Multi-temperature-zone multi-layer composite thermal insulation material and preparation method thereof
By introducing sodium silicate colloid into the battery pack insulation material and optimizing the particle size and content of SiC particles, combined with surface modification treatment, we have solved the problem of the decline in insulation performance of existing insulation materials under pressure and the thermal radiation after the introduction of sunscreen agents. Balancing the problem, achieving more efficient thermal insulation performance.
Patent Information
- Application Number
- CN202410828012.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-06-25
AI Technical Summary
The thermal insulation performance of existing battery pack insulation materials decreases under pressure, and when the sunscreen agent is introduced, it suppresses thermal radiation but increases solid-phase thermal conductivity, making it difficult to achieve a balanced thermal insulation performance.
Multi-temperature zone multi-layer composite insulation materials are used. By introducing sodium silicate colloid and optimizing the particle size and content of SiC particles, combined with surface modification treatment, the thermal insulation performance of the material in different temperature ranges is improved.
It significantly improves the thermal insulation performance of composite thermal insulation materials under pressure, ensures that the positive effects outweigh the negative effects in different temperature ranges, and improves the overall thermal insulation performance.
Smart Images

Figure BDA0004911070670000081 
Figure BDA0004911070670000101 
Figure BDA0004911070670000131
Abstract
Description
Technical Field
[0001] The present invention relates to the field of thermal insulation materials, and in particular to a multi-temperature zone multi-layer composite thermal insulation material and a preparation method thereof. Background Art
[0002] The energy storage part and energy conversion part of the battery pack exist in the same space, which can easily cause a chain reaction of exothermic reactions in the case of overcharging, puncture, or collision, resulting in thermal runaway accidents such as smoke, fire, or even explosion. Thermal runaway is the most serious safety accident of power batteries, which directly threatens the life safety of users. In recent years, the problem of thermal runaway propagation in battery packs has been mainly solved through thermal protection technology. That is, protective materials are set between battery cells, between battery modules, and between the battery box and the passenger compartment to increase the thermal resistance of heat transfer from the thermal runaway battery cell to other battery components, thereby achieving the purpose of preventing the spread of thermal runaway.
[0003] Similarly, the current research on thermal runaway of power battery systems also focuses on solving the thermal runaway safety problem that is triggered by thermal runaway of a single cell and then spreads to the entire battery pack. Because when a single cell triggers thermal runaway, its heat generation increases sharply, and the heat dissipation is far less than the heat generation, causing heat to be rapidly transferred to the surrounding cells, quickly triggering large-scale thermal runaway of the surrounding cells, posing a safety hazard. It can be said that the thermal runaway of a single cell is the source of thermal runaway of the entire battery pack. Therefore, thermal protection between cells usually involves adding insulation materials between the cells to block the spread of thermal runaway from the runaway cell to the surrounding cells, reducing damage to the battery pack and incidental destructive effects.
[0004] At present, the thermal insulation material between battery cells is often prepared by impregnation, spraying or supercritical method to prepare aerogel insulation sheets with different substrates. The aerogel powder in these insulation sheets is unevenly distributed. Using water as solvent, the aerogel powder is mixed with ceramic fiber, and different functional additives are added to make a ceramic fiber aerogel mixed slurry. The slurry is then filtered through a filter to make sheets. After a part of the water is sucked away by vacuum, the thickness of the product is controlled by a pressing plate. After drying in a drying oven, the ceramic fiber aerogel insulation sheet is obtained by rolling or slicing. Although the distribution of aerogel powder in the material is relatively uniform, the inorganic insulation powder is easily squeezed out of the substrate when it is squeezed from the outside, which leads to a decrease in the thermal insulation performance of the product.
[0005] In addition, since aerogel materials (such as SiO2 aerogel) cannot form a thermal barrier to infrared light in the 3-8μm band, although the extinction coefficient of the sunscreen is significantly higher than that of the aerogel material in this range, it can effectively improve the thermal conductivity of the aerogel material in the short-wave range, thereby inhibiting high-temperature thermal radiation and improving the thermal insulation performance of the thermal insulation material. However, the researchers found that after the introduction of the sunscreen, while inhibiting thermal radiation, it will also increase the solid-phase thermal conductivity of the material. In other words, if the selection and dosage of the sunscreen are inappropriate, it may reduce the thermal insulation performance of the aerogel material.
[0006] In summary, how to improve the thermal insulation performance of thermal insulation materials under pressure, and how to balance the inhibition of thermal radiation (positive effect) and the increase of solid-phase thermal conductivity (negative effect) caused by the introduction of sunscreens, are technical problems that need to be solved urgently. Summary of the invention
[0007] In order to solve the above technical problems, the present invention provides a multi-temperature zone multi-layer composite thermal insulation material and a preparation method thereof. First, the present invention improves the thermal insulation performance of the composite thermal insulation material under pressure by introducing sodium silicate colloid into the composite thermal insulation material; second, the present invention optimizes the particle size and content of SiC particles in each thermal insulation layer according to the specific use environment, so that after the SiC particles are introduced into the thermal insulation layer in different temperature ranges, the positive effect can be ensured to be greater than the negative effect, thereby improving the comprehensive thermal insulation performance of the composite thermal insulation material.
[0008] The specific technical scheme of the present invention is: In the first aspect, the present invention provides a multi-temperature zone multi-layer composite thermal insulation material, which includes at least one high-temperature zone insulation layer, at least one medium-temperature zone insulation layer and at least one low-temperature zone insulation layer in order from near to far from the heat source.
[0009] The high temperature zone thermal insulation layer, the medium temperature zone thermal insulation layer and the low temperature zone thermal insulation layer all include an inorganic fiber substrate, and inorganic thermal insulation powder, SiC particles and sodium silicate colloid dispersed in the inorganic fiber substrate.
[0010] The particle sizes of the shading particles in the high temperature zone insulation layer, the medium temperature zone insulation layer and the low temperature zone insulation layer are 1.3-2.5 μm, 2.5-4 μm and 4-7 μm respectively, and the contents are 0.4-0.6 wt%, 0.3-0.35 wt% and 0.1-0.2 wt% respectively.
[0011] Firstly, in view of the problem that the existing thermal insulation materials are easily squeezed under pressure, resulting in a decrease in thermal insulation performance, the present invention introduces sodium silicate colloid into the composite thermal insulation material. During the preparation process, the sodium silicate aqueous solution (i.e., water glass) is evenly distributed in the inorganic fiber substrate to form a water glass sol. The hydration film in the water glass sol is then destroyed by a physical dehydration method, so that the water glass sol becomes a viscous liquid → a semi-solid → a colloid (sodium silicate) in sequence after losing water. The sodium silicate colloid has a certain strength, thereby improving the hardness of the composite thermal insulation material and having better resistance to compressive deformation, thereby improving the thermal insulation performance of the composite thermal insulation material after being compressed.
[0012] Secondly, as described in the background technology section, although adding a sunscreen to the thermal insulation material can effectively improve the shading performance of inorganic thermal insulation powders such as aerogel in the short-wave range, thereby inhibiting high-temperature radiation. However, the introduction of the sunscreen will also increase the solid phase thermal conductivity, which will reduce the thermal insulation performance of the thermal insulation material. Therefore, the thermal insulation performance of the thermal insulation material can only be improved when the positive effect of adding the sunscreen is sufficient to cover its negative effect. To this end, the present invention has conducted in-depth research: (a) The present invention selects SiC particles as sunscreen agents, which are not easily oxidized at high temperatures (>300°C) and have good high-temperature stability; (b) The present invention has found through research that: within the incident light band range of 3.0-6.0μm, the spectral extinction coefficient of the composite thermal insulation material is the largest when the SiC particle size is about 2.0μm; within the incident light band range of 5.5-9.0μm, the spectral extinction coefficient of the composite thermal insulation material is the largest when the SiC particle size is about 3.0μm; and the maximum spectral extinction coefficient decreases with the increase of the sunscreen agent particle size, so the optimal added particle size of SiC particles gradually decreases with the increase of temperature.
[0013] In addition, regarding the content of SiC particles: When the temperature is about 200°C, the main heat transfer mode of the composite thermal insulation material containing SiC particles is gas-solid heat conduction, and the contribution of radiation heat transfer is relatively small. At this time, the effect of SiC particles on the equivalent thermal conductivity of the composite thermal insulation material is small. When the SiC particle content is 0.1-0.2wt%, the thermal conductivity of the composite thermal insulation material is the lowest. As the content of SiC particles further increases (>0.2wt%), the decrease in radiation thermal conductivity is less than the increase in gas-solid thermal conductivity. The equivalent thermal conductivity of the composite thermal insulation material increases with the increase in the content of SiC particles. Therefore, excessive SiC particle content will have a counterproductive effect. When the temperature rises to 300°C, the gas-solid thermal conductivity of the composite thermal insulation material remains basically unchanged, but its radiation thermal conductivity increases significantly. At this time, radiation heat transfer becomes the main heat transfer mode, and radiation heat transfer decreases rapidly with the increase in SiC particle content. However, when the SiC particle content is further increased, gas-solid heat conduction becomes the main heat transfer mode again because the thermal conductivity of the SiC particles themselves is much greater than that of the inorganic fiber matrix. At this time, the thermal conductivity of the composite insulation material is the lowest when the SiC particle content is about 0.3-0.35wt%. Similarly, when the temperature is further increased to above 500°C, the optimal content of SiC particles needs to be increased to about 0.4-0.6wt%. Therefore, as the temperature increases, the SiC content needs to be gradually increased.
[0014] In summary, the present invention optimizes the particle size and content of SiC particles in each insulation layer according to the specific use environment, so that after introducing SiC particles into the insulation layers in different temperature ranges, it can ensure that the positive effect is greater than the negative effect, thereby improving the comprehensive insulation performance of the composite insulation material.
[0015] Preferably, the insulation temperatures of the high temperature zone insulation layer, the medium temperature zone insulation layer and the low temperature zone insulation layer are 500-800°C, 300-500°C and <300°C respectively.
[0016] According to the composition of the high temperature zone insulation layer, the medium temperature zone insulation layer and the low temperature zone insulation layer in the composite thermal insulation material of the present invention, preferably, the content of inorganic fiber substrate in the high temperature zone insulation layer, the medium temperature zone insulation layer and the low temperature zone insulation layer is 30-70wt%, the content of inorganic thermal insulation powder is 20-50wt%, and the content of sodium silicate colloid is 1-3wt%.
[0017] The present invention finds that the content of sodium silicate is critical. If the content is too high, the thermal conductivity of sodium silicate colloid is higher than that of air, and excessive generation of sodium silicate colloid will reduce the porosity of the thermal insulation layer. Therefore, excessive sodium silicate will reduce the thermal insulation performance of the composite thermal insulation material; if the content of sodium silicate is too low, the improvement effect is limited. Therefore, controlling the content within the above range will achieve better results.
[0018] Preferably, the material of the inorganic fiber substrate is selected from one or more of glass fiber, high silica fiber, aluminum silicate fiber, alkaline earth silicate fiber and mullite fiber, preferably aluminum silicate fiber.
[0019] The inorganic heat-insulating powder is selected from one or more of inorganic aerogel powder, fumed silica, precipitated silica, hollow glass microspheres, hollow ceramic microspheres, expanded vermiculite and expanded perlite.
[0020] Preferably, the multi-temperature zone multi-layer composite thermal insulation material has a cold surface temperature of ≤110°C after being subjected to 700°C, 0.9 MPa and pressure for 5 minutes.
[0021] In a second aspect, the present invention provides a method for preparing a multi-temperature zone multi-layer composite thermal insulation material, comprising: 1) Add dispersant and wetting agent to water and stir evenly, add inorganic thermal insulation powder, SiC particles and inorganic fiber in turn and stir evenly after each addition to obtain slurry; paper the slurry, filter the water to obtain a sheet, and then spray a sodium silicate aqueous solution (i.e., water glass) on the surface of the sheet by means of surface glue spraying, and vacuum suction the sheet to make the sodium silicate evenly distributed inside the material, and then dry to obtain a high temperature zone insulation layer, a medium temperature zone insulation layer and a low temperature zone insulation layer respectively.
[0022] 2) The high temperature zone insulation layer, the medium temperature zone insulation layer and the low temperature zone insulation layer are stacked in sequence to obtain a multi-temperature zone multi-layer composite insulation material.
[0023] Preferably, the surface of the SiC particles is grafted with polyacrylic acid, and the preparation method thereof comprises: modifying SiC particles with an alkenyl-containing silane coupling agent to obtain SiC particles with alkenyl grafted on the surface, copolymerizing the SiC particles with acrylic acid monomers under high-energy electron beam irradiation to obtain SiC particles with polyacrylic acid grafted on the surface.
[0024] The present invention finds that SiC particles are easily lost during the process of forming the material, thereby affecting the thermal insulation performance of the composite thermal insulation material. To this end, the present invention performs surface grafting modification of SiC particles with polyacrylic acid (first modifying SiC particles with an alkenyl-containing silane coupling agent so that the surface has alkenyl groups, and then using the alkenyl groups to copolymerize with acrylic acid). After the above modification, a small amount of polyacrylic acid can promote a certain degree of flocculation of inorganic fibers during the process of forming, thereby wrapping the SiC particles in the inorganic fiber substrate and reducing the loss rate. And compared with adding polyacrylic acid alone, SiC particles with polyacrylic acid grafted on the surface can generate interfacial bonding force with inorganic fibers, and have higher stability.
[0025] Preferably, during the high-energy electron beam irradiation, the energy of the high-energy electron beam is 30-60 kGy, and the amount of acrylic acid used is 10-20 wt % of the SiC particles.
[0026] The present invention finds that the amount of polyacrylic acid used in the modification process has a significant effect on the high temperature radiation suppression ability of SiC particles. If the amount of polyacrylic acid used is too small, the effect of reducing the loss of SiC particles is limited; on the contrary, if the amount is too large, the surface of the SiC particles will be wrapped in a large area, thereby affecting its light shielding performance.
[0027] As a further preference, the copolymerized monomers also include acrylic acid phosphate, and the mass ratio of acrylic acid to acrylic acid phosphate is (4-6):1.
[0028] In order to further enhance the bonding strength between SiC particles and inorganic fibers during the papermaking process, an appropriate amount of acrylic acid phosphate can be doped into the acrylic acid monomer. After copolymerization of acrylic acid phosphate, the bonding strength between the polymer and the inorganic fibers can be further enhanced, thereby further reducing the loss rate of SiC particles.
[0029] Preferably, the dispersant is selected from one or more of polyvinyl alcohol, polyethylene oxide, silane coupling agent, sodium dodecylbenzene sulfonate and sodium isopropylnaphthalene sulfonate.
[0030] Preferably, the wetting agent is selected from one or more of sodium hydroxyethyl cellulose, sodium carboxymethyl cellulose, bentonite and diatomaceous earth.
[0031] Preferably, in the raw materials of the high temperature zone insulation layer, the medium temperature zone insulation layer and the low temperature zone insulation layer, the dispersant accounts for 0.5-5wt% and the wetting agent accounts for 0.5-5wt%.
[0032] Compared with the prior art, the beneficial effects of the present invention are: (1) The present invention introduces sodium silicate colloid into the composite thermal insulation material. During the preparation process, the sodium silicate aqueous solution (i.e., water glass) is evenly distributed in the inorganic fiber substrate to form a water glass sol. The hydration film in the water glass sol is then destroyed by a physical dehydration method, so that the water glass sol loses water and turns into a viscous liquid → a semi-solid → a sodium silicate colloid in sequence. The sodium silicate colloid has a certain strength, thereby improving the hardness of the composite thermal insulation material and having a better ability to resist compressive deformation.
[0033] (2) According to the specific use environment, the present invention optimizes the particle size and content of SiC particles in each insulation layer, so that after the SiC particles are introduced into the insulation layers in different temperature ranges, the positive effect can be ensured to be greater than the negative effect, thereby improving the comprehensive insulation performance of the composite insulation material.
[0034] (3) The present invention grafts polyacrylic acid onto the surface of SiC particles. During the papermaking process, polyacrylic acid can promote a certain degree of flocculation of inorganic fibers, thereby wrapping the SiC particles in the inorganic fiber matrix, reducing its loss rate, and thereby improving the thermal insulation performance of the composite thermal insulation material. DETAILED DESCRIPTION
[0035] The present invention will be further described below in conjunction with the embodiments.
[0036] Overall embodiment First, a multi-temperature zone multi-layer composite thermal insulation material includes, in order from near to far from the heat source, at least one high-temperature zone thermal insulation layer, at least one medium-temperature zone thermal insulation layer and at least one low-temperature zone thermal insulation layer.
[0037] The high temperature zone thermal insulation layer, the medium temperature zone thermal insulation layer and the low temperature zone thermal insulation layer all include an inorganic fiber substrate, and inorganic thermal insulation powder, SiC particles and sodium silicate colloid dispersed in the inorganic fiber substrate.
[0038] The particle sizes of SiC particles in the high temperature zone insulation layer, the medium temperature zone insulation layer and the low temperature zone insulation layer are 1.3-2.5 μm, 2.5-4 μm and 4-7 μm respectively, and the contents are 0.4-0.6 wt%, 0.3-0.35 wt% and 0.1-0.2 wt% respectively.
[0039] In some specific implementation cases, the insulation temperatures of the high temperature zone insulation layer, the medium temperature zone insulation layer and the low temperature zone insulation layer are 500-800°C, 300-500°C and <300°C respectively.
[0040] In some specific implementation cases, the content of inorganic fiber substrate in the high temperature zone insulation layer, medium temperature zone insulation layer and low temperature zone insulation layer is 30-70wt%, the content of inorganic insulation powder is 20-50wt%, and the content of sodium silicate colloid is 1-3wt%.
[0041] In some specific implementation cases, the material of the inorganic fiber substrate is selected from one or more of glass fiber, high silica fiber, aluminum silicate fiber, alkaline earth silicate fiber and mullite fiber, preferably aluminum silicate fiber.
[0042] In some specific implementation cases, the inorganic thermal insulation powder is selected from one or more of inorganic aerogel powder, fumed silica, precipitated silica, hollow glass microspheres, hollow ceramic microspheres, expanded vermiculite and expanded perlite.
[0043] In some specific implementation cases, the thickness of a single layer of the high temperature zone thermal insulation layer, the medium temperature zone thermal insulation layer and the low temperature zone thermal insulation layer is 0.5-2 mm.
[0044] In some specific implementation cases, the cold surface temperature of the multi-temperature zone multi-layer composite thermal insulation material is ≤110°C after being subjected to 700°C and 0.9 MPa pressure for 5 minutes.
[0045] Secondly, a method for preparing a multi-temperature zone multi-layer composite thermal insulation material comprises: 1) Add dispersant and wetting agent to water and stir evenly, add inorganic thermal insulation powder, SiC particles with different contents, and inorganic fiber in turn and stir evenly after each addition to obtain slurry; paper the slurry, filter the water to obtain a sheet, and then spray the sodium silicate aqueous solution on the surface of the sheet by surface coating. The sheet passes through the coating head at a rate of 2 m / min, and negative pressure suction is performed under the sheet to make the sodium silicate evenly distributed inside the material, and then dry to obtain a high temperature zone insulation layer, a medium temperature zone insulation layer, and a low temperature zone insulation layer, respectively.
[0046] 2) The high temperature zone insulation layer, the medium temperature zone insulation layer and the low temperature zone insulation layer are stacked in sequence to obtain a multi-temperature zone multi-layer composite insulation material.
[0047] In some specific implementation cases, the surface of the SiC particles is grafted with polyacrylic acid, and the preparation method thereof comprises: modifying the SiC particles with an alkenyl-containing silane coupling agent to obtain SiC particles with alkenyl grafted on the surface, copolymerizing the SiC particles with acrylic acid monomers under high-energy electron beam irradiation to obtain SiC particles with polyacrylic acid grafted on the surface; during the high-energy electron beam irradiation, the energy of the high-energy electron beam is 30-60 kGy, and the amount of acrylic acid used is 10-20 wt % of the SiC particles.
[0048] In some specific implementation cases, SiC particles are modified using an alkenyl silane coupling agent solution, the solvent of the alkenyl silane coupling agent solution is 90-98 vol% ethanol aqueous solution, and the concentration of the alkenyl silane coupling agent is 3-7 wt%.
[0049] In some more specific implementation cases, the reaction temperature of the modification is 50-70° C., and the reaction time is 50-70 min.
[0050] In some more preferred implementation cases, the comonomer also includes acrylic acid phosphate, and the mass ratio of acrylic acid to acrylic acid phosphate is (4-6):1.
[0051] In some specific implementation cases, the dispersant is selected from one or more of polyvinyl alcohol, polyethylene oxide, silane coupling agent, sodium dodecylbenzene sulfonate and sodium isopropylnaphthalene sulfonate. In some specific implementation cases, the wetting agent is selected from one or more of sodium hydroxyethyl cellulose, sodium carboxymethyl cellulose, bentonite and diatomaceous earth. In some specific implementation cases, in the raw materials of the high temperature zone insulation layer, the medium temperature zone insulation layer and the low temperature zone insulation layer, the dispersant accounts for 0.5-5wt%, and the wetting agent accounts for 0.5-5wt%.
[0052] (I) Influence of different SiC particle contents: Test Example 1 A method for preparing a multi-temperature zone multi-layer composite thermal insulation material comprises the following steps: (1) Preparation of thermal insulation layer in low temperature zone: Add water to the dispersion tank; Add dispersant silane coupling agent KH550, content 0.9wt% (accounting for all raw materials, excluding water), wetting agent sodium carboxymethyl cellulose, content 1wt% (accounting for all raw materials, excluding water), speed 1000rpm, stirring time 8min; Add inorganic thermal insulation powder fumed silica, the content is 40wt% (accounting for all raw materials, excluding water), the speed is 1000rpm, and the stirring time is 10min; Adding SiC with an average particle size of about 5 μm and a content of 0.2 wt% (of all raw materials, excluding water); Add aluminum silicate fiber with a content of 56.9wt% (accounting for all raw materials, excluding water), rotate speed 1000rpm, and stir for 8min; add adhesive polyvinyl butyral with a content of 1wt% (accounting for all raw materials, excluding water), rotate speed 800rpm, and stir for 3min; pump the prepared slurry into a flow box, filter water through a papermaking machine to make sheets; pass through a drying tunnel at 130°C for 10min to dry.
[0053] (2) Preparation of thermal insulation layer in medium temperature zone: Add water to the dispersion tank; Add dispersant silane coupling agent KH550, content 0.9wt% (accounting for all raw materials, excluding water), wetting agent sodium carboxymethyl cellulose, content 1wt% (accounting for all raw materials, excluding water), speed 1000rpm, stirring time 8min; Add inorganic thermal insulation powder fumed silica, the content is 40wt% (accounting for all raw materials, excluding water), the speed is 1000rpm, and the stirring time is 10min; Add SiC with an average particle size of about 3 μm and a content of 0.3% (to all raw materials, excluding water); Add aluminum silicate fiber with a content of 56.8wt% (accounting for all raw materials, excluding water), rotate speed 1000rpm, and stir for 8min; add adhesive polyvinyl butyral with a content of 1wt% (accounting for all raw materials, excluding water), rotate speed 800rpm, and stir for 3min; pump the prepared slurry into a flow box, filter water through a papermaking machine to make sheets; pass through a drying tunnel at 130°C for 10min to dry.
[0054] (3) Preparation of thermal insulation layer in high temperature area: Add water to the dispersion tank; Add dispersant silane coupling agent KH550, content 0.9wt% (accounting for all raw materials, excluding water), wetting agent sodium carboxymethyl cellulose, content 1wt% (accounting for all raw materials, excluding water), speed 1000rpm, stirring time 8min; Add inorganic thermal insulation powder fumed silica, the content is 40wt% (accounting for all raw materials, excluding water), the speed is 1000rpm, and the stirring time is 10min; Adding SiC with an average particle size of about 1.5 μm and a content of 0.5 wt% (accounting for all raw materials, excluding water); Add aluminum silicate fiber with a content of 56.6wt% (accounting for all raw materials, excluding water), rotate speed 1000rpm, and stir for 8min; add adhesive polyvinyl butyral with a content of 1wt% (accounting for all raw materials, excluding water), rotate speed 800rpm, and stir for 3min; pump the prepared slurry into a flow box, filter water through a papermaking machine to make sheets; pass through a drying tunnel at 130°C for 10min to dry.
[0055] (4) A high temperature zone insulation layer (single layer thickness of 1 mm, number of layers of 1 layer), a medium temperature zone insulation layer (single layer thickness of 1 mm, number of layers of 1 layer), and a low temperature zone insulation layer (single layer thickness of 1 mm, number of layers of 1 layer) are sequentially stacked and vacuum packaged with a PET film to obtain a multi-temperature zone multilayer composite insulation material.
[0056] Test Example 2 The difference between this test example and test example 1 is that SiC is not added to each thermal insulation layer (the difference is replaced by aluminum silicate fiber).
[0057] Test Example 3 The difference between this test example and test example 1 is that the average particle size of SiC in each heat insulation layer is 5 μm, and the content is 0.2 wt% (the difference is adjusted by aluminum silicate fiber).
[0058] Test Example 4 The difference between this test example and test example 1 is that the average particle size of SiC in each heat-insulating layer is 3 μm, and the content is 0.3 wt% (the difference is adjusted by aluminum silicate fiber).
[0059] Test Example 5 The difference between this test example and test example 1 is that the average particle size of SiC in each heat insulation layer is 1.5 μm, and the content is 0.5 wt% (the difference is adjusted by aluminum silicate fiber).
[0060] Performance Testing The thermal conductivity of the low temperature zone insulation layer, medium temperature zone insulation layer and high temperature zone insulation layer obtained in each test case was tested respectively: GB / T10294-2008; then the thermal insulation performance of the composite thermal insulation material was tested, the high temperature zone insulation layer of the composite thermal insulation material was placed on a constant 700°C heating table, and a pressure of 0.9MPa was applied to test the temperature of the low temperature zone insulation layer of the composite thermal insulation material. The test results are shown in Table 1: Table 1 From the comparison of the data in Table 1, it can be seen that: Compared with Test Example 2, Test Example 1 adds SiC of different particle sizes and contents to each insulation layer, and it can be found that the thermal conductivity of each insulation layer is significantly reduced; in Test Examples 3-5, compared with Test Example 1, the difference is that the particle size and content of SiC added to each insulation layer are the same, that is, no gradient SiC is set. From the data of Test Example 3, it can be found that, except for the low-temperature zone insulation layer, the thermal conductivity of the medium-temperature zone insulation layer and the high-temperature zone insulation layer are significantly higher than that of Test Example 1, and even slightly higher than that of Test Example 2. This shows that in the medium and high-temperature zone insulation layers of Test Example 3, the negative effect of adding SiC is greater than the positive effect, resulting in an increase in the thermal conductivity instead of a decrease. Similarly, similar results appeared in Test Examples 4 and 5.
[0061] (II) The influence of sodium silicate colloid: Test Example 6 A method for preparing a multi-temperature zone multi-layer composite thermal insulation material comprises the following steps: (1) Preparation of thermal insulation layer in low temperature zone: Add water to the dispersion tank; Add dispersant silane coupling agent KH550, content 0.9wt% (accounting for all raw materials, excluding water), wetting agent sodium carboxymethyl cellulose, content 1wt% (accounting for all raw materials, excluding water), speed 1000rpm, stirring time 8min; Add inorganic thermal insulation powder fumed silica, the content is 40wt% (accounting for all raw materials, excluding water), the speed is 1000rpm, and the stirring time is 10min; Add SiC with an average particle size of 5 μm and a content of 0.2 wt% (accounting for all raw materials, excluding water); Aluminum silicate fiber was added, with a content of 56.9 wt% (accounting for all raw materials, excluding water), the rotation speed was 1000 rpm, and the stirring time was 8 min; the prepared slurry was pumped into a headbox, and the sheet was made by filtering water through a papermaking machine; By means of surface glue spraying, the flow rate is controlled to spray a sodium silicate aqueous solution with a concentration of 40wt% onto the surface of the sheet, the sheet passes through the glue spraying head at a rate of 2 meters / min, and negative pressure suction is performed under the sheet to make the sodium silicate aqueous solution evenly distributed inside the material; the sodium silicate colloid content is 1wt% (accounting for all raw materials, excluding water); Dry in a drying oven at 130°C for 10 minutes.
[0062] (2) Preparation of thermal insulation layer in medium temperature zone: Add water to the dispersion tank; Add dispersant silane coupling agent KH550, content 0.9wt% (accounting for all raw materials, excluding water), wetting agent sodium carboxymethyl cellulose, content 1wt% (accounting for all raw materials, excluding water), speed 1000rpm, stirring time 8min; Add inorganic thermal insulation powder fumed silica, the content is 40wt% (accounting for all raw materials, excluding water), the speed is 1000rpm, and the stirring time is 10min; Add SiC with an average particle size of 3 μm and a content of 0.3% (accounting for all raw materials, excluding water); Aluminum silicate fiber was added, with a content of 56.8 wt% (accounting for all raw materials, excluding water), the rotation speed was 1000 rpm, and the stirring time was 8 min; the prepared slurry was pumped into a headbox, and the sheet was made by filtering water through a papermaking machine; By means of surface glue spraying, the flow rate is controlled to spray a sodium silicate aqueous solution with a concentration of 40wt% onto the surface of the sheet, the sheet passes through the glue spraying head at a rate of 2 meters / min, and negative pressure suction is performed under the sheet to make the sodium silicate aqueous solution evenly distributed inside the material; the sodium silicate colloid content is 1wt% (accounting for all raw materials, excluding water); Dry in a drying oven at 130°C for 10 minutes.
[0063] (3) Preparation of thermal insulation layer in high temperature area: Add water to the dispersion tank; Add dispersant silane coupling agent KH550, content 0.9wt% (accounting for all raw materials, excluding water), wetting agent sodium carboxymethyl cellulose, content 1wt% (accounting for all raw materials, excluding water), speed 1000rpm, stirring time 8min; Add inorganic thermal insulation powder fumed silica, the content is 40wt% (accounting for all raw materials, excluding water), the speed is 1000rpm, and the stirring time is 10min; Add SiC with an average particle size of 1.5 μm and a content of 0.5 wt% (accounting for all raw materials, excluding water); Add aluminum silicate fiber, the content is 56.6wt% (accounting for all raw materials, excluding water), the speed is 1000rpm, and the stirring time is 8min; The prepared slurry is pumped into the headbox and the sheet is made by filtering water through the papermaking machine; By means of surface glue spraying, the flow rate is controlled to spray a sodium silicate aqueous solution with a concentration of 40wt% onto the surface of the sheet, the sheet passes through the glue spraying head at a rate of 2 meters / min, and negative pressure suction is performed under the sheet to make the sodium silicate aqueous solution evenly distributed inside the material; the sodium silicate colloid content is 1wt% (accounting for all raw materials, excluding water); Dry in a drying oven at 130°C for 10 minutes.
[0064] (4) A high temperature zone insulation layer (single layer thickness of 1 mm, number of layers of 1 layer), a medium temperature zone insulation layer (single layer thickness of 1 mm, number of layers of 1 layer), and a low temperature zone insulation layer (single layer thickness of 1 mm, number of layers of 1 layer) are sequentially stacked and vacuum packaged with a PET film to obtain a multi-temperature zone multilayer composite insulation material.
[0065] Test Example 7 The difference between this test example and test example 6 is that the content of sodium silicate colloid in each layer is 2 wt % (the difference is replaced by aluminum silicate fiber).
[0066] Test Case 8 The difference between this test example and test example 6 is that the content of sodium silicate colloid in each layer is 3wt% (the difference is replaced by aluminum silicate fiber).
[0067] Test Example 9 The difference between this test example and test example 6 is that the content of sodium silicate colloid in each layer is 4 wt % (the difference is replaced by aluminum silicate fiber).
[0068] Performance Testing The performance of the composite thermal insulation materials obtained in Test Examples 6-9 was tested and compared with that in Test Example 1. The results are shown in Table 2: Table 2 From the data comparison in Table 2, it can be seen that: compared with Test Example 1, after adding an appropriate amount of sodium silicate colloid to Test Examples 6-8, the cold surface temperature has been significantly reduced, indicating that the addition of sodium silicate colloid can significantly improve the thermal insulation performance of the composite thermal insulation material under pressure (the cold surface temperature is tested under a pressure of 0.9MPa); in Test Example 9, the addition amount of sodium silicate colloid is 4wt%, and it is found that the cold surface temperature is higher than that of Test Example 1. This is because the thermal conductivity of the colloid formed after the sodium silicate aqueous solution is dehydrated is higher than that of air, and the porosity of the composite thermal insulation material is excessively reduced, which leads to a decrease in the thermal insulation performance of the composite thermal insulation material. In summary, the optimal addition amount of sodium silicate colloid is 1-3wt%.
[0069] (III) The influence of surface modified SiC: Test Example 10 A method for preparing a multi-temperature zone multi-layer composite thermal insulation material comprises the following steps: (1) Preparation of thermal insulation layer in low temperature zone: Add water to the dispersion tank; Add dispersant silane coupling agent KH550, content 0.9wt% (accounting for all raw materials, excluding water), wetting agent sodium carboxymethyl cellulose, content 1wt% (accounting for all raw materials, excluding water), speed 1000rpm, stirring time 8min; Add inorganic thermal insulation powder fumed silica, the content is 40wt% (accounting for all raw materials, excluding water), the speed is 1000rpm, and the stirring time is 10min; Adding surface-modified SiC with an average particle size of 5 μm and a content of 0.2 wt% (of all raw materials, excluding water); Aluminum silicate fiber was added, with a content of 55.9 wt% (accounting for all raw materials, excluding water), the rotation speed was 1000 rpm, and the stirring time was 8 min; the prepared slurry was pumped into a headbox, and the sheet was made by filtering water through a papermaking machine; By means of surface glue spraying, a 50wt% sodium silicate aqueous solution is sprayed onto the surface of the sheet at a controlled flow rate. The sheet passes through the glue spraying head at a rate of 1.8 m / min, and negative pressure suction is performed under the sheet to make the sodium silicate evenly distributed inside the material; the sodium silicate colloid content is 2wt% (of all raw materials, excluding water); Dry in a drying oven at 130°C for 10 minutes.
[0070] (2) Preparation of thermal insulation layer in medium temperature zone: Add water to the dispersion tank; Add dispersant silane coupling agent KH550, content 0.9wt% (accounting for all raw materials, excluding water), wetting agent sodium carboxymethyl cellulose, content 1wt% (accounting for all raw materials, excluding water), speed 1000rpm, stirring time 8min; Add inorganic thermal insulation powder fumed silica, the content is 40wt% (accounting for all raw materials, excluding water), the speed is 1000rpm, and the stirring time is 10min; Add surface-modified SiC with an average particle size of 3 μm and a content of 0.3% (to all raw materials, excluding water); Aluminum silicate fiber was added, with a content of 55.8 wt% (accounting for all raw materials, excluding water), the rotation speed was 1000 rpm, and the stirring time was 8 min; the prepared slurry was pumped into a headbox, and the sheet was made by filtering water through a papermaking machine; By means of surface glue spraying, a 50wt% sodium silicate aqueous solution is sprayed onto the surface of the sheet at a controlled flow rate. The sheet passes through the glue spraying head at a rate of 1.8 m / min, and negative pressure suction is performed under the sheet to make the sodium silicate evenly distributed inside the material; the sodium silicate colloid content is 2wt% (of all raw materials, excluding water); Dry in a drying oven at 130°C for 10 minutes.
[0071] (3) Preparation of thermal insulation layer in high temperature area: Add water to the dispersion tank; Add dispersant silane coupling agent KH550, content 0.9wt% (accounting for all raw materials, excluding water), wetting agent sodium carboxymethyl cellulose, content 1wt% (accounting for all raw materials, excluding water), speed 1000rpm, stirring time 8min; Add inorganic thermal insulation powder fumed silica, the content is 40wt% (accounting for all raw materials, excluding water), the speed is 1000rpm, and the stirring time is 10min; Adding surface-modified SiC with an average particle size of 1.5 μm and a content of 0.5 wt% (of all raw materials, excluding water); Aluminum silicate fiber is added, the content is 55.6wt% (accounting for all raw materials, excluding water), the rotation speed is 1000rpm, and the stirring time is 8min; by means of surface glue spraying, the flow rate is controlled to spray a 50wt% sodium silicate aqueous solution onto the surface of the sheet, the sheet passes through the glue spraying head at a rate of 1.8 meters / min, and negative pressure suction is performed under the sheet to make the sodium silicate evenly distributed inside the material; the sodium silicate colloid content is 2wt% (accounting for all raw materials, excluding water); The prepared slurry is pumped into the headbox and the sheet is made by filtering water through the papermaking machine; Dry in a drying oven at 130°C for 10 minutes.
[0072] (4) A high temperature zone insulation layer (single layer thickness of 1 mm, number of layers of 1 layer), a medium temperature zone insulation layer (single layer thickness of 1 mm, number of layers of 1 layer), and a low temperature zone insulation layer (single layer thickness of 1 mm, number of layers of 1 layer) are sequentially stacked and vacuum packaged with a PET film to obtain a multi-temperature zone multilayer composite insulation material.
[0073] The preparation method of surface-modified SiC in the above preparation method is: adding SiC to a 98 vol% ethanol aqueous solution containing 5 wt% of γ-methacryloxypropyltrimethoxysilane to prepare a dispersion containing 10 wt% of SiC, mechanically stirring the reaction for 30 minutes under heating conditions of 60°C, filtering, and drying to obtain SiC with alkenyl grafted on the surface. Adding the SiC with alkenyl grafted on the surface to an ethanol solution containing 1.5 wt% of acrylic acid at a mass ratio of 1:10, ultrasonically treating until uniformly dispersed, irradiating the obtained dispersion with high-energy electron beam energy (energy of 50 kGy) in nitrogen, filtering the obtained product, washing it with ethanol three times, and vacuum drying to obtain SiC with polyacrylic acid grafted on the surface.
[0074] Test Example 11 The difference between this test example and test example 10 is that the preparation method of surface modified SiC is different: SiC is added to a 98 vol% ethanol aqueous solution containing 5 wt% of γ-methacryloxypropyltrimethoxysilane to prepare a dispersion containing 10 wt% of SiC, and the reaction is mechanically stirred for 30 minutes under heating conditions of 60°C, filtered, and dried to obtain SiC with alkenyl grafted on the surface. SiC with alkenyl grafted on the surface is added to an ethanol solution containing 2.5 wt% of acrylic acid at a mass ratio of 1:10, and ultrasonically treated until uniformly dispersed, and the resulting dispersion is irradiated with high-energy electron beam energy (energy of 50 kGy) in nitrogen, and the resulting product is filtered, washed with ethanol 3 times, and vacuum dried to obtain SiC with polyacrylic acid grafted on the surface.
[0075] Test Example 12 The difference between this test example and test example 10 is that the preparation method of surface modified SiC is different: SiC is added to a 98 vol% ethanol aqueous solution containing 5 wt% of γ-methacryloxypropyltrimethoxysilane to prepare a dispersion containing 10 wt% of SiC, and the reaction is mechanically stirred for 30 minutes under heating conditions of 60°C, filtered, and dried to obtain SiC with alkenyl grafted on the surface. SiC with alkenyl grafted on the surface is added to an ethanol solution containing 1.2 wt% of acrylic acid and 0.3 wt% of acrylic acid phosphate at a mass ratio of 1:10, and ultrasonically treated until uniformly dispersed, and the resulting dispersion is irradiated with high-energy electron beam energy (energy of 50 kGy) in nitrogen, and the resulting product is filtered, washed with ethanol 3 times, and vacuum dried to obtain SiC with polyacrylic acid grafted on the surface.
[0076] Performance Testing The performance of the composite thermal insulation materials obtained in Test Examples 10-12 was tested and compared with that in Test Example 7. The test results are shown in Table 3: Table 3 It can be seen from the data in Table 3 that compared with Test Example 7, the surface modified SiC used in Test Examples 10-12. Among them, from the comparison of Test Examples 9-11, it can be found that the use of an appropriate amount of acrylic acid (Test Example 10) and SiC copolymerization modification has a positive effect on the thermal insulation performance of the composite thermal insulation material, but if the amount of acrylic acid is too high (Test Example 11), it will have a negative effect. This may be that the excessive amount of polyacrylic acid grafting will cause the surface of the SiC particles to be wrapped in a large area, thereby affecting its performance. In addition, it can be seen from Test Example 12 that the thermal insulation performance of the composite thermal insulation material can be further improved by doping an appropriate amount of acrylic acid phosphate during copolymerization modification.
[0077] The raw materials and equipment used in the present invention, unless otherwise specified, are all commonly used raw materials and equipment in the art; the methods used in the present invention, unless otherwise specified, are all conventional methods in the art.
[0078] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A multi-temperature zone multi-layer composite thermal insulation material, Features: The heat source comprises, in order from near to far, at least one high temperature zone heat insulation layer, at least one medium temperature zone heat insulation layer and at least one low temperature zone heat insulation layer; The high temperature zone insulation layer, the medium temperature zone insulation layer and the low temperature zone insulation layer all include an inorganic fiber substrate, an inorganic insulation powder, SiC particles and sodium silicate colloid dispersed in the inorganic fiber substrate; The particle sizes of the shading particles in the high temperature zone insulation layer, the medium temperature zone insulation layer and the low temperature zone insulation layer are 1.3-2.5 μm, 2.5-4 μm and 4-7 μm respectively, and the contents are 0.4-0.6 wt%, 0.3-0.35 wt% and 0.1-0.2 wt% respectively.
2. The multi-temperature zone multi-layer composite thermal insulation material according to claim 1, Features: The thermal insulation temperatures of the high temperature zone thermal insulation layer, the medium temperature zone thermal insulation layer and the low temperature zone thermal insulation layer are 500-800°C, 300-500°C and <300°C respectively.
3. The multi-temperature zone multi-layer composite thermal insulation material according to claim 1 or 2, Features: The content of the inorganic fiber substrate in the high temperature zone insulation layer, the medium temperature zone insulation layer and the low temperature zone insulation layer is 30-70wt%, the content of the inorganic insulation powder is 20-50wt%, and the content of the sodium silicate colloid is 1-3wt%.
4. The multi-temperature zone multi-layer composite thermal insulation material according to claim 1 or 2, Features: The material of the inorganic fiber substrate is selected from one or more of glass fiber, high silica fiber, aluminum silicate fiber, alkaline earth silicate fiber and mullite fiber; The inorganic heat-insulating powder is selected from one or more of inorganic aerogel powder, fumed silica, precipitated silica, hollow glass microspheres, hollow ceramic microspheres, expanded vermiculite and expanded perlite.
5. The multi-temperature zone multi-layer composite thermal insulation material according to claim 1 or 2, Features: After 5 minutes at 700℃, 0.9MPa and pressure, the cold surface temperature is ≤110℃.
6. A method for preparing the multi-temperature zone multi-layer composite thermal insulation material according to any one of claims 1 to 5, Features include: 1) Add dispersant and wetting agent to water and stir well, then add inorganic thermal insulation powder, SiC particles and inorganic fiber in sequence and stir well after each addition to obtain slurry; The slurry is paper-made, and the water is filtered to obtain a sheet, and then a sodium silicate aqueous solution is sprayed on the surface of the sheet by means of surface spraying glue, and the sheet is vacuum-sucked and dried to obtain a high-temperature zone insulation layer, a medium-temperature zone insulation layer, and a low-temperature zone insulation layer respectively; 2) The high temperature zone insulation layer, the medium temperature zone insulation layer and the low temperature zone insulation layer are stacked in sequence to obtain a multi-temperature zone multi-layer composite insulation material.
7. The preparation method according to claim 6, Features: The surface of the SiC particles is grafted with polyacrylic acid, and the preparation method thereof is as follows: SiC particles are modified with an alkenyl-containing silane coupling agent to obtain SiC particles with alkenyl grafted on the surface, and the SiC particles are copolymerized with acrylic acid monomers under high-energy electron beam irradiation; during the high-energy electron beam irradiation, the energy of the high-energy electron beam is 30-60 kGy, and the amount of acrylic acid used is 10-20wt% of the SiC particles.
8. The preparation method according to claim 7, Features: The copolymerized monomers also include acrylic acid phosphate, and the mass ratio of acrylic acid to acrylic acid phosphate is (4-6):
1.
9. The preparation method according to claim 7, Features: The dispersant is selected from one or more of polyvinyl alcohol, polyethylene oxide, silane coupling agent, sodium dodecylbenzene sulfonate and sodium isopropylnaphthalene sulfonate; The wetting agent is selected from one or more of sodium hydroxyethyl cellulose, sodium carboxymethyl cellulose, bentonite and diatomaceous earth.
10. The preparation method according to claim 6, Features: In the raw materials of the high temperature zone heat insulation layer, the medium temperature zone heat insulation layer and the low temperature zone heat insulation layer, the dispersant accounts for 0.5-5wt% and the wetting agent accounts for 0.5-5wt%.
Citation Information
Patent Citations
High-performance multi-layer thin-mat composite thermal insulation material and manufacturing method thereof
CN103449777A
Multilayer-arranged heat insulating material and preparation method thereof
CN105330212A
Aerogel gradient thermal insulation material containing endothermic opacifying agent
CN107696630A
Gradient nano thermal insulation material and preparation method thereof
CN110511048A
Electrically conducting-inorganic substance-containing silicon carbide-based fine particles, electromagnetic wave absorbing material and electromagnetic wave absorber
US20070062719A1
Cited By
Heat insulation pad for battery and battery pack
CN122025935A
Thermal insulation pad for a battery and battery pack
CN122025935B