purity (≥99.999%) and low gas content (O≤500ppm).

[0003] At present, tungsten silicon targets are mainly obtained by powder metallurgy, that is, mixing tungsten powder and silicon powder and then hot pressing and sintering. However, since the oxygen content of silicon powder on the market is generally ≥4500ppm, it cannot meet the requirements of tungsten silicon targets for sputtering.

[0004] For example, CN113981387A discloses a method for preparing a tungsten silicon target, comprising: (1) subjecting tungsten powder and silicon powder to a first heat treatment to obtain a tungsten silicon alloy; (2) crushing the tungsten silicon alloy obtained in step (1) to obtain a tungsten silicon alloy powder; (3) subjecting the tungsten silicon alloy powder obtained in step (2) to a second heat treatment to obtain a tungsten silicon target. The above preparation method cannot effectively control the oxygen content in the tungsten silicon target, and there is a phenomenon of uneven distribution of the alloy phase and elemental silicon.

[0005] CN103695852A discloses a method for manufacturing a tungsten silicon target, including: providing high-purity tungsten powder and high-purity silicon powder; mixing the tungsten powder and the silicon powder by a wet mixing process to form a mixed powder; cold pressing the mixed powder to form a tungsten silicon target blank; and vacuum hot pressing the tungsten silicon target blank to form a tungsten silicon target. This manufacturing method is prone to introduce impurities during the powder mixing process, and drying and crushing after the powder is wet mixed is prone to destroy the uniformity of the powder, which is not conducive to the control of the uniformity of the microstructure of the final product.

[0006] Therefore, it is of great significance to provide a method for preparing a tungsten silicon target material that can improve the uniformity and density of the target material microstructure, reduce the oxygen content, and avoid the agglomeration of elemental silicon. Summary of the invention

[0007] In view of the above problems, the purpose of the present invention is to provide a method for preparing a tungsten silicon target. Compared with the prior art, the preparation method provided by the present invention can avoid the introduction of metal and non-metal impurities, reduce the oxygen content of the target, improve the microstructure uniformity and density of the target, and avoid the agglomeration of alloy phase or elemental silicon.

[0008] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0009] The present invention provides a method for preparing a tungsten silicon target material, the preparation method comprising the following steps:

[0010] (1) subjecting the tungsten silicon alloy raw material to compaction, cold isostatic pressing and machining in sequence to obtain an ingot;

[0011] The cold isostatic pressing treatment includes a first pressurization, a first pressure holding, a second pressurization, a second pressure holding, a third pressurization and a third pressure holding performed in sequence;

[0012] (2) subjecting the ingot obtained in step (1) to packaging, welding, degassing and hot isostatic pressing in sequence to obtain a tungsten silicon target;

[0013] The hot isostatic pressing treatment includes a first heating, a second heating and a first heat preservation performed in sequence.

[0014] In the preparation method provided by the present invention, on the one hand, using tungsten silicon alloy as a raw material can avoid the powder mixing process required for using silicon powder and tungsten powder, avoid the introduction of impurities during powder mixing, and thus reduce the oxygen content; on the one hand, by controlling the first pressure increase, the second pressure holding, the second pressure increase, the second pressure holding, the third pressure increase and the third pressure holding in sequence during the cold isostatic pressing process, the molding process of the alloy powder can be controlled to avoid stratification and cracking; on the other hand, by controlling the first temperature increase, the second temperature increase and the first temperature holding in sequence during the hot isostatic pressing process, the moldability of the target material can be further controlled, the density of the target material can be improved, and the grain size of the alloy phase can be avoided to be too large to agglomerate with elemental silicon, thereby improving the uniformity of the tungsten silicon target material.

[0015] Preferably, the particle size of the tungsten silicon alloy raw material in step (1) is 0.8-10 μm, for example, it can be 0.8 μm, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm or 10 μm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0016] In the present invention, the particle size of the tungsten-silicon alloy raw material is preferably controlled within a specific range, which can further improve the compactness of the tungsten-silicon target material and avoid agglomeration of elemental silicon.

[0017] Preferably, the mass percentage of silicon in the tungsten silicon alloy raw material is 28.5-29.5%, for example, it can be 28.5%, 28.6%, 28.8%, 29%, 29.2%, 29.4% or 29.5%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0018] Preferably, the purity of the tungsten silicon alloy raw material is ≥99.999wt%, for example, it can be 99.9991wt%, 99.9992wt%, 99.9993wt% or 99.9994wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0019] Preferably, the flatness after compaction and molding in step (1) is less than 1 mm, for example, it can be 0.9 mm, 0.8 mm, 0.7 mm, 0.6 mm, 0.5 mm, 0.4 mm, 0.3 mm, 0.2 mm or 0.1 mm, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0020] Preferably, the density after compaction and molding is ≥30%, for example, it can be 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39% or 40%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0021] In the present invention, the mold for molding generally adopts a rubber sleeve.

[0022] Preferably, the first pressurization rate in step (1) is 9-10 MPa / min, for example, 9 MPa / min, 9.2 MPa / min, 9.4 MPa / min, 9.6 MPa / min, 9.8 MPa / min or 10 MPa / min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0023] Preferably, the endpoint pressure of the first pressurization is 90-110 MPa, for example, it can be 90 MPa, 92 MPa, 94 MPa, 96 MPa, 98 MPa, 100 MPa, 102 MPa, 104 MPa, 106 MPa, 108 MPa or 110 MPa, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0024] In the present invention, it is preferred to control the endpoint pressure of the first pressurization to be within a specific range, which can further improve the density of the blank and prevent the blank from cracking when demolding.

[0025] Preferably, the first pressure holding time is 5-6 minutes, for example, it can be 5 minutes, 5.2 minutes, 5.4 minutes, 5.6 minutes, 5.8 minutes or 6 minutes, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0026] Preferably, the second boost rate is 4-5 MPa / min, for example, 4 MPa / min, 4.2 MPa / min, 4.4 MPa / min, 4.6 MPa / min, 4.8 MPa / min or 5 MPa / min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0027] Preferably, the endpoint pressure of the second pressurization is 170-190 MPa, for example, it can be 170 MPa, 172 MPa, 174 MPa, 176 MPa, 178 MPa, 180 MPa, 182 MPa, 184 MPa, 186 MPa, 188 MPa or 190 MPa, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0028] In the present invention, it is preferred to control the endpoint pressure of the second pressurization to be within a specific range, which can further improve the density of the blank and prevent the blank from cracking when demolding.

[0029] Preferably, the second pressure holding time is 5-30 min, for example, it can be 5 min, 6 min, 8 min, 10 min, 12 min, 14 min, 16 min, 18 min, 20 min, 22 min, 24 min, 26 min, 28 min or 30 min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0030] Preferably, the third boost rate is 2-3 MPa / min, for example, it can be 2 MPa / min, 2.2 MPa / min, 2.4 MPa / min, 2.6 MPa / min, 2.8 MPa / min or 3 MPa / min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0031] Preferably, the endpoint pressure of the third boost is 230-290 MPa, for example, it can be 230 MPa, 235 MPa, 240 MPa, 245 MPa, 250 MPa, 255 MPa, 260 MPa, 265 MPa, 270 MPa, 275 MPa, 280 MPa, 285 MPa or 290 MPa, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0032] In the present invention, it is preferred to control the endpoint pressure of the third pressurization to be within a specific range, which can further improve the density of the blank and prevent the blank from cracking when demolding.

[0033] Preferably, the third pressure holding time is 15-35 min, for example, it can be 15 min, 16 min, 18 min, 20 min, 22 min, 24 min, 26 min, 28 min, 30 min, 32 min, 34 min or 35 min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0034] Preferably, the machining in step (1) comprises: machining the top surface and the bottom surface of the blank obtained after cold isostatic pressing treatment respectively.

[0035] In the present invention, the machining device may be, for example, a surface grinder.

[0036] Preferably, the flatness of the top and bottom surfaces after machining is ≤0.05 mm, for example, it can be 0.05 mm, 0.04 mm, 0.03 mm, 0.02 mm or 0.01 mm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0037] Preferably, the degassing temperature in step (2) is 400-550°C, for example, it can be 400°C, 410°C, 420°C, 430°C, 440°C, 450°C, 460°C, 470°C, 480°C, 490°C, 500°C, 520°C or 550°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0038] Preferably, the degassing time in step (2) is 5-9 h, for example, 5 h, 5.5 h, 6 h, 6.5 h, 7 h, 7.5 h, 8 h, 8.5 h or 9 h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0039] Preferably, the first heating rate in step (2) is 9-10°C / min, for example, it can be 9°C / min, 9.2°C / min, 9.4°C / min, 9.6°C / min, 9.8°C / min or 10°C / min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0040] Preferably, the endpoint temperature of the first heating is 790-810°C, for example, it can be 790°C, 792°C, 794°C, 796°C, 798°C, 800°C, 802°C, 804°C, 806°C, 808°C or 810°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0041] In the present invention, it is preferred to control the end temperature of the first heating to be within a specific range, which can further improve the formability and density of the target material.

[0042] Preferably, the second heating rate is 2-3°C / min, for example, it can be 2°C / min, 2.2°C / min, 2.4°C / min, 2.6°C / min, 2.8°C / min or 3°C / min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0043] Preferably, the endpoint temperature of the second heating is 1320-1390°C, for example, it can be 1320°C, 1330°C, 1340°C, 1350°C, 1360°C, 1370°C, 1380°C or 1390°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0044] In the present invention, it is preferred to control the end point temperature of the second heating to be within a specific range, which can further improve the density and formability of the target material.

[0045] Preferably, the first insulation time is 30-120 min, for example, it can be 30 min, 40 min, 50 min, 60 min, 70 min, 80 min, 90 min, 100 min, 110 min or 120 min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0046] In the present invention, it is preferred to control the first insulation time within a specific range, which can further improve the density of the target material, while avoiding the growth of alloy phase grains and agglomeration of elemental silicon, thereby improving the uniformity of the microstructure.

[0047] Preferably, the first insulation pressure is 100-180MPa, for example, it can be 100MPa, 105MPa, 120MPa, 125MPa, 130MPa, 135MPa, 140MPa, 145MPa, 150MPa, 155MPa, 160MPa, 165MPa, 170MPa, 175MPa or 180MPa, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0048] As a preferred technical solution of the present invention, the preparation method comprises the following steps:

[0049] (1) tungsten silicon alloy raw material with a particle size of 0.8-10 μm and a purity of 99.999 wt% is compacted and molded to a flatness of less than 1 mm and a density of ≥30%, and then a first pressure is increased at a rate of 9-10 MPa / min to an end pressure of 90-110 MPa and a first pressure is maintained for 5-6 min, and then a second pressure is increased at a rate of 4-5 MPa / min to an end pressure of 170-190 MPa and a second pressure is maintained for 5-30 min, and then a third pressure is increased at a rate of 2-3 MPa / min to an end pressure of 230-290 MPa and a third pressure is maintained for 15-35 min to obtain a billet, and the top and bottom surfaces of the billet are respectively machined to a flatness of ≤0.05 mm to obtain an ingot;

[0050] (2) The ingots obtained in step (1) are packaged, assembled and welded in sequence, and then degassed at 400-550°C for 5-9h, and then heated to an end temperature of 790-810°C at a rate of 9-10°C / min, and then heated to 1320-1390°C at a rate of 2-3°C / min and kept warm for 30-120min at a pressure of 100-180MPa to obtain a tungsten silicon target.

[0051] Compared with the prior art, the present invention has the following beneficial effects:

[0052] (1) The preparation method provided by the present invention can avoid the introduction of metal and non-metal impurities in the powder mixing process and reduce the oxygen content of the target material.

[0053] (2) The preparation method provided by the present invention combines cold isostatic pressing with hot isostatic pressing. On the one hand, cold isostatic pressing promotes the forming of alloy powder, avoids stratification and cracking, and initially improves the density. On the other hand, hot isostatic pressing further improves the density of the target material, while controlling the size of the alloy phase grains and elemental silicon, avoiding elemental silicon agglomeration, and improving the uniformity of the microstructure.

[0054] (3) The preparation method provided by the present invention can make the oxygen content of the tungsten silicon target material reach below 300 ppm, and can reach below 250 ppm under optimal conditions; can make the density of the tungsten silicon target material reach above 98%, and can reach above 99.6% under optimal conditions; can make the alloy phase grain size in the tungsten silicon target material reach below 35 μm, and can reach below 25 μm under optimal conditions, and the elemental silicon size reach below 30 μm, and can reach below 20 μm under optimal conditions. DETAILED DESCRIPTION

[0055] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0056] Example 1

[0057] This embodiment provides a method for preparing a tungsten silicon target, the preparation method comprising the following steps:

[0058] (1) a tungsten silicon alloy raw material (mass percentage of silicon is 29%) with a particle size of 0.8-10 μm and a purity of 99.999 wt% is compacted and molded to a flatness of 0.5 mm and a density of 30%, and then a first pressure is increased at a rate of 9.5 MPa / min to an end pressure of 100 MPa and a first pressure is maintained for 5 min, and then a second pressure is increased at a rate of 4.5 MPa / min to an end pressure of 180 MPa and a second pressure is maintained for 16 min, and then a third pressure is increased at a rate of 3 MPa / min to an end pressure of 280 MPa and a third pressure is maintained for 20 min to obtain a billet, and the top and bottom surfaces of the billet are respectively machined to a flatness of 0.05 mm to obtain an ingot;

[0059] (2) The ingots obtained in step (1) are packaged, assembled and welded in sequence, and then degassed at 500°C for 7 hours, and then heated to a final temperature of 800°C at a rate of 10°C / min, and then heated to 1360°C at a rate of 3°C / min and kept warm for 120 minutes at a pressure of 140 MPa to obtain a tungsten silicon target.

[0060] Example 2

[0061] This embodiment provides a method for preparing a tungsten silicon target, the preparation method comprising the following steps:

[0062] (1) a tungsten silicon alloy raw material (mass percentage of silicon is 29.5%) with a particle size of 0.8-10 μm and a purity of 99.999 wt% is compacted and molded to a flatness of 0.3 mm and a density of 30%, and then a first pressure is increased at a rate of 9 MPa / min to an end pressure of 110 MPa and a first pressure is maintained for 6 min, and then a second pressure is increased at a rate of 4 MPa / min to an end pressure of 170 MPa and a second pressure is maintained for 30 min, and then a third pressure is increased at a rate of 2 MPa / min to an end pressure of 290 MPa and a third pressure is maintained for 15 min to obtain a billet, and the top and bottom surfaces of the billet are respectively machined to a flatness of 0.04 mm to obtain an ingot;

[0063] (2) The ingots obtained in step (1) are packaged, assembled and welded in sequence, and then degassed at 400°C for 9 hours. Thereafter, the temperature is first increased at a rate of 9°C / min to an end temperature of 810°C, and then the temperature is secondly increased to 1320°C at a rate of 2°C / min and first kept warm for 100 minutes at a pressure of 100 MPa to obtain a tungsten silicon target.

[0064] Example 3

[0065] This embodiment provides a method for preparing a tungsten silicon target, the preparation method comprising the following steps:

[0066] (1) a tungsten silicon alloy raw material (mass percentage of silicon is 29.5%) with a particle size of 0.8-10 μm and a purity of 99.999 wt% is compacted and molded to a flatness of 0.2 mm and a density of 35%, and then a first pressure increase is performed at a rate of 10 MPa / min to an end pressure of 90 MPa and a first pressure holding is performed for 5.5 min, and then a second pressure increase is performed at a rate of 5 MPa / min to an end pressure of 190 MPa and a second pressure holding is performed for 5 min, and then a third pressure increase is performed at a rate of 2.5 MPa / min to an end pressure of 230 MPa and a third pressure holding is performed for 35 min to obtain a billet, and the top and bottom surfaces of the billet are respectively machined to a flatness of 0.04 mm to obtain an ingot;

[0067] (2) The ingots obtained in step (1) are packaged, assembled and welded in sequence, and then degassed at 550°C for 5 hours, and then heated to a final temperature of 790°C at a rate of 9°C / min, and then heated to 1390°C at a rate of 2°C / min and kept warm for 50 minutes at a pressure of 180 MPa to obtain a tungsten silicon target.

[0068] Example 4

[0069] This embodiment provides a method for preparing a tungsten-silicon target material. The only difference from Embodiment 1 is that the particle size of the tungsten-silicon alloy raw material is 20-30 μm.

[0070] Example 5

[0071] This embodiment provides a method for preparing a tungsten silicon target material, and the only difference compared with Embodiment 1 is that the end point pressure of the third pressurization is 220 MPa.

[0072] Example 6

[0073] This embodiment provides a method for preparing a tungsten silicon target material, and the only difference compared with Embodiment 1 is that the end point pressure of the third pressurization is 300 MPa.

[0074] Example 7

[0075] This embodiment provides a method for preparing a tungsten silicon target material, which is different from Embodiment 1 only in that the end temperature of the second heating is 1200°C.

[0076] Example 8

[0077] This embodiment provides a method for preparing a tungsten silicon target material, which is different from Embodiment 1 only in that the end temperature of the second heating is 1400°C.

[0078] Example 9

[0079] This embodiment provides a method for preparing a tungsten silicon target material. The only difference compared with Embodiment 1 is that the first insulation time is 20 minutes.

[0080] Comparative Example 1

[0081] This comparative example provides a method for preparing a tungsten silicon target. The only difference compared with Example 1 is that the first temperature increase is not performed, that is, the hot isostatic pressing treatment is replaced by: under a pressure of 140 MPa, the temperature is increased to 1360°C at a rate of 3°C / min and kept warm for 120 minutes.

[0082] Comparative Example 2

[0083] This comparative example provides a method for preparing a tungsten silicon target. The only difference compared with Example 1 is that the second temperature increase is not performed, that is, the hot isostatic pressing treatment is replaced by: under a pressure of 140 MPa, the temperature is increased at a rate of 10°C / min to an end temperature of 800°C and kept warm for 120 minutes.

[0084] The oxygen content of the tungsten silicon targets prepared in Examples 1-9 and Comparative Examples 1-2 was measured using a LECO oxygen analyzer. The results are shown in Table 1.

[0085] The density of the tungsten silicon targets prepared in Examples 1-9 and Comparative Examples 1-2 was measured using the Archimedes drainage method. The results are shown in Table 1.

[0086] The sizes of the alloy phase grains and elemental silicon in the tungsten silicon targets prepared in Examples 1-9 and Comparative Examples 1-2 were measured using an electron microscope. The results are shown in Table 1.

[0087] Table 1

[0088]

[0089]

[0090] From the data in Table 1, we can see the following points:

[0091] (1) It can be seen from the data of Examples 1-9 that the preparation method provided by the present invention can make the oxygen content of the tungsten silicon target material reach below 300 ppm, and can reach below 250 ppm under optimal conditions; can make the density of the tungsten silicon target material reach above 98%, and can reach above 99.6% under optimal conditions; can make the alloy phase grain size in the tungsten silicon target material reach below 35 μm, and can reach below 25 μm under optimal conditions, and the elemental silicon size reach below 30 μm, and can reach below 20 μm under optimal conditions.

[0092] (2) A comprehensive comparison of the data of Example 1 and Example 4 shows that the only difference between Example 4 and Example 1 is that the particle size of the tungsten silicon alloy raw material is not within the preferred range of the present invention. The size of the alloy phase grains and the size of elemental silicon in Example 4 are significantly higher than those in Example 1. It can be seen that the present invention can further avoid grain growth and avoid elemental silicon agglomeration by preferentially controlling the particle size of the tungsten silicon alloy raw material.

[0093] (3) A comprehensive comparison of the data of Example 1 and Examples 5-6 shows that the only difference between Example 5-6 and Example 1 is that the endpoint pressure of the third boost is not within the preferred range of the present invention, and the oxygen content of Example 1 is significantly lower than that of Examples 5-6. It can be seen that the present invention can further reduce the oxygen content of the tungsten silicon target by preferably controlling the endpoint pressure of the third boost.

[0094] (4) Comprehensive comparison of the data of Example 1 and Examples 7-8 shows that the only difference between Example 7-8 and Example 1 is that the end temperature of the second heating is not within the preferred range of the present invention, the density in Example 1 is significantly higher than that in Example 7, and the oxygen content in Example 1 is significantly lower than that in Example 8. It can be seen that the present invention can improve the density of the target material while reducing the oxygen content of the target material by preferably controlling the end temperature of the second heating.

[0095] (5) A comprehensive comparison of the data of Example 1 and Example 9 shows that the only difference between Example 9 and Example 1 is that the first insulation time is not within the preferred range of the present invention, and the oxygen content in Example 1 is significantly lower than that in Example 9. It can be seen that the present invention can further reduce the oxygen content by preferably controlling the first insulation time.

[0096] (6) Comprehensive comparison of the data of Example 1 and Comparative Examples 1-2 shows that the only difference between Comparative Example 1-2 and Example 1 is that the first and second heating processes are not performed, respectively. The oxygen content in Example 1 is significantly lower than that in Comparative Example 1-2, and the density in Example 1 is significantly higher than that in Comparative Example 1-2. It can be seen that the present invention can improve the density of the target material while reducing the oxygen content of the target material by adopting a combined process of the first and second heating processes.

[0097] In summary, the preparation method provided by the present invention can avoid the introduction of metal and non-metal impurities, reduce the oxygen content of the target material, improve the microstructure uniformity and density of the target material, and avoid the agglomeration of elemental silicon.

[0098] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing a tungsten silicon target, characterized in that: The preparation method comprises the following steps: (1) subjecting the tungsten silicon alloy raw material to compaction, cold isostatic pressing and machining in sequence to obtain an ingot; The cold isostatic pressing treatment includes a first pressurization, a first pressure holding, a second pressurization, a second pressure holding, a third pressurization and a third pressure holding performed in sequence; (2) subjecting the ingot obtained in step (1) to packaging, welding, degassing and hot isostatic pressing in sequence to obtain a tungsten silicon target; The hot isostatic pressing treatment includes a first heating, a second heating and a first heat preservation performed in sequence.

2. The preparation method according to claim 1, characterized in that: The particle size of the tungsten silicon alloy raw material in step (1) is 0.8-10 μm; Preferably, the mass percentage of silicon in the tungsten silicon alloy raw material is 28.5-29.5%; Preferably, the purity of the tungsten silicon alloy raw material is ≥99.999wt%.

3. The preparation method according to claim 1 or 2, characterized in that: The flatness after compaction and molding in step (1) is less than 1 mm; Preferably, the density after compaction and molding is ≥30%.

4. The preparation method according to any one of claims 1 to 3, characterized in that Step (1) The first pressure increase rate is 9-10 MPa / min; Preferably, the endpoint pressure of the first pressurization is 90-110 MPa; Preferably, the first pressure-maintaining time is 5-6 minutes; Preferably, the second pressure increase rate is 4-5 MPa / min; Preferably, the endpoint pressure of the second pressurization is 170-190 MPa; Preferably, the second pressure holding time is 5-30 minutes; Preferably, the rate of the third pressure increase is 2-3 MPa / min; Preferably, the endpoint pressure of the third pressurization is 230-290 MPa; Preferably, the third pressure holding time is 15-35 minutes.

5. The preparation method according to any one of claims 1 to 4, characterized in that: The machining in step (1) comprises: machining the top surface and the bottom surface of the blank obtained after the cold isostatic pressing treatment respectively; Preferably, the flatness of the top surface and the bottom surface after machining is respectively ≤0.05 mm.

6. The preparation method according to any one of claims 1 to 5, characterized in that: The degassing temperature in step (2) is 400-550°C.

7. The preparation method according to any one of claims 1 to 6, characterized in that: The degassing time in step (2) is 5-9h.

8. The preparation method according to any one of claims 1 to 7, characterized in that: Step (2) the first heating rate is 9-10°C / min; Preferably, the endpoint temperature of the first heating is 790-810°C; Preferably, the second heating rate is 2-3°C / min; Preferably, the end temperature of the second heating is 1320-1390°C; Preferably, the first insulation time is 30-120 min.

9. The preparation method according to claim 8, characterized in that: The first insulation pressure is 100-180 MPa.

10. The preparation method according to any one of claims 1 to 9, characterized in that: The preparation method comprises the following steps: (1) tungsten silicon alloy raw material with a particle size of 0.8-10 μm and a purity of ≥99.999wt% is compacted and molded to a flatness of <1 mm and a density of ≥30%, and then a first pressure is increased at a rate of 9-10 MPa / min to an end pressure of 90-110 MPa and a first pressure is maintained for 5-6 min, and then a second pressure is increased at a rate of 4-5 MPa / min to an end pressure of 170-190 MPa and a second pressure is maintained for 5-30 min, and then a third pressure is increased at a rate of 2-3 MPa / min to an end pressure of 230-290 MPa and a third pressure is maintained for 15-35 min to obtain a billet, and the top and bottom surfaces of the billet are respectively machined to a flatness of ≤0.05 mm to obtain an ingot; (2) The ingots obtained in step (1) are packaged, assembled and welded in sequence, and then degassed at 400-550°C for 5-9h, and then heated to an end temperature of 790-810°C at a rate of 9-10°C / min, and then heated to 1320-1390°C at a rate of 2-3°C / min and kept warm for 30-120min at a pressure of 100-180MPa to obtain a tungsten silicon target.

Citation Information

Cited By

  • Preparation method of tungsten-silicon alloy target material

    CN120624997A