Method for preparing spherical porous carbon by dry method, spherical porous carbon and lithium ion battery

Preparing spherical porous carbon by dry method solves the problems of complex preparation process and high cost in the existing technology, achieves high compaction density and environmentally friendly production, is suitable for large-scale production, and improves the stability of the negative electrode material.

CN118851171APending Publication Date: 2024-10-29SHENZHEN SOLID ADVANCED MATERIALS TECH CO LTD

Patent Information

Application Number
CN202411322341.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-23
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

The preparation process of spherical porous carbon in the prior art has problems such as complex reactions, harsh preparation conditions, long preparation process, high cost, and unfriendly environment. In addition, the irregular-shaped porous carbon causes uneven expansion stress of the negative electrode material when lithium is inserted and expands. Easy to break, low compaction density.

Method used

The method of preparing spherical porous carbon by dry method includes providing a heated and meltable carbon precursor for crushing and superficial solidification treatment, heating and carbonizing to activate pores, and purifying, pickling, washing until neutral, and drying. Disperse and classify to obtain spherical porous carbon with good particle size distribution.

Benefits of technology

It achieves no synthesis reaction, no use of organic solvents, no waste water or by-products, high product yield, suitable for large-scale production, and provides higher compaction density and more convenient preparation methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118851171A_ABST
    Figure CN118851171A_ABST
Patent Text Reader

Abstract

The invention relates to a method for preparing spherical porous carbon by a dry method, spherical porous carbon and a lithium ion battery. The dry method preparation specifically comprises the following steps: S1, providing a carbon precursor which can be melted by heating, and crushing the carbon precursor until D50 is 4-20 microns; s2, performing superficial layer curing treatment on the crushed carbon precursor; s3, carrying out heating carbonization on the carbon precursor after the superficial layer of the surface is cured, and curing to obtain spherical carbon after the final carbonization temperature of the carbon precursor at the center of a particle is reached; s4, carrying out activation and pore forming on the spherical carbon; s5, the spherical carbon obtained after pore forming is sequentially subjected to purification, acid pickling, water washing to be neutral, drying, scattering and grading, and the spherical porous carbon with good particle size distribution is obtained. According to the present invention, the preparation process does not require the synthesis reaction, does not use the organic solvent, does not produce the wastewater, does not produce the by-product, has the high product yield, and is suitable for the large-scale production, and the spherical porous carbon with the high compaction density is provided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of negative electrode materials for lithium ion batteries, and in particular to a method for preparing spherical porous carbon by a dry method, the spherical porous carbon and a lithium ion battery. Background Art

[0002] Porous silicon-carbon negative electrode materials use porous carbon as a carrier, and deposit silicon sources into the pores of porous carbon under a certain temperature and pressure to form silicon-carbon negative electrode materials. The pores of porous carbon are mainly micropores, and the deposited silicon is separated by the micropores of porous carbon. There are no large particles of silicon, and the expansion stress is small. At the same time, the porous structure of porous carbon provides space for the expansion of silicon. Therefore, porous silicon-carbon negative electrode materials have the advantages of good anti-expansion and long cycle performance, and are unanimously recognized as one of the most promising battery negative electrode materials in the future. Porous carbon is the core material of porous silicon-carbon negative electrode materials. The morphology, composition, and pore structure of porous carbon have a significant impact on the performance of porous silicon-carbon negative electrode materials.

[0003] At present, most porous carbons are irregular in shape. The silicon-carbon negative electrode materials prepared from irregular porous carbon have the following disadvantages: 1. The silicon-carbon negative electrode materials are in granular form. The irregular silicon-carbon negative electrode materials are subjected to uneven forces in all directions when they are expanded by lithium insertion, and the particles are easily broken, which affects the cycle performance; 2. When the irregular silicon-carbon negative electrode materials are rolled to prepare the pole pieces, they are more easily crushed due to the overlap between the particles and the shear force, resulting in reduced initial efficiency; 3. There are large gaps between the particles of the irregular silicon-carbon negative electrode materials, and the compaction density is low, which is not conducive to improving the energy density of the battery. That is, irregular porous carbon has the following problems: the particles are easy to crush, the compaction density is low, and the expansion stress in all directions during the negative electrode lithium insertion process is uneven, and it is easy to break.

[0004] Preparing porous carbon into spheres can solve the above three problems. The key to spherical porous carbon is the preparation of raw material spherical carbon. The preparation of spherical carbon in the prior art mostly synthesizes spherical carbon precursors in a reactor, or spheroidizes them in a liquid phase, and then separates, dries, and carbonizes the mother liquor and spherical carbon precursor. In addition to the spherical carbon precursor, the production process also has by-products, the reaction is complex, the preparation conditions are harsh, the preparation process is long, the cost is high, and it is not environmentally friendly.

[0005] Existing patent 1: Preparation method of spherical activated carbon (patent number: CN103641115A) discloses: Spherical porous carbon is prepared by suspension polymerization synthesis, and the raw materials used are: initiator 0.5~5, monomer 80~120, cross-linking agent 1~10, porogen 1~30, surfactant 0.5~5, water 250~500. The raw materials are put into the reactor and filled with inert gas, stirred, heated, cooled after reaction, filtered and washed with distilled water to obtain spherical resin. The preparation process requires polymerization reaction, filtration, and washing. The organic solvents involved in the process are flammable, explosive, and toxic, and organic wastewater is generated, which is not suitable for large-scale production or has high large-scale production costs.

[0006] Existing patent 2: A method for preparing mesophase carbon microspheres using asphalt thermal cracking oil (patent number: CN109179371A) discloses: by utilizing the nucleation center, the carbon precursor in the mother liquor undergoes a polymerization reaction, the molecular weight increases, and the carbon precursor grows into a sphere in the nucleation center in an in-situ growth manner. The preparation steps are: 1. Dissolve the asphalt thermal cracking oil with a first organic solvent and then distill to obtain a soluble component; 2. Heat treat the soluble component obtained in step 1 in a tubular closed container to obtain a thermal polymerization product; 3. Dissolve the thermal polymerization product obtained in step 2 with a second organic solvent and then filter to obtain a filter cake, then crush the filter cake, and then carbonize it after drying to obtain spherical carbon. The preparation process requires synthetic polymerization reaction, organic solvent dissolution, filtration, and drying, the process is complicated, and the organic solvent used is flammable and explosive. And after the solvent is dissolved, the soluble part is caused as a by-product, which greatly reduces the yield of spherical carbon.

[0007] Therefore, the existing technology needs to be improved. Summary of the invention

[0008] In the prior art, the preparation process of spherical porous carbon produces by-products in addition to the spherical carbon precursor, and there are problems such as complex reaction, harsh preparation conditions, long preparation process, high cost, and environmental unfriendliness. Therefore, the present invention provides a method for dry-process preparation of spherical porous carbon, spherical porous carbon and lithium-ion battery for solving the above problems.

[0009] To achieve the above object, in a first aspect, the present invention provides a method for preparing spherical porous carbon by dry process, which specifically comprises the following steps: S1, providing a heated fusible carbon precursor, and crushing it to a D50 of 4-20 μm; S2, performing superficial curing treatment on the crushed carbon precursor; S3, carbonizing the carbon precursor after the superficial layer of the surface is cured by heating, and curing the carbon precursor after reaching the final carbonization temperature of the carbon precursor in the center of the particle to obtain spherical carbon; S4, activating and pore-forming the spherical carbon; S5. The pore-forming spherical carbon is purified, acid-washed, washed with water until neutral, dried, and broken up and classified to obtain spherical porous carbon with good particle size distribution.

[0010] In one implementation, in S1, the carbon precursor is asphalt or resin, and the resin includes any one of phenolic resin, furan resin, epoxy resin, polyimide resin, asphalt-based resin and cellulose resin.

[0011] In one implementation, in S2, the superficial curing treatment of the epidermis includes a cross-linking curing method and / or a surface wrapping method, wherein the cross-linking curing method specifically includes using a reagent that can undergo cross-linking curing with the carbon precursor to perform shallow thin layer cross-linking curing, wherein the reagent includes any one of air, oxygen-deficient, nitric acid, hydrogen peroxide and urotropine; the surface wrapping method includes using non-melting fine particles for surface wrapping, wherein the non-melting fine particles are carbon black or carbon nanotubes.

[0012] In one implementation, in S2, the surface coating method specifically includes the following steps: the carbon precursor is a phenolic resin, the crushed phenolic resin and carbon black are mixed in a ratio of (8~15):1, and mixed in a mixer at a speed of 500r / min for 6 hours to evenly coat the carbon black fine powder on the surface of the phenolic resin particles, the mixed material is poured into a tray and placed in a blast oven, and the temperature is increased from room temperature to 90℃~250℃ at a rate of 2℃ / min~5℃ / min and kept at a constant temperature for 20min~60min to achieve shallow curing of the surface of the carbon precursor.

[0013] In one implementation, in S3, the carbonization temperature is 500°C to 700°C, and the carbonization time is 1 to 2.5 hours.

[0014] In one implementation, in S4, the activating agent used for the activation pore formation includes any one or a combination of two of water vapor, carbon dioxide, potassium hydroxide and sodium hydroxide.

[0015] In one implementation, in S4, using potassium hydroxide for activation and pore formation specifically includes: mixing the spherical carbon and KOH in a ratio of 1:1 to 1:4, putting them into a sagger, and performing alkali activation and pore formation in a box furnace, the activation temperature is 700 to 1000°C, and the activation time is 1h to 3h.

[0016] In one implementation, in S5, specifically includes: adding 20 times the weight of water of the spherical carbon for alkali washing, and then using 10% hydrochloric acid for pickling, and after pickling, using excess water to rinse the filter cake until the filtrate is neutral and then drying.

[0017] In a second aspect, the present invention further provides a spherical porous carbon, which is prepared by any one of the above-mentioned methods for preparing spherical porous carbon by dry method.

[0018] In a third aspect, the present invention further provides a lithium-ion battery, which uses the above-mentioned spherical porous carbon as a negative electrode material.

[0019] Beneficial effects: The present invention performs a superficial solidification treatment on the carbon precursor to keep the center of the particle fusible, and heats the carbon precursor after the superficial solidification to carbonize it, and obtains spherical porous carbon after activation and pore formation. The preparation process does not require synthetic reaction, does not use organic solvents, does not generate waste water, and has no by-products. The product yield is high and is suitable for large-scale production. At the same time, the cost of the preparation process is reduced, providing a more convenient preparation method; at the same time, a spherical porous carbon with a higher compaction density is provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 It is a flow chart of the steps of the method for preparing spherical porous carbon by dry method provided by the present invention; Figure 2 It is a schematic diagram of particle changes in the method for preparing spherical porous carbon by dry method provided by the present invention; Figure 3 is an electron microscope image of the spherical porous carbon obtained in Example 1; Figure 4 yes Figure 3 A detailed enlarged image of the spherical porous carbon is shown; Figure 5 It is an electron microscope comparison diagram of the crushing conditions of the spherical porous carbon provided in Example 1 and the comparative example.

[0021] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0022] In order to make the purpose, technical solutions and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with the accompanying drawings and examples. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the description of the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" described below means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms is not necessarily for the same embodiment or example. Moreover, the technical features involved in each embodiment of the present invention can be combined with each other as long as they do not conflict with each other.

[0023] Combined with reference Figure 1 and Figure 2, Figure 1 is a flow chart of the steps of the method for preparing spherical porous carbon by dry method provided by the present invention, Figure 2 It is a schematic diagram of particle changes in the method for preparing spherical porous carbon by dry method provided by the present invention.

[0024] The present invention provides a method for preparing spherical porous carbon by dry process, which specifically comprises the following steps: S1, providing a heated fusible carbon precursor, and crushing it to a D50 of 4-20 μm; S2, performing superficial curing treatment on the crushed carbon precursor; S3, carbonizing the carbon precursor after the superficial layer of the surface is cured by heating, and curing the carbon precursor after reaching the final carbonization temperature of the carbon precursor in the center of the particle to obtain spherical carbon; S4, activating and pore-forming the spherical carbon; S5. The pore-forming spherical carbon is purified, acid-washed, washed with water until neutral, dried, and broken up and classified to obtain spherical porous carbon with good particle size distribution.

[0025] Specifically, in S1, the carbon precursor is asphalt or resin. In S1, the resin includes any one of phenolic resin, furan resin, epoxy resin, polyimide resin, asphalt-based resin and cellulose resin. Among them, phenolic resin has good heat resistance and carbonization rate. Furan resin has a high carbon content and carbonization rate. Epoxy resin has good mechanical properties and processing properties, but the carbonization rate is relatively low. Polyimide resin has excellent heat resistance and mechanical properties. Asphalt-based resin is made by modifying petroleum or coal tar and has a high carbon content. Cellulose resin is derived from natural cellulose.

[0026] Specifically, in S2, the superficial curing treatment of the epidermis includes a cross-linking curing method and / or a surface wrapping method, wherein the cross-linking curing method specifically includes using a reagent that can undergo cross-linking curing with the carbon precursor to perform shallow thin layer cross-linking curing, wherein the reagent includes any one of air, oxygen-deficient, nitric acid, hydrogen peroxide and urotropine; the surface wrapping method includes using non-melting fine particles for surface wrapping, wherein the non-melting fine particles are carbon black or carbon nanotubes.

[0027] Furthermore, the surface coating method specifically includes the following steps: the carbon precursor is phenolic resin, the crushed phenolic resin and carbon black are mixed in a ratio of (8~15):1, and mixed in a VC mixer at a speed of 500r / min for 6 hours to evenly coat the carbon black fine powder on the surface of the phenolic resin particles, the mixed material is poured into a tray and placed in a blast oven, and the temperature is increased from room temperature to 90℃~250℃ at a rate of 2℃ / min~5℃ / min and kept at a constant temperature for 20min~60min to achieve superficial curing of the carbon precursor.

[0028] Specifically, in S3, the carbonization temperature is 500°C to 700°C, and the carbonization time is 1 to 2.5 hours. During the carbonization process, the surface of the particles that have undergone superficial curing treatment does not melt, and the heated fusible carbon precursor inside the particles melts into balls to obtain solidified spherical carbon.

[0029] Specifically, in S4, the activating agent used for the activation pore formation includes any one of water vapor, carbon dioxide, potassium hydroxide and sodium hydroxide. The activation pore formation using potassium hydroxide specifically includes: mixing the spherical carbon with KOH in a ratio of 1:1 to 1:4, putting it into a sagger, and performing alkali activation pore formation in a box furnace, the activation temperature is 700 to 1000°C, and the activation time is 1h to 3h.

[0030] Specifically, in S5, it specifically includes: adding 20 times the weight of water of the spherical carbon to wash the alkali, and then using 10% hydrochloric acid to acid wash, and then using excess water to rinse the filter cake until the filtrate is neutral and then drying. And breaking up and classifying to obtain spherical porous carbon with good particle size distribution.

[0031] Embodiment 1: S1. Grind the solid phenolic resin with a jet mill to D10=3.1 μm, D50=8.5 μm, and D90=15.3 μm, wherein the softening point of the phenolic resin is 110° C. and it is a thermosetting phenolic resin.

[0032] S2, the above-mentioned crushed phenolic resin and carbon black are mixed in a mass ratio of 9: 1, and then mixed in a VC mixer at a speed of 500r / min for 6 hours, so that the carbon black fine powder is evenly coated on the surface of the phenolic resin particles. The above-mentioned mixed materials are poured into a tray, placed in a blast oven, and heated from room temperature to 180°C at a rate of 5°C / min for 20 minutes to achieve the preparation of spherical resin. Because the softening point of phenolic resin is 110°C, it will melt and form balls when the temperature reaches about 110°C, and the carbon black wrapped on the surface of the phenolic resin particles blocks the fusion between the particles. Due to the use of thermosetting phenolic resin, the temperature continues to rise and the resin undergoes cross-linking and curing to form a spherical resin.

[0033] S3, carbonizing the spherical resin at a carbonization temperature of 700° C. for 1 hour to obtain spherical carbon.

[0034] S4. The spherical carbon and KOH are mixed in a ratio of 1:2, put into a sagger, and alkali activated to form pores in a box furnace. The activation conditions are: temperature 900° C., time 3 hours.

[0035] S5. After activation, add 20 times the weight of water of the spherical carbon to wash the alkali, and then use 10% hydrochloric acid to pickle. After pickling, use excess water to rinse the filter cake until the filtrate is neutral, then dry it, and then break it up and classify it to obtain spherical porous carbon.

[0036] The spherical porous carbon obtained in this example is as follows Figure 3 and Figure 4 As shown, Figure 3 is an electron microscope image of the spherical porous carbon obtained in Example 1, Figure 4 yes Figure 3 A detailed enlarged image of the spherical porous carbon is shown.

[0037] Embodiment 2: S1. Select high-temperature asphalt with a softening point of 280℃ and crush it to D10=3.4μm, D50=8.3μm, and D90=13μm.

[0038] S2. The surface of the crushed high-temperature asphalt is subjected to a non-melting treatment, and the non-melting condition is to heat the asphalt to 350°C at a heating rate of 2°C / min in a blast oven and keep the temperature constant for 1 hour.

[0039] S3. Carbonize the asphalt after the surface non-melting treatment at a carbonization temperature of 500° C. for 1 hour to obtain spherical carbon.

[0040] S4. The spherical carbon and KOH are mixed in a ratio of 1:2, put into a sagger, and alkali activated to form pores in a box furnace. The activation conditions are: temperature 900° C., time 3 hours.

[0041] S5. After activation, add 20 times the weight of water of the spherical carbon to wash the alkali, and then use 10% hydrochloric acid to pickle. After pickling, use excess water to rinse the filter cake until the filtrate is neutral, then dry it, and then break it up and classify it to obtain spherical porous carbon.

[0042] Embodiment 3: S1. Select high-temperature asphalt with a softening point of 200°C and crush it to D10=5.4μm, D50=10.3μm, and D90=15.2μm.

[0043] S2. Mix the crushed asphalt and carbon black in a mass ratio of 9:1, and then mix them in a VC mixer at a speed of 500r / min for 6 hours to evenly coat the surface of the asphalt particles with the carbon black fine powder. Put the mixed materials into a rotary kiln, introduce air into the rotary kiln, heat it to 250°C at a heating rate of 5°C / min, and keep it at this temperature for 1 hour.

[0044] S3. Switch the mixed gas to nitrogen, raise the temperature to 500°C for carbonization, and the carbonization time is 1 hour.

[0045] S4. The carbonized spherical carbon is mixed with KOH at a mass ratio of 1:2, put into a sagger, and alkali activated to form pores in a box furnace. The activation conditions are: temperature 900° C., time 3 hours.

[0046] S5. After activation, add 20 times the weight of water of the spherical carbon to wash the alkali, and then use 10% hydrochloric acid to pickle. After pickling, use excess water to rinse the filter cake until the filtrate is neutral, then dry it, and then break it up and classify it to obtain spherical porous carbon.

[0047] The porous carbon parameter data of the above embodiments and comparative examples are shown in Table 1.

[0048] Table 1, porous carbon parameter data table of Examples 1 to 3 and Comparative Examples: ;

[0049] It can be seen from Table 1 that compared with the comparative example, the spherical porous carbon provided by Examples 1 to 3 has a higher compaction density.

[0050] The spherical porous carbon provided in Example 1 was deposited with silane to prepare a porous silicon-carbon negative electrode material, which was mixed with graphite to prepare electrodes with different compaction densities. The crushing of the porous silicon-carbon particles was observed by SEM. Figure 5 As shown, Figure 5 The following is a comparison of the crushing conditions of the spherical porous carbon provided in Example 1 and the comparative example under electron microscope. Figure 5 It can be seen that the commercial porous carbon has broken at a compaction density of 1.6 g / cc, while the spherical porous carbon prepared in Example 1 has not broken when compacted to 1.9 cc, showing a high compaction density.

[0051] In summary, the present invention performs a superficial solidification treatment on the carbon precursor to keep the center of the particle fusible, and heats the carbon precursor after the superficial solidification of the skin to carbonize, and obtains spherical porous carbon after activation and pore formation. The preparation process does not require synthetic reaction, does not use organic solvents, does not generate waste water, and has no by-products. The product yield is high and is suitable for large-scale production. At the same time, the cost of the preparation process is reduced, providing a more convenient preparation method; at the same time, a spherical porous carbon with a higher compaction density is provided.

[0052] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made by using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A method for preparing spherical porous carbon by dry process, It is characterized in that The specific steps include: S1, providing a heated fusible carbon precursor, and crushing it to a D50 of 4-20 μm; S2, performing superficial curing treatment on the crushed carbon precursor; S3, carbonizing the carbon precursor after the superficial layer of the surface is cured by heating, and curing the carbon precursor after reaching the final carbonization temperature of the carbon precursor in the center of the particle to obtain spherical carbon; S4, activating and pore-forming the spherical carbon; S5. The pore-forming spherical carbon is purified, acid-washed, washed with water until neutral, dried, and broken up and classified to obtain spherical porous carbon with good particle size distribution.

2. The method for preparing spherical porous carbon by dry method according to claim 1, It is characterized in that In S1, the carbon precursor is pitch or resin, and the resin includes any one of phenolic resin, furan resin, epoxy resin, polyimide resin, pitch-based resin and cellulose resin.

3. The method for preparing spherical porous carbon by dry method according to claim 1, It is characterized in that In S2, the superficial curing treatment of the epidermis includes a cross-linking curing method and / or a surface wrapping method. The cross-linking curing method specifically includes using a reagent that can undergo cross-linking curing with the carbon precursor to perform shallow thin layer cross-linking curing, and the reagent includes any one of air, oxygen-deficient, nitric acid, hydrogen peroxide and urotropine; the surface wrapping method includes using non-melting fine particles for surface wrapping, and the non-melting fine particles are carbon black or carbon nanotubes.

4. The method for preparing spherical porous carbon by dry method according to claim 3, It is characterized in that In S2, the surface coating method specifically includes the following steps: the carbon precursor is phenolic resin, the crushed phenolic resin and carbon black are mixed in a ratio of (8~15):1, and mixed in a mixer at a speed of 500r / min for 6 hours to evenly coat the carbon black fine powder on the surface of the phenolic resin particles, the mixed material is poured into a tray and placed in a blast oven, and the temperature is increased from room temperature to 90℃~250℃ at a rate of 2℃ / min~5℃ / min and kept at a constant temperature for 20min~60min to achieve superficial curing of the carbon precursor.

5. The method for preparing spherical porous carbon by dry method according to claim 1, It is characterized in that In S3, the carbonization temperature is 500°C~700°C, and the carbonization time is 1~2.5h.

6. The method for preparing spherical porous carbon by dry method according to claim 1, It is characterized in that In S4, the activating agent used for the activation pore formation includes any one or a combination of two of water vapor, carbon dioxide, potassium hydroxide and sodium hydroxide.

7. The method for preparing spherical porous carbon by dry method according to claim 6, It is characterized in that In S4, the activation and pore formation using potassium hydroxide specifically includes: mixing the spherical carbon and KOH in a ratio of 1:1-1:4, putting them into a sagger, and performing alkali activation and pore formation in a box furnace, the activation temperature is 700-1000° C., and the activation time is 1h-3h.

8. The method for preparing spherical porous carbon by dry method according to claim 1, It is characterized in that In S5, specifically, it includes: adding water 20 times the weight of the spherical carbon to wash with alkali, and then using 10% hydrochloric acid to carry out acid washing. After the acid washing, the filter cake is washed with excess water until the filtrate is neutral and then dried.

9. A spherical porous carbon, It is characterized in that The spherical porous carbon is prepared by the dry method for preparing the spherical porous carbon according to any one of claims 1 to 8.

10. A lithium ion battery, It is characterized in that The spherical porous carbon described in claim 9 is used as the negative electrode material.

Citation Information

Patent Citations

  • Nitrogen / phosphorus double-doped spherical porous carbon, preparation method thereof and lithium ion battery

    CN118359195A

  • Manufacture of adsorbent

    JP1990122828A

Cited By

  • Method for increasing mesopores in lignin-based porous carbon for lithium battery silicon carbon

    CN120589749A

  • Method for improving mesoporous of porous carbon for lignin-based lithium battery silicon-carbon

    CN120589749B