Petroleum asphalt-based amphiphilic carbon material for preparing carbon ink and preparation method of petroleum asphalt-based amphiphilic carbon material
Through the combined use of petroleum pitch-based amphiphilic carbon materials and carbon black, the problems of slow drying speed and writing smearing of carbon ink are solved, achieving fast drying and good tinting strength and water resistance, making it suitable for students.
Patent Information
- Application Number
- CN202410826952.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-10-29
AI Technical Summary
Existing carbon ink dries slowly, easily causing local contamination and writing smear, affecting text clarity.
Petroleum asphalt-based amphiphilic carbon material and carbon black are used as colorants, and the affinity between the material and water is enhanced through a mixed acid oxidation method to improve the coloring ability and water resistance of the ink and achieve rapid drying.
The combined use of petroleum asphalt-based amphiphilic carbon materials and carbon black improves the coloring power and water resistance of the ink, avoids smearing, and is suitable for students.
Smart Images

Figure BDA0004910788440000071 
Figure BDA0004910788440000091 
Figure BDA0004910788440000101
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of raw materials for office supplies, and relates to a petroleum asphalt-based amphiphilic carbon material for preparing carbon ink and a preparation method thereof. Background Art
[0002] As a type of black ink, carbon ink has thick and shiny handwriting, and the black and white on the paper are very eye-catching. Carbon ink is often made of carbon black material that is insoluble in water. Carbon black is a kind of amorphous carbon. As a colorant, carbon black has good stability, strong adhesion, and stable chemical properties. Since carbon is chemically stable at room temperature and pressure and is not easy to react with other substances, text materials written in carbon ink are easy to store for a long time and never fade. Carbon ink has the properties of cold resistance, water resistance, heat resistance, light resistance, chemical corrosion resistance, etc., and has strong covering power.
[0003] The traditional production method of carbon ink in my country began in the early 1960s, using chemical oxidation, that is, using oxidants such as concentrated nitric acid, potassium permanganate, potassium dichromate, hydrogen peroxide, etc. to oxidize carbon black, so that the surface of carbon black particles has hydrophilic groups such as carboxyl and hydroxyl groups to produce strong hydrophilicity. Although this method is feasible, it is costly and takes 20-32 hours to oxidize, which is a long time.
[0004] Chinese patent CN201811237441.8 discloses a carbon ink, which is prepared by oxidizing carbon black with nitric acid to give it a polar group on its surface, and then grafting glycerol molecules on the surface of carbon black to enhance the affinity between carbon black and water, and also improve the dispersibility of carbon black. This invention method improves the affinity between carbon black particles and water, and prolongs the intermittent writing time of this carbon ink. This method still involves oxidation of carbon black, which is costly and has certain limitations.
[0005] In the past, there was a problem during use. That is, carbon ink dried slowly and took a long time, causing local contamination of clothing or palms, and also causing the phenomenon of text smearing, making the text information unclear. Summary of the invention
[0006] In order to overcome the shortcomings of the prior art, the present invention provides a petroleum asphalt-based amphiphilic carbon material for preparing carbon ink and a preparation method thereof, and the petroleum asphalt-based amphiphilic carbon material and the preparation method thereof are feasible in process. The petroleum asphalt-based amphiphilic carbon material prepared by the method of the present invention has a strong affinity for water. Compared with a single carbon black colorant, the use of this petroleum asphalt-based amphiphilic carbon material and carbon black as a colorant improves the coloring ability and water resistance of the ink. The petroleum asphalt-based amphiphilic carbon material and carbon black prepared by the present invention are used in combination as a colorant, and the prepared carbon ink has good coloring power and water resistance, can be quickly dried in a shorter time, and avoids the phenomenon of smearing.
[0007] The above object of the present invention is achieved through the following technical solutions:
[0008] A method for preparing a petroleum asphalt-based amphiphilic carbon material comprises the following steps:
[0009] (1) Raw material pretreatment:
[0010] a. The raw material petroleum asphalt resin is crushed with a pulverizer, and then ball-milled with a ball mill. The ball-milled resin powder is passed through 500 mesh and 400 mesh ultrasonic vibrating screens, and the resin powder with a particle size between 29μm-37μm is intercepted. The median particle size D50 = 32.14μm is detected by a laser particle size analyzer, and the sealed and stored in a desiccator for standby use;
[0011] b.. The raw material petroleum asphalt resin is crushed by a pulverizer, and then ball-milled by a ball mill. The ball-milled resin powder is passed through 300-mesh and 200-mesh ultrasonic vibration screens respectively, and the resin powder with a particle size between 49μm and 74μm is intercepted. The median particle size D50 is 60.06μm after detection by a laser particle size analyzer. The powder is sealed and stored in a desiccator for later use;
[0012] c. The raw petroleum asphalt resin is crushed by a pulverizer, and then ball-milled by a ball mill. The ball-milled resin powder is passed through 150 mesh and 105 mesh ultrasonic vibration screens, and the resin powder with a particle size between 98μm and 141μm is intercepted. The median particle size D50 is 125.3μm after detection by a laser particle size analyzer. The powder is sealed and stored in a desiccator for later use;
[0013] d. The raw petroleum asphalt resin was crushed with a pulverizer, and then ball-milled with a ball mill. The ball-milled resin powder was sieved through a 75-mesh sieve and a 60-mesh sieve, and the resin powder with a particle size between 197 μm and 247 μm was intercepted. The median particle size D50 was 230.2 μm after detection by a laser particle size analyzer, and the resin powder was sealed and stored in a desiccator for later use;
[0014] (2) Oxidation:
[0015] A mixed acid composed of concentrated sulfuric acid and concentrated nitric acid is placed in a two-mouthed glass flask, a condenser is connected to the flask, and cooling water is refluxed through the condenser. Any of the spare raw materials obtained in step a, b, c, and d in step (1) is slowly and intermittently added to the mixed acid, and stirred continuously. After the addition is completed, the bottle mouth is plugged with a glass stopper, and heated to a specified temperature to cause an oxidation reaction, and the reaction is kept at a constant temperature for a period of time.
[0016] (3) Filtration:
[0017] After the reaction of step (2) is completed, pour all the products in the flask (including a mixture of part of the precipitate, part of the suspended matter and the remaining sulfuric acid, nitric acid, etc.) into deionized water, and the volume ratio of the product to deionized water is 1:4-7; terminate the reaction and let it stand for 12 hours. Use a glass filtration device and Whatman filter paper to filter to obtain a filter cake. The filtrate is neutralized with sodium carbonate solution and discharged after meeting the standards.
[0018] (4) Washing:
[0019] The filter cake obtained by suction filtration in step (3) is washed with deionized water until it becomes neutral.
[0020] (5) Drying:
[0021] The filter cake obtained by washing in step (4) is placed in an oven and dried at 105°C±5°C to obtain a petroleum asphalt-based amphiphilic carbon material after mixed acid oxidation.
[0022] Furthermore, in step (1), the petroleum asphalt resin is obtained by distilling ethylene cracking tar to remove light components and then thermally polymerizing the petroleum asphalt resin. The petroleum asphalt resin has a coking value of 58.31%, a sulfur content of 0.1%, an ash content of 0.032%, a softening point of 202.5°C, and a density of 0.9715 g / cm at 20°C. 3 , the soluble element content is as follows:
[0023] Lead Chromium Cr CadmiumCd Arsenic Antimony Sb Mercury Selenium Barium 0.185 0.358 0.000 0.000 0.000 0.205 0.102 0.000
[0024] The unit of each element content in the table is ppm.
[0025] Furthermore, in step (2), the mixed acid is a mixed acid composed of concentrated sulfuric acid with a mass percentage concentration of 98% and concentrated nitric acid with a mass percentage concentration of 65%, the volume ratio of concentrated sulfuric acid to concentrated nitric acid is 7:3, the ratio of the solid content of the petroleum asphalt resin reacted with the mixed acid to the mixed acid is 1g:10-30ml, the reaction temperature is 40°C-50°C, the stirring rate is 800-850r / min, and the reaction time is 6-8 hours.
[0026] Furthermore, in step (3), the conductivity of the deionized water is 0.055 μS / cm; the pore size of the Whatman filter paper is 1.5 μm;
[0027] Furthermore, in step (4), the filter cake obtained after suction filtration in step (3) is washed with deionized water, and the filtrate is tested to be neutral;
[0028] Furthermore, in step (5), the filter cake obtained after washing in step (4) is placed in an oven at 105±5°C and dried for 8 hours to obtain a petroleum asphalt-based amphiphilic carbon material oxidized by mixed acid.
[0029] The performance indicators of the petroleum asphalt-based amphiphilic carbon material for preparing carbon ink prepared by the above preparation method are: contact angle with water is 44.60°-75.09°, color depth K / S is 6.74-6.87, and pH value is 2.26-2.56.
[0030] The application of the petroleum asphalt-based amphiphilic carbon material prepared by the above preparation method in the preparation of carbon ink is as follows:
[0031] The petroleum asphalt-based amphiphilic carbon material is used to prepare carbon ink, which specifically includes the following steps:
[0032] (a) grinding 23-30% of the total mass of low-structured carbon black without surface treatment and 8-12% of the total mass of petroleum asphalt-based amphiphilic carbon material, drying them at 95° C.-105° C. for 20-30 h, taking them out and storing them in a desiccator for later use;
[0033] (b) weighing 0.05-1% of methyl silicone oil, 1-2% of gelatin, 0.05-0.15% of triethylamine, 0.03-0.08% of polyvinyl alcohol, 0.05-0.1% of sodium benzoate, 0.01-0.02% of nano titanium dioxide, 0.02-0.04% of nano zinc oxide and 30-40% of deionized water in proportion to the total mass, mixing and stirring evenly;
[0034] (c) adding 10-15% of the total mass of alkali-swellable acrylic acid and stirring evenly to prepare a mother solution for standby use;
[0035] (d) adding 3-4% of the total mass of the dispersant naphthol polyoxyethylene ether, pretreated carbon black and amphiphilic carbon material to the reserved mother liquid, and stirring evenly to obtain liquid A;
[0036] (e) dispersing the liquid A obtained in step (d) by ultrasonic oscillation for 40-50 minutes to obtain liquid B;
[0037] (f) centrifuging the liquid B obtained in step (e) for 10 minutes to remove the precipitate to obtain liquid C;
[0038] (g) adding 8-15% of anhydrous ethanol to the liquid C obtained in step (f), dispersing the mixture by ultrasonic oscillation for 10-15 minutes, and degassing the mixture under vacuum for 30 minutes to obtain carbon ink.
[0039] The invention uses petroleum asphalt resin as raw material, adopts mixed acid for oxidation, and sequentially undergoes oxidation, filtration, washing and drying processes to prepare the petroleum asphalt-based amphiphilic carbon material for carbon ink.
[0040] The petroleum asphalt-based amphiphilic carbon material provided by the present invention has a petroleum asphalt resin itself which is a non-polar organic mixture insoluble in water. The resin particles undergo oxidation, nitration and sulfonation reactions with concentrated sulfuric acid and concentrated nitric acid. The number of hydrophilic polar groups on the surface of the resin particles increases after mixed acid oxidation, so that the affinity of the petroleum asphalt-based amphiphilic carbon material with water is greatly enhanced. The petroleum asphalt-based amphiphilic carbon material is used for the preparation of carbon ink and can be used together with carbon black as a colorant to enhance the coloring ability and water resistance of the ink.
[0041] The beneficial effects of the present invention compared with the prior art are:
[0042] 1. Using petroleum asphalt resin as raw material, the mixed acid oxidation method is used to make the surface of petroleum asphalt resin particles have many hydrophilic polar groups, which greatly enhances the affinity of the petroleum asphalt-based amphiphilic carbon material with water;
[0043] 2. After mixed acid oxidation, the petroleum asphalt-based amphiphilic carbon material is obtained, which can be used as a colorant together with carbon black to enhance the coloring ability and water resistance of the ink.
[0044] 3. The present invention aims to provide a petroleum asphalt-based amphiphilic carbon material that can be used for carbon ink and a preparation method thereof. The present invention uses petroleum asphalt resin as raw material and adopts a mixed acid oxidation method to broaden the application scope of petroleum asphalt resin and enrich the new idea of preparing colorants used in carbon ink; the prepared petroleum asphalt-based amphiphilic carbon material and carbon black are used in combination as carbon ink colorants to enhance the coloring ability and water resistance of the ink. The carbon ink prepared with this amphiphilic carbon material can achieve rapid drying and avoid smearing, and is suitable for students. DETAILED DESCRIPTION
[0045] The present invention is described in detail below by specific examples, but the protection scope of the present invention is not limited. Unless otherwise specified, the experimental methods used in the present invention are all conventional methods, and the experimental equipment, materials, reagents, etc. used can be obtained from commercial channels.
[0046] The amphiphilic carbon material prepared by the method of the present invention makes the surface of the petroleum asphalt resin particles rich in hydrophilic polar groups such as hydroxyl, carboxyl, sulfonic acid, etc. The amphiphilic material has a strong affinity for water and has the characteristics of ordinary asphalt. The amphiphilic carbon material belongs to a petroleum asphalt-based amphiphilic carbon material.
[0047] The detection items and detection methods in the present invention include:
[0048] Average particle size of petroleum asphalt resin: Laser particle size analyzer
[0049] Element content analysis: Inductively coupled plasma optical emission spectrometer
[0050] Water resistance: Tested according to the method specified in "QB / T1745.2-2018 Fountain Pen Ink Part 2: Carbon Ink"
[0051] Chroma: Tested according to the method specified in "QB / T1745.2-2018 Fountain Pen Ink Part 2: Carbon Ink"
[0052] Contact Angle: Surface Tensiometer
[0053] Volatile matter: Tested in accordance with "GB / T7047-2006 Determination of volatile matter content of pigment carbon black"
[0054] Intermittent writing time: Tested according to the method specified in "QB / T1745.2-2018 Fountain Pen Ink Part 2: Carbon Ink"
[0055] Volatile organic compound content VOCs: refers to the percentage of the mass of organic matter that can volatilize at room temperature and pressure in carbon ink to the total mass of ink; tested in accordance with the determination method of volatile organic compounds (VOCs) content in ink GB / T38608-2020
[0056] Color depth K / S: Use a colorimeter to test the color intensity K / S value of the sample under D65 light source and 10° standard observation angle. Each sample is measured 3 times at random locations and the average value is taken.
[0057] Example 1
[0058] In this embodiment, the raw material petroleum asphalt resin is subjected to mixed acid oxidation, filtration, washing, and drying processes to prepare an amphiphilic carbon material for carbon ink.
[0059] The raw material petroleum asphalt resin is a black solid powder block with a coking value of 58.31%, a total sulfur content of 0.10%, an ash content of 0.032%, a softening point of 202.5℃, and a density of 0.9715g / cm at 20℃. 3 .
[0060] (1) Raw material pretreatment: The raw material petroleum asphalt resin is crushed by a pulverizer, and then ball-milled by a ball mill. The ball-milled resin powder is passed through 500-mesh and 400-mesh ultrasonic vibration screens respectively, and the resin powder with a particle size between 29 μm and 37 μm is intercepted. The median particle size D50 is 32.14 μm after detection by a laser particle size analyzer. The resin powder is sealed and stored in a desiccator for future use;
[0061] (2) Mixed acid oxidation: 100 g of the petroleum asphalt resin pretreated in step (1) was slowly and intermittently added to a mixed acid consisting of 98% by mass concentrated sulfuric acid and 65% by mass concentrated nitric acid in a volume ratio of 7:3. The stirring rate was continuously 830 r / min. The ratio of the resin solid content to the mixed acid was 1 g:16 ml. After the addition was completed, the temperature was raised and maintained at 43.6°C to allow an oxidation reaction to occur. The reaction time was 7.5 hours.
[0062] (3) Filtration: After the reaction in step (2) is completed, the product (a mixture of part of the precipitate, part of the suspended matter and the remaining sulfuric acid, nitric acid, etc. in the flask) is poured into deionized water to terminate the reaction. The volume ratio of the product to deionized water is 1:5; let it stand for 12 hours. Use Whatman filter paper with a pore size of 1.5 microns and filter with a glass filtration device to obtain a filter cake.
[0063] (4) Washing: The filter cake obtained after suction filtration in step (3) is washed with deionized water until the filtrate is neutral upon detection.
[0064] (5) Drying: The neutral product obtained after washing in step (4) is placed in an oven and dried at 105±5°C for 8 hours to obtain a solid resin product after mixed acid oxidation, which is the amphiphilic carbon material. The test results of the amphiphilic carbon material after mixed acid oxidation are shown in Table 1.
[0065] Embodiment 2:
[0066] In step (1), the raw material is pretreated as follows: the raw material petroleum asphalt resin is crushed by a pulverizer, and then ball-milled by a ball mill. The ball-milled resin powder is passed through a 300-mesh and a 200-mesh ultrasonic vibration sieve, respectively, and the resin powder with a particle size between 49 μm and 74 μm is intercepted. The median particle size D50 is 60.06 μm after detection by a laser particle size analyzer, and the resin powder is sealed and stored in a desiccator for later use;
[0067] The ratio of resin solid content to mixed acid is 1g:16ml. After the addition is completed, the temperature is raised and maintained at 43.6°C to allow oxidation reaction to occur for 7.5 hours. Others are the same as in Example 1. The test results of the amphiphilic carbon material after mixed acid oxidation are shown in Table 1.
[0068] Embodiment 3:
[0069] In step (1), the raw material is pretreated by crushing the raw material petroleum asphalt resin with a pulverizer, then ball milling with a ball mill, passing the ball-milled resin powder through 150 mesh and 105 mesh ultrasonic vibration screens respectively, intercepting the resin powder with a particle size between 98 μm and 141 μm, and detecting it with a laser particle size analyzer, the median particle size D50 = 125.3 μm, and sealing and storing it in a desiccator for later use;
[0070] The ratio of resin solid content to mixed acid is 1g:16ml. After the addition is completed, the temperature is raised and maintained at 43.6°C to allow oxidation reaction to occur for 7.5 hours. Others are the same as in Example 1. The test results of the amphiphilic carbon material after mixed acid oxidation are shown in Table 1.
[0071] Embodiment 4:
[0072] In step (1), the raw material is pretreated by crushing the raw material petroleum asphalt resin with a pulverizer, then ball milling with a ball mill, passing the ball-milled resin powder through a 60-mesh sieve and a 75-mesh sieve respectively, intercepting the resin powder with a particle size between 200 μm and 250 μm, and detecting it with a laser particle size analyzer, the median particle size D50 is 230.2 μm, and the resin powder is sealed and stored in a desiccator for later use;
[0073] The ratio of resin solid content to mixed acid is 1g:26ml. After the addition is completed, the temperature is raised and maintained at 50°C to allow oxidation reaction to occur for 7.5 hours. Other conditions are the same as in Example 1. The comparison of the test results of the amphiphilic carbon material after mixed acid oxidation and the raw material is shown in Table 1.
[0074] Table 1 Technical index test and raw material comparison data of amphiphilic carbon materials
[0075]
[0076]
[0077] The contact angle is the measured contact angle between the resin material and water.
[0078] From the test results in Table 1, it can be seen that the original contact angle of the raw petroleum asphalt resin with water before oxidation is large, and the contact angle with water after mixed acid oxidation is significantly reduced, indicating that the affinity of the petroleum asphalt resin with water is greatly enhanced after oxidation; after the raw petroleum asphalt resin is oxidized by mixed acid, the resin color depth K / S is reduced to a certain extent, but it is not much different from that before oxidation. It can be considered that the color performance of the amphiphilic carbon material obtained after mixed acid oxidation has not changed significantly. The volatile matter is greater than 8% and the pH value is less than 3, which fully demonstrates that under the process conditions of the present invention, the surface physical properties and electrochemical properties of the prepared amphiphilic carbon material have changed significantly. This is because the surface of the amphiphilic carbon material carries a considerable number of oxygen-containing functional groups.
[0079] Application Example 1:
[0080] The amphiphilic carbon material prepared in Example 1 is used to prepare carbon ink, comprising the following steps:
[0081] S1. Grind 300 g of low-structured carbon black without surface treatment and 120 g of amphiphilic carbon material accounting for 12% of the total mass fraction, dry them at 95°C-105°C for 20-30h, take them out and put them in a dryer for later use;
[0082] S2. Weigh 0.5 g of methyl silicone oil, 17 g of gelatin, 1.4 g of triethylamine, 0.3 g of polyvinyl alcohol, 0.5 g of sodium benzoate, 0.1 g of nano-titanium dioxide, 0.2 g of nano-zinc oxide and 300 g of deionized water in proportion and mix and stir evenly;
[0083] S3. Add 150 g of alkali-swellable acrylic acid and stir well as a spare mother liquor;
[0084] S4. Add 30 g of naphthol polyethylene ether dispersant, pretreated carbon black and amphiphilic carbon material to the reserved mother liquor and stir evenly to obtain liquid A;
[0085] S5. Disperse the solution A obtained in step S4 by ultrasonic oscillation for 40-50 minutes to obtain solution B;
[0086] S6. Centrifuge the liquid B obtained in step S5 for 10 minutes to remove the precipitate to obtain liquid C;
[0087] S7. Add 80 grams of anhydrous ethanol to the liquid C obtained in step S6, disperse under ultrasonic oscillation for 10-15 minutes, and degas under vacuum for 30 minutes to obtain carbon ink. The indicators of the carbon ink prepared with the amphiphilic carbon material are measured, and the test data are shown in Table 2.
[0088] Application Example 2
[0089] The amphiphilic carbon material prepared in Example 2 is used to prepare carbon ink, comprising the following steps:
[0090] S1. Grind 240 g of low-structured carbon black without surface treatment and 100 g of amphiphilic carbon material accounting for 10% of the total mass fraction, dry them at 95°C-105°C for 20-30h, take them out and put them in a dryer for later use;
[0091] S2. Weigh 0.8 g of methyl silicone oil, 10 g of gelatin, 1.5 g of triethylamine, 0.5 g of polyvinyl alcohol, 0.8 g of sodium benzoate, 0.1 g of nano-titanium dioxide, 0.3 g of nano-zinc oxide and 380 g of deionized water in proportion and mix and stir evenly;
[0092] S3. Add 120 g of alkali-swellable acrylic acid and stir well as a spare mother liquor;
[0093] S4. Add 36 g of naphthol polyethylene ether dispersant, pretreated carbon black and amphiphilic carbon material to the reserved mother liquor and stir evenly to obtain liquid A;
[0094] S5. Disperse the solution A obtained in step S4 by ultrasonic oscillation for 40-50 minutes to obtain solution B;
[0095] S6. Centrifuge the liquid B obtained in step S5 for 10 minutes to remove the precipitate to obtain liquid C;
[0096] S7. Add 110 g of anhydrous ethanol to the liquid C obtained in step S6, disperse under ultrasonic oscillation for 10-15 minutes, and degas under vacuum for 30 minutes to obtain carbon ink. The indicators of the carbon ink prepared with the amphiphilic carbon material are measured, and the test data are shown in Table 2.
[0097] Application Example 3
[0098] The amphiphilic carbon material prepared in Example 3 is used for preparing carbon ink, comprising the following steps:
[0099] S1. Grind 260 g of low-structured carbon black without surface treatment and 90 g of amphiphilic carbon material accounting for 9% of the total mass fraction, dry them at 95°C-105°C for 20-30h, take them out and put them in a dryer for later use;
[0100] S2. Weigh 0.7 g of methyl silicone oil, 13 g of gelatin, 0.75 g of triethylamine, 0.45 g of polyvinyl alcohol, 0.7 g of sodium benzoate, 0.15 g of nano-titanium dioxide, 0.25 nano-zinc oxide and 350 g of deionized water in proportion and mix and stir evenly;
[0101] S3. Add 130 g of alkali-swellable acrylic acid and stir well as a spare mother liquor;
[0102] S4. Add 34 g of naphthol polyethylene ether dispersant, pretreated carbon black and amphiphilic carbon material to the reserved mother liquor and stir evenly to obtain liquid A;
[0103] S5. Disperse the solution A obtained in step S4 by ultrasonic oscillation for 40-50 minutes to obtain solution B;
[0104] S6. Centrifuge the liquid B obtained in step S5 for 10 minutes to remove the precipitate to obtain liquid C;
[0105] S7. Add 120 g of anhydrous ethanol to the liquid C obtained in step S6, disperse under ultrasonic oscillation for 10-15 minutes, and degas under vacuum for 30 minutes to obtain carbon ink. The indicators of the carbon ink prepared with the amphiphilic carbon material are measured, and the test data are shown in Table 2.
[0106] Application Example 4
[0107] The amphiphilic carbon material prepared in Example 4 is used for preparing carbon ink, comprising the following steps:
[0108] S1. Grind 240 g of low-structured carbon black without surface treatment and 90 g of amphiphilic carbon material accounting for 9% of the total mass fraction, dry them at 95°C-105°C for 20-30h, take them out and put them in a dryer for later use;
[0109] S2. Weigh 0.6 g of methyl silicone oil, 20 g of gelatin, 0.5 g of triethylamine, 0.6 g of polyvinyl alcohol, 0.9 g of sodium benzoate, 0.15 of nano-titanium dioxide, 0.25 of nano-zinc oxide and 340 g of deionized water according to the proportion, and stir evenly;
[0110] S3. Add 120 g of alkali-swellable acrylic acid and stir well as a spare mother liquor;
[0111] S4. Add 37 g of naphthol polyethylene ether dispersant, pretreated carbon black and amphiphilic carbon material to the reserved mother liquor and stir evenly to obtain liquid A;
[0112] S5. Disperse the solution A obtained in step S4 by ultrasonic oscillation for 40-50 minutes to obtain solution B;
[0113] S6. Centrifuge the liquid B obtained in step S5 for 10 minutes to remove the precipitate to obtain liquid C;
[0114] S7. Add 150 g of anhydrous ethanol to the liquid C obtained in step S6, disperse under ultrasonic oscillation for 10-15 minutes, and degas under vacuum for 30 minutes to obtain carbon ink. The indicators of the carbon ink prepared with the amphiphilic carbon material are measured, and the test data are shown in Table 2.
[0115] Application Comparative Example 1.
[0116] According to the preparation method of Example 1, low-structure carbon black without surface treatment is used as a single colorant in this comparative example, and the oil absorption value is less than 100×10 -5 m 3 / kg, the particle size after grinding is ≤1μm, the particle size of the carbon black is 0.4μm≤D90≤0.5μm, the particle size is normally distributed and ﹤1.5, used as a control. The test data is shown in Table 2. Among them, D90 refers to the volume Dv90, the same below.
[0117] Application Comparative Example 2.
[0118] According to the preparation method of the above-mentioned comparative example 1, the low-structured carbon black without surface treatment is used as the single colorant in this comparative example, and the oil absorption value is less than 100×10 -5 m 3 / kg, the particle size of carbon black after grinding is ≤5 microns, the distribution is normal distribution, D90 = 3.8 μm, used as a control. The test data is shown in Table 2.
[0119] Table 2 Test data of prepared carbon ink
[0120]
[0121]
[0122] Among them, the qualified standard of chromaticity is not less than the advanced contrast color standard; the volatile organic matter content in the ink is less than 0.5%;
[0123] From the test results in Table 2, it can be seen that the carbon ink prepared by the amphiphilic carbon material obtained by oxidizing petroleum asphalt resin with four specifications of D50 particle size of 32.14μm, 60.06μm, 125.3μm and 230.2μm has qualified chromaticity, water resistance greater than 24hr, intermittent writing time greater than 30 minutes; the percentage of lead and chromium is less than 5ppm; and the antioxidant performance reaches level 3.
[0124] The invention uses petroleum asphalt resin as raw material, adopts mixed acid for oxidation, and sequentially undergoes oxidation, filtration, washing and drying processes to prepare the petroleum asphalt-based amphiphilic carbon material for carbon ink.
[0125] The amphiphilic carbon material for carbon ink provided by the present invention has an enhanced affinity for water compared to before oxidation. Compared with a single carbon black colorant, the combination of the petroleum asphalt-based amphiphilic carbon material and carbon black as a colorant improves the coloring ability and water resistance of the ink. The preparation process of the present invention is feasible, and the prepared carbon ink has good coloring power, permeability, and water resistance, can be quickly dried in a short time, and the smear phenomenon is avoided. It is suitable for students to use.
[0126] The above-described embodiments are only preferred embodiments of the present invention, but not all feasible embodiments of the present invention. For those skilled in the art, any obvious changes made thereto without departing from the principles and spirit of the present invention should be considered to be included in the scope of protection of the claims of the present invention.
Claims
1. A method for preparing a petroleum asphalt-based amphiphilic carbon material, Its characteristics are: The following steps are involved: (1) Raw material pretreatment: a. The raw material petroleum asphalt resin is crushed with a pulverizer, and then ball-milled with a ball mill. The ball-milled resin powder is passed through 500 mesh and 400 mesh ultrasonic vibrating screens, and the resin powder with a particle size between 29μm-37μm is intercepted. The median particle size D50 = 32.14μm is detected by a laser particle size analyzer, and the sealed and stored in a desiccator for standby use; b.. The raw material petroleum asphalt resin is crushed by a pulverizer, and then ball-milled by a ball mill. The ball-milled resin powder is passed through 300-mesh and 200-mesh ultrasonic vibration screens respectively, and the resin powder with a particle size between 49μm and 74μm is intercepted. The median particle size D50 is 60.06μm after detection by a laser particle size analyzer. The powder is sealed and stored in a desiccator for later use; c. The raw petroleum asphalt resin is crushed by a pulverizer, and then ball-milled by a ball mill. The ball-milled resin powder is passed through 150 mesh and 105 mesh ultrasonic vibration screens, and the resin powder with a particle size between 98μm and 141μm is intercepted. The median particle size D50 is 125.3μm after detection by a laser particle size analyzer. The powder is sealed and stored in a desiccator for later use; d. The raw petroleum asphalt resin was crushed with a pulverizer, and then ball-milled with a ball mill. The ball-milled resin powder was sieved through a 75-mesh sieve and a 60-mesh sieve, and the resin powder with a particle size between 197 μm and 247 μm was intercepted. The median particle size D50 was 230.2 μm after detection by a laser particle size analyzer, and the resin powder was sealed and stored in a desiccator for later use; (2) Oxidation: A mixed acid composed of concentrated sulfuric acid and concentrated nitric acid is placed in a two-necked glass flask, a condenser is connected to the flask, and cooling water is refluxed through the condenser; any one of the spare raw materials obtained in step a, b, c, and d in step (1) is slowly and intermittently added to the mixed acid, and stirring is continued. After the addition is completed, the bottle mouth is plugged with a glass stopper, and heated to a specified temperature to cause an oxidation reaction, and the reaction is kept at a constant temperature for a period of time; (3) Filtration: After the reaction of step (2) is completed, the product in the flask is poured into deionized water to terminate the reaction and allowed to stand for 12 hours; a glass filtration device is used to filter using whatman filter paper to obtain a filter cake; the filtrate is neutralized with sodium carbonate solution and discharged after reaching the standard; (4) Washing: The filter cake obtained by suction filtration in step (3) is washed with deionized water until it becomes neutral; (5) Drying: The filter cake obtained by washing in step (4) is placed in an oven and dried at 105°C±5°C to obtain a petroleum asphalt-based amphiphilic carbon material after mixed acid oxidation.
2. A method for preparing a petroleum asphalt-based amphiphilic carbon material as claimed in claim 1, Its characteristics are: In step (1), the petroleum asphalt resin is obtained by distilling ethylene cracking tar to remove light components and then thermally polymerizing the petroleum asphalt resin; the petroleum asphalt resin has a coking value of 58.31%, a sulfur content of 0.1%, an ash content of 0.032%, a softening point of 202.5°C, and a density of 0.9715 g / cm at 20°C. 3 , the soluble element content is as follows: The unit of each element content in the table is ppm.
3. A method for preparing a petroleum asphalt-based amphiphilic carbon material as claimed in claim 1, Its characteristics are: In step (2), the mixed acid is a mixed acid composed of concentrated sulfuric acid with a mass percentage concentration of 98% and concentrated nitric acid with a mass percentage concentration of 65%, the volume ratio of concentrated sulfuric acid to concentrated nitric acid is 7:3, the ratio of the solid content of the petroleum asphalt resin reacted with the mixed acid to the mixed acid is 1g:10-30ml, the reaction temperature is 40°C-50°C, the stirring rate is 800-850r / min, and the reaction time is 6-8 hours.
4. A method for preparing a petroleum asphalt-based amphiphilic carbon material as claimed in claim 1, Its characteristics are: In step (3), the conductivity of the deionized water is 0.055 μS / cm; and the pore size of the Whatman filter paper is 1.5 μm.
5. A method for preparing a petroleum asphalt-based amphiphilic carbon material as claimed in claim 1, Its characteristics are: In step (4), the filter cake obtained after suction filtration in step (3) is washed with deionized water, and the filtrate is tested to be neutral.
6. A method for preparing a petroleum asphalt-based amphiphilic carbon material as claimed in claim 1, Its characteristics are: In step (5), the filter cake obtained after washing in step (4) is placed in an oven at 105±5° C. and dried for 8 hours to obtain a petroleum asphalt-based amphiphilic carbon material oxidized by mixed acid.
7. Use of the petroleum asphalt-based amphiphilic carbon material prepared by the method for preparing a petroleum asphalt-based amphiphilic carbon material as described in any one of claims 1 to 6 in preparing carbon ink.
8. The use according to claim 7, Its characteristics are: The petroleum asphalt-based amphiphilic carbon material is used to prepare carbon ink, which specifically includes the following steps: (a) grinding 23-30% of the total mass of low-structured carbon black without surface treatment and 8-12% of the total mass of petroleum asphalt-based amphiphilic carbon material, drying them at 95° C.-105° C. for 20-30 h, taking them out and storing them in a desiccator for later use; (b) weighing 0.05-1% of methyl silicone oil, 1-2% of gelatin, 0.05-0.15% of triethylamine, 0.03-0.08% of polyvinyl alcohol, 0.05-0.1% of sodium benzoate, 0.01-0.02% of nano titanium dioxide, 0.02-0.04% of nano zinc oxide and 30-40% of deionized water in proportion to the total mass, mixing and stirring evenly; (c) adding 10-15% of the total mass of alkali-swellable acrylic acid and stirring evenly to prepare a mother solution for standby use; (d) adding 3-4% of the total mass of a dispersant naphthol polyoxyethylene ether, pretreated carbon black and an amphiphilic carbon material to the reserved mother liquor, and stirring the mixture to obtain a feed liquid A; (e) dispersing the liquid A obtained in step (d) by ultrasonic oscillation for 40-50 minutes to obtain liquid B; (f) centrifuging the liquid B obtained in step (e) for 10 minutes to remove the precipitate to obtain liquid C; (g) adding 8-15% of anhydrous ethanol to the liquid C obtained in step (f), dispersing the mixture by ultrasonic oscillation for 10-15 minutes, and degassing the mixture under vacuum for 30 minutes to obtain carbon ink.
Citation Information
Patent Citations
Active carbon for preparing carbon electrode of super capacitor and preparation method thereof
CN101844765A
Nano carbon microsphere cathode material of lithium ion cell and its preparation method
CN102351163A
Quick-drying carbon ink and preparation method thereof
CN104610810A
Preparation method for petroleum-coke-based mesoporous carbon and application
CN106495125A
Process for preparing water ink
CN1334300A
Cited By
Water-soluble lithium battery negative electrode coating material capable of forming hard carbon characteristic and preparation method of water-soluble lithium battery negative electrode coating material
CN121097034A