Method for preparing mineral wool by using copper pyrogenic process to capture waste automobile exhaust catalyst slag
Using copper fire capture technology to prepare mineral wool from waste automobile exhaust catalyst slag, it solves the problems of low recovery rate of precious metal resources and unenvironmental waste treatment, achieves efficient recovery and high-value utilization, and produces minerals with excellent performance. Cotton products meet environmental protection requirements.
Patent Information
- Application Number
- CN202411220788.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-10-29
AI Technical Summary
In the existing technology, the recovery rate of precious metal resources is low and the waste treatment is not environmentally friendly. It is difficult to effectively utilize the precious metal resources in the waste automobile exhaust catalyst, and there are environmental pollution problems.
Using copper fire capture technology, waste automobile exhaust catalyst slag is pretreated, smelted, cooled, pulverized, magnetically separated, re-melted at high temperature and centrifugally blown to prepare mineral wool products with excellent performance and achieve efficient recovery of precious metals. and high-value utilization of waste.
It significantly improves the recovery rate of precious metals, reduces environmental pollution, and produces high-performance mineral wool products that meet the GB/T 11835-2016 standard. It has excellent thermal insulation, heat insulation and fire protection properties and meets green environmental protection requirements.
Smart Images

Figure CN118851560A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of copper pyrometallurgy capture slag value-added approach, and specifically relates to a method for preparing mineral wool by utilizing copper pyrometallurgy to capture waste automobile exhaust catalyst slag. Background Art
[0002] Precious metals are scarce resources worldwide, especially platinum group metal minerals, which are extremely scarce in my country. The copper pyrometallurgical capture technology of waste automobile exhaust catalyst slag recovers precious metals by high-temperature smelting of waste catalysts, and separates the slag from other components. This method has a short process flow, low wastewater volume, high recovery rate, and the leached slag can be harmlessly treated. Waste automobile exhaust catalysts contain a large amount of precious metals. After being captured by the copper pyrometallurgical capture method, the slag still contains a certain amount of metal components.
[0003] Mineral wool is a fiber material made from mineral raw materials melted at high temperature and then centrifugally blown, and has excellent thermal insulation, heat insulation and fireproof properties. The applicant of the present invention has found that the use of copper fire method to capture waste automobile exhaust catalyst slag meets the raw material requirements of mineral wool. If the slag can be used to prepare mineral wool, it can not only alleviate the shortage of precious metal resources, but also reduce the pollution of waste to the environment.
[0004] Therefore, the present invention develops an efficient and environmentally friendly treatment method based on the characteristics of copper pyrometallurgy to capture waste automobile exhaust catalyst slag, expands the value-added approach of copper pyrometallurgy to capture slag, and has important practical significance and application prospects. Summary of the invention
[0005] In view of the problems of low precious metal resource recovery rate and environmentally unfriendly waste treatment in the prior art, the present invention provides a method for preparing mineral wool by capturing waste automobile exhaust catalyst slag using copper pyrometallurgy. The method not only improves the recovery efficiency of precious metals, but also realizes high-value utilization of waste and produces mineral wool products with excellent performance. The advantages of the present invention are high efficiency and environmental protection, which meet the requirements of resource recycling and green environmental protection.
[0006] To achieve the above objectives, the present invention provides the following technical solutions.
[0007] A method for preparing mineral wool by capturing waste automobile exhaust catalyst slag using a copper pyrolysis method mainly comprises the following steps: Step 1, pretreatment of waste automobile exhaust catalyst: remove pollutants on the surface of waste automobile exhaust catalyst, and use a crusher to crush it into particles with a diameter of less than 3 mm suitable for smelting, and set the sieve hole diameter of the screening machine to 2 mm to screen out the raw materials used in the test.
[0008] Step 2, copper pyrometallurgical capture: the automobile exhaust catalyst pretreated in step 1 is sent into a 100kVA DC arc furnace, and precious metal components such as Pt, Pd, and Rh in the catalyst are captured by pyrometallurgical reduction smelting technology to generate slag.
[0009] Step 3, slag cooling and crushing: the slag produced by copper pyrometallurgy in step 2 is sent to a cooling tank, the cooled slag is crushed by a crusher to control the particle diameter to be less than 1 mm, and the metal impurities in the slag are further removed by magnetic separation technology; the screened slag is transferred to a magnetic separator equipped with a vibrating screening system and an automatic collection device for processing, and the magnetic field strength is 8000Gs.
[0010] Step 4, secondary high-temperature melting in the electric furnace: the slag, graphite powder, glass slag and copper slag treated in step 3 are mixed and sent into a 1000KVA electric furnace for secondary melting; during the melting process, oxygen is injected through the air intake system on the top of the furnace.
[0011] Step 5, centrifugal blowing fiberization treatment: In step 4, the molten slag is discharged from the electric furnace and flows into a high-speed rotating centrifuge, so that the slag is thrown out to form preliminary fibers; the thrown molten fibers are further stretched and refined by a high-pressure airflow through an air ejector; and mechanical stretching is performed under the action of a glass wool fiberizing machine.
[0012] Step 6, cooling and collecting mineral wool: the high-temperature mineral wool fibers after fiberization in step 5 are dropped from the outlet of the blowing device onto the cooling conveyor belt, and are rapidly cooled by the cooling fan and the spray device above the conveyor belt; the cooled mineral wool fibers are conveyed by the cooling conveyor belt to the automatic collection conveyor belt system; finally, the collected mineral wool fibers are compressed and packaged by the automatic packaging machine.
[0013] Furthermore, in step 1, a dust collector is provided, and the dust collection efficiency is ≥ 99%.
[0014] Furthermore, in step 2, the smelting temperature is between 1200° C. and 1400° C., and the smelting time is 2 to 4 hours.
[0015] Furthermore, in step 2, during the smelting process, the high-temperature furnace gas generated by the DC arc furnace passes through a heat exchanger to exchange heat with the cold air entering the arc furnace, so that the cold air is preheated to 400°C~500°C before entering the furnace; the cooling rate of the heat exchanger is 10°C / minute.
[0016] Furthermore, in step 3, the cooling trough has dimensions of 5 meters in length, 2 meters in width, and 1.5 meters in depth, is made of refractory bricks, and the cooling water flow rate is set to 240L / min~270L / min.
[0017] Furthermore, in step 4, the amount of graphite powder added is 2% to 8% of the mass of the slag, the amount of limestone added is 2% to 20% of the mass of the slag, and the amount of slag-forming agent copper slag added is 10% to 50% of the mass of the slag.
[0018] Furthermore, in step 4, the temperature of the electric arc furnace is 1200°C to 1400°C, the melting time is controlled to be 1.5 hours to 2 hours, and the flow rate of oxygen is 20m 3 / min~30m 3 / min.
[0019] Furthermore, in step 5, the centrifuge speed is 3000 r / min~5000 r / min; the air ejector pressure is 0.5 MPa~1.0 MPa; and the speed of the glass wool fiberizing machine is 20 m / s~40 m / s.
[0020] Furthermore, in step 6, the wind speed of the cooling fan is 15m / s~20m / s, and the cooling temperature is 20℃~30℃; the water flow rate of the spray device is 60L / min~70L / min, and the water temperature is 15℃~20℃.
[0021] Furthermore, in step 6, the collection speed of the automatic collection conveyor belt system is controlled between 5m / min and 7m / min, and the packaging pressure of the automatic packaging machine is 70KPa to 80KPa.
[0022] The mineral wool prepared through the above steps has excellent performance and meets the GB / T 11835-2016 standard, and is suitable for fields such as construction, industrial equipment and ships.
[0023] Compared with the prior art, the beneficial effects of the present invention are as follows.
[0024] 1. The present invention uses copper pyrometallurgy to efficiently capture precious metals in waste automobile exhaust catalysts, thus achieving efficient utilization of resources. Compared with the traditional wet treatment process, the copper pyrometallurgy process is shorter and produces less wastewater, ensuring efficient recovery of precious metals and complete separation of slag, significantly improving the recovery rate of precious metals, and reducing environmental pollution. The captured slag can be directly used for mineral wool preparation, while utilizing copper slag and glass slag in industrial production, reducing the waste treatment process and reducing treatment costs.
[0025] 2. The present invention adopts magnetic separation technology and high-temperature melting process in the slag treatment process to ensure the purity and liquefaction effect of the slag. By removing metal impurities and controlling the melting temperature, the slag can form a uniform fiber structure during the fiberization process. This method not only improves the quality of mineral wool, but also increases the strength and durability of mineral wool, and broadens its application range.
[0026] 3. The present invention utilizes a centrifugal blowing process to process high-temperature molten slag into mineral wool fibers, and the production process is efficient and environmentally friendly. By precisely controlling the rotation speed and air flow pressure of the centrifuge, the fineness and uniformity of the mineral wool fibers are optimized, and the final product has excellent thermal insulation, heat insulation and fireproof properties. Compared with the traditional mineral wool preparation method, the method of the present invention significantly improves product quality and production efficiency.
[0027] 4. The copper fire method is used to capture the slag of waste automobile exhaust catalyst to prepare mineral wool. By high-temperature melting and fiberization of the slag, it not only realizes the reuse of waste resources, but also produces high-value-added mineral wool products. This method improves resource utilization, reduces waste emissions, and meets the requirements of green environmental protection. Through experimental verification, the mineral wool prepared by this method has excellent performance and meets the GB / T 11835-2016 standard, and has broad application prospects.
[0028] The present invention provides an efficient and environmentally friendly treatment method, which not only solves the difficult problem of treating waste automobile exhaust catalysts, but also achieves efficient utilization of resources and environmental protection goals, and has important practical significance and application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 It is a flow chart of the present invention. DETAILED DESCRIPTION
[0030] In order to make those skilled in the art better understand the technical solution of the present invention, the present invention is further described below in conjunction with specific embodiments. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments. These embodiments should be understood to be only used to illustrate the present invention and not to limit the protection scope of the present invention. After reading the contents recorded in the present invention, all other embodiments obtained after various changes or modifications made to the present invention based on the technical solution and embodiments of the present invention also fall within the scope of protection of the claims of the present invention.
[0031] A method for preparing mineral wool by capturing waste automobile exhaust catalyst slag using a copper pyrolysis method mainly comprises the following steps: Step 1. Pretreatment of waste automobile exhaust catalysts: remove pollutants from the surface of waste automobile exhaust catalysts, and use a crusher to crush them into particles with a diameter of less than 3 mm suitable for smelting. The sieve hole diameter of the screening machine is set to 2 mm to screen out the raw materials used in the test, and a dust collector is equipped to collect dust and prevent pollution, and the dust collection efficiency is ≥99%.
[0032] Step 2, copper pyrometallurgical capture: the pretreated automobile exhaust catalyst is sent into a 100kVA DC arc furnace, the smelting temperature is between 1200℃~1400℃, the smelting time is 2~4 hours, and the precious metal components such as Pt, Pd, Rh in the catalyst are captured by pyrometallurgical reduction smelting technology to generate slag; during the smelting process, the high-temperature furnace gas generated by the DC arc furnace passes through a heat exchanger and exchanges heat with the cold air entering the arc furnace, so that the cold air is preheated to 400℃~500℃ and then enters the furnace, thereby reducing fuel consumption, improving energy utilization efficiency and reducing heat loss; the cooling rate of the heat exchanger is 10℃ / minute.
[0033] Step 3, slag cooling and crushing: The slag produced by copper pyrometallurgy is sent to a cooling tank of 5 meters long, 2 meters wide and 1.5 meters deep, made of refractory bricks to adapt to high temperature environments; the cooling water flow rate is set to 240L / min~270L / min to ensure that the slag is cooled to room temperature and evenly cooled through the cooling pipe; the cooled slag is crushed by a crusher to control the particle diameter below 1 mm; magnetic separation technology is used to further remove metal impurities in the slag to improve the purity of the raw materials; the screened slag is transferred to a magnetic separator equipped with a vibrating screening system and an automatic collection device for processing, and the magnetic field strength is 8000Gs. Ensure the stability of the operation and the final quality of the mineral wool.
[0034] Step 4, secondary high-temperature melting in the electric furnace: the slag, graphite powder, glass slag and copper slag treated in step 3 are mixed and sent to a 1200KVA electric furnace for secondary melting. The amount of graphite powder added is 2% to 8% of the slag mass, the amount of limestone added is 2% to 20% of the slag mass, and the amount of slag-forming agent copper slag added is 10% to 50% of the slag mass. During the melting process, oxygen is injected through the air intake system on the top of the furnace, and the flow rate is set to 20m 3 / min~30m 3 / min to promote chemical reactions in the slag and oxidative removal of residual metals; the temperature of the electric furnace is set to 1200℃~1400℃, and a high-efficiency resistance heating system and a precise temperature controller (±5℃) are used to ensure the uniformity and stability of the furnace temperature. The melting time is controlled at 1.5 hours~2 hours to fully dissolve residual impurities in the slag and improve the fluidity of the slag.
[0035] Step 5, centrifugal blowing fiberization treatment: In step 4, the molten slag is discharged from the electric furnace and flows into a high-speed rotating centrifuge (3000r / min~5000r / min), so that the slag is thrown out to form preliminary fibers. The thrown molten fibers are further stretched and refined by a high-pressure airflow (0.5 MPa~1.0 MPa) such as an air ejector to ensure the uniformity and stability of the fiber structure; under the action of a glass wool fiberizing machine (speed of 20m / s~40m / s), the fibers are made more uniform and slender through continuous mechanical stretching.
[0036] Step 6, mineral wool cooling and collection: The high-temperature mineral wool fibers after fiberization in step 5 are dropped from the outlet of the blowing device onto the cooling conveyor belt, and are rapidly cooled by the cooling fan (wind speed 15m / s~20m / s, cooling temperature 20℃~30℃) and the spray device (water flow 60L / min~70L / min, water temperature 15℃~20℃) above the conveyor belt. The cooled mineral wool fibers are transported by the cooling conveyor belt to the automatic collection conveyor belt system, and the collection speed is controlled at 5m / min~7m / min to ensure that the mineral wool fibers are not damaged or deformed during the collection process. Finally, the collected mineral wool fibers are compressed and packaged by an automatic packaging machine (packaging pressure 70KPa~80KPa) to ensure their volume and transportation convenience.
[0037] The mineral wool prepared through the above steps has excellent performance and meets the GB / T 11835-2016 standard, and is suitable for fields such as construction, industrial equipment and ships.
[0038] Example 1.
[0039] The waste catalyst raw material used in the test was from an automobile parts factory in Shenyang, with a PtO2 content of 0.05%, a PdO content of 0.02%, a Rh2O3 content of 0.01%, an Al2O3 content of 40.24%, a SiO2 content of 22.46%, a MgO content of 5.41%, a CaO content of 1.5%, a Fe2O3 content of 2.34%, a TiO2 content of 2.52%, a MnO content of 0.18%, a ZnO content of 0.05%, a CuO content of 0.63%, and a C content of 1.0%. The raw material was smelted at 1300°C in a 100kVA DC arc furnace by a copper pyrometallurgical capture method to obtain slag, in which the Al2O3 content was 18.56%, the SiO2 content was 37.23%, the MgO content was 22.60%, the CaO content was 19.04%, and the Fe2O3 content was 0.662%. The C content in graphite powder is 85%, the SiO2 content in glass slag is 68.46%, the Al2O3 content in the slag-making agent copper slag is 3.05%, the SiO2 content is 24.41%, the MgO content is 5.29%, the CaO content is 20.95%, and the Fe2O3 content is 26.23%.
[0040] The slag is sent to the cooling tank, and the cooling water flow rate is set to 250L / min to ensure that the slag is cooled from 1300℃ to room temperature. The cooled slag is crushed by a crusher, and the particle diameter is controlled below 1.5mm to remove large impurities. The slag is further screened in a magnetic separator with a magnetic field strength of 8000Gs. The screened slag, graphite powder (6% of the slag mass), glass slag (15% of the slag mass) and copper slag (30% of the slag mass) are fully mixed and sent to a 1200KVA submerged arc furnace for secondary melting. The temperature is set to 1350℃, the melting time is 2 hours, and the oxygen flow rate is 25m 3 / min, to ensure that the residual impurities in the slag are fully dissolved. The molten slag is discharged from the electric furnace and flows into a high-speed rotating centrifuge (speed 4500r / min), and is thrown out to form preliminary fibers. Under the combined action of high-pressure airflow (0.9 MPa) and glass wool fiber forming machine (speed 30m / s), the thrown molten fibers are made more uniform and slender through continuous mechanical stretching. The fiberized high-temperature mineral wool fibers fall from the outlet of the blowing device onto the cooling conveyor belt, and are rapidly cooled by the cooling fan (wind speed 18m / s, cooling temperature 22℃) and the spray device (60L / min, water temperature 16℃). The cooled mineral wool fibers are transported by the cooling conveyor belt to the automatic collection conveyor belt system, and the collection speed is controlled at 6m / min. Finally, the mineral wool fibers are compressed and packaged by an automatic packaging machine (packaging pressure 80KPa).
[0041] The final mineral wool product has a density of 86kg / m 3 , thermal conductivity 0.040W / (M0 K), organic matter content is 1.4%, heat load shrinkage temperature is 630℃, and slag ball content (particle size>0.25mm) is 5.8%.
[0042] Example 2.
[0043] The waste catalyst raw materials used in the test were from a waste metal recycling station in Wuhan, with PtO2 content of 0.06%, PdO content of 0.03%, Rh2O3 content of 0.01%, Al2O3 content of 38.24%, SiO2 content of 25.46%, MgO content of 4.41%, CaO content of 1.8%, Fe2O3 content of 2.84%, TiO2 content of 2.32%, MnO content of 0.28%, ZnO content of 0.08%, CuO content of 0.73%, and C content of 1.2%. The raw materials were smelted at 1350℃ in a 100kVA DC arc furnace by pyrometallurgical capture to obtain slag, in which the Al2O3 content of 19.76%, SiO2 content of 36.23%, MgO content of 21.60%, CaO content of 20.04%, and Fe2O3 content of 0.762%. The C content in graphite powder is 87%, the SiO2 content in glass slag is 67.46%, the Al2O3 content in the slag-making agent copper slag is 3.85%, the SiO2 content is 24.41%, the MgO content is 5.29%, the CaO content is 21.95%, and the Fe2O3 content is 25.23%.
[0044] The slag is sent to the cooling tank, and the cooling water flow rate is set to 260L / min to ensure that the slag is cooled from 1350℃ to room temperature. The cooled slag is crushed by a crusher, and the particle diameter is controlled below 1.3mm to remove large impurities. The slag is further screened in a magnetic separator with a magnetic field strength of 8500Gs. The screened slag, graphite powder (7% of the slag mass), glass slag (13% of the slag mass) and copper slag (35% of the slag mass) are mixed and sent to a 1200KVA submerged arc furnace for secondary melting. The temperature is set to 1300℃, the melting time is 1.8 hours, and the oxygen flow rate is 27m 3 / min, to ensure that the residual impurities in the slag are fully dissolved. The molten slag is discharged from the electric furnace and flows into a high-speed rotating centrifuge (speed 4600r / min), and is thrown out to form preliminary fibers. Under the combined action of high-pressure airflow (0.8 MPa) and glass wool fiber forming machine (speed 20m / s), the thrown molten fibers are made more uniform and slender through continuous mechanical stretching. The fiberized high-temperature mineral wool fibers fall from the outlet of the blowing device onto the cooling conveyor belt, and are rapidly cooled by the cooling fan (wind speed 17m / s, cooling temperature 24℃) and the spray device (65L / min, water temperature 17℃). The cooled mineral wool fibers are transported by the cooling conveyor belt to the automatic collection conveyor belt system, and the collection speed is controlled at 6.5m / min. Finally, the mineral wool fibers are compressed and packaged by an automatic packaging machine (packaging pressure 75KPa).
[0045] The final mineral wool product has a density of 85kg / m 3 , thermal conductivity 0.041W / (M 0 K), organic matter content is 1.3%, heat load shrinkage temperature is 640℃, and slag ball content (particle size>0.25mm) is 5.5%.
[0046] Example 3.
[0047] The waste catalyst raw material used in the test was from an automobile dismantling plant in Chongqing, with a PtO2 content of 0.05%, a PdO content of 0.03%, a Rh2O3 content of 0.01%, an Al2O3 content of 37.24%, a SiO2 content of 24.46%, a MgO content of 5.71%, a CaO content of 1.7%, a Fe2O3 content of 2.54%, a TiO2 content of 2.62%, a MnO content of 0.48%, a ZnO content of 0.06%, a CuO content of 0.83%, and a C content of 1.3%. The raw materials were smelted at 1340°C in a 100kVA DC arc furnace by pyrometallurgical capture to obtain slag, in which the Al2O3 content was 18.46%, the SiO2 content was 37.23%, the MgO content was 21.60%, the CaO content was 19.54%, and the Fe2O3 content was 0.762%. The C content in graphite powder is 86%, the SiO2 content in glass slag is 67.46%, the Al2O3 content in the slag-making agent copper slag is 3.45%, the SiO2 content is 24.41%, the MgO content is 5.09%, the CaO content is 21.85%, and the Fe2O3 content is 26.33%.
[0048] The slag is sent to the cooling tank, and the cooling water flow rate is set to 255L / min to ensure that the slag is cooled from 1200℃ to room temperature. The cooled slag is crushed by a crusher, and the particle diameter is controlled below 1.2mm to remove large impurities. The slag is further screened in a magnetic separator with a magnetic field strength of 8200Gs. The screened slag, graphite powder (6% of the slag mass), glass slag (12% of the slag mass) and copper slag (32% of the slag mass) are mixed and sent to a 1200KVA submerged arc furnace for secondary melting. The temperature is set to 1250℃, the melting time is 1.9 hours, and the oxygen flow rate is 22m 3 / min, to ensure that the residual impurities in the slag are fully dissolved. The molten slag is discharged from the electric furnace and flows into a high-speed rotating centrifuge (speed 4700r / min), and is thrown out to form preliminary fibers. Under the combined action of high-pressure airflow (0.9 MPa) and glass wool fiber forming machine (speed 40m / s), the thrown molten fibers are made more uniform and slender through continuous mechanical stretching. The fiberized high-temperature mineral wool fibers fall from the outlet of the blowing device onto the cooling conveyor belt, and are rapidly cooled by the cooling fan (wind speed 20m / s, cooling temperature 21℃) and the spray device (60L / min, water temperature 16℃). The cooled mineral wool fibers are transported by the cooling conveyor belt to the automatic collection conveyor belt system, and the collection speed is controlled at 6m / min. Finally, the mineral wool fibers are compressed and packaged by an automatic packaging machine (packaging pressure 75KPa).
[0049] The final mineral wool product has a density of 84kg / m 3 , thermal conductivity 0.038W / (M 0 K), organic matter content is 1.2%, heat load shrinkage temperature is 635℃, and slag ball content (particle size>0.25mm) is 5.6%.
[0050] Comparative example 1.
[0051] The waste catalyst raw materials used in the test were from a waste metal recycling station in Wuhan, with PtO2 content of 0.06%, PdO content of 0.03%, Rh2O3 content of 0.01%, Al2O3 content of 38.24%, SiO2 content of 25.46%, MgO content of 4.41%, CaO content of 1.8%, Fe2O3 content of 2.84%, TiO2 content of 2.32%, MnO content of 0.28%, ZnO content of 0.08%, CuO content of 0.73%, and C content of 1.2%. The raw materials were smelted at 1350℃ in a 100kVA DC arc furnace by pyrometallurgical capture to obtain slag, in which the Al2O3 content of 19.76%, SiO2 content of 36.23%, MgO content of 21.60%, CaO content of 20.04%, and Fe2O3 content of 0.762%. The C content in graphite powder is 87%, the SiO2 content in glass slag is 67.46%, the Al2O3 content in slag-making agent steel slag is 10.89%, the SiO2 content is 36.06%, the MgO content is 5.22%, the CaO content is 45.77%, and the Fe2O3 content is 0.96%.
[0052] The slag is sent to the cooling tank, and the cooling water flow rate is set to 260L / min to ensure that the slag is cooled from 1350℃ to room temperature. The cooled slag is crushed by a crusher, and the particle diameter is controlled below 1.3mm to remove large impurities. The slag is further screened in a magnetic separator with a magnetic field strength of 8500Gs. The screened slag, graphite powder (7% of the slag mass), glass slag (13% of the slag mass) and steel slag (35% of the slag mass) are mixed and sent to a 1200KVA submerged arc furnace for secondary melting. The temperature is set to 1150℃, the melting time is 1.8 hours, and the oxygen flow rate is 27m 3 / min, to ensure that the residual impurities in the slag are fully dissolved. The molten slag is discharged from the electric furnace and flows into a high-speed rotating centrifuge (speed 4600r / min), and is thrown out to form preliminary fibers. Under the combined action of high-pressure airflow (0.8 MPa) and glass wool fiber forming machine (speed 20m / s), the thrown molten fibers are made more uniform and slender through continuous mechanical stretching. The fiberized high-temperature mineral wool fibers fall from the outlet of the blowing device onto the cooling conveyor belt, and are rapidly cooled by the cooling fan (wind speed 17m / s, cooling temperature 24℃) and the spray device (65L / min, water temperature 17℃). The cooled mineral wool fibers are transported by the cooling conveyor belt to the automatic collection conveyor belt system, and the collection speed is controlled at 6.5m / min. Finally, the mineral wool fibers are compressed and packaged by an automatic packaging machine (packaging pressure 75KPa).
[0053] The final mineral wool product has a density of 90kg / m 3 , thermal conductivity 0.050W / (M0 K), organic matter content 1.8%, heat load shrinkage temperature 590 ° C, slag ball content (particle size > 0.25mm) is 6.5%. The effect of cotton mineral product is obviously not as good as that of Example 2.
[0054] Comparative example 2.
[0055] The waste catalyst raw material used in the test was from an automobile dismantling plant in Chongqing, with a PtO2 content of 0.05%, a PdO content of 0.03%, a Rh2O3 content of 0.01%, an Al2O3 content of 37.24%, a SiO2 content of 24.46%, a MgO content of 5.71%, a CaO content of 1.7%, a Fe2O3 content of 2.54%, a TiO2 content of 2.62%, a MnO content of 0.48%, a ZnO content of 0.06%, a CuO content of 0.83%, and a C content of 1.3%. The raw materials were smelted at 1340°C in a 100kVA DC arc furnace by pyrometallurgical capture to obtain slag, in which the Al2O3 content was 18.46%, the SiO2 content was 37.23%, the MgO content was 21.60%, the CaO content was 19.54%, and the Fe2O3 content was 0.762%. The C content in graphite powder is 86%, the SiO2 content in glass slag is 67.46%, the Al2O3 content in the slag-making agent copper slag is 3.45%, the SiO2 content is 24.41%, the MgO content is 5.09%, the CaO content is 21.85%, and the Fe2O3 content is 26.33%.
[0056] The slag is sent to the cooling tank, and the cooling water flow rate is set to 255L / min to ensure that the slag is cooled from 1200℃ to room temperature. The cooled slag is crushed by a crusher, and the particle diameter is controlled below 1.2mm to remove large impurities. The crushed slag, graphite powder (6% of the slag mass), glass slag (12% of the slag mass) and copper slag (32% of the slag mass) are mixed and sent to a 1200KVA submerged arc furnace for secondary melting. The temperature is set to 1250℃, the melting time is 1.9 hours, and the oxygen flow rate is 22m 3 / min, to ensure that the residual impurities in the slag are fully dissolved. The molten slag is discharged from the electric furnace and flows into a high-speed rotating centrifuge (speed 4700r / min), and is thrown out to form preliminary fibers. Under the combined action of high-pressure airflow (0.9 MPa) and glass wool fiber forming machine (speed 40m / s), the thrown molten fibers are made more uniform and slender through continuous mechanical stretching. The fiberized high-temperature mineral wool fibers fall from the outlet of the blowing device onto the cooling conveyor belt, and are rapidly cooled by the cooling fan (wind speed 20m / s, cooling temperature 21℃) and the spray device (60L / min, water temperature 16℃). The cooled mineral wool fibers are transported by the cooling conveyor belt to the automatic collection conveyor belt system, and the collection speed is controlled at 6m / min. Finally, the mineral wool fibers are compressed and packaged by an automatic packaging machine (packaging pressure 75KPa).
[0057] The final mineral wool product has a density of 92kg / m 3 , thermal conductivity 0.052W / (M 0 K), organic matter content 1.9%, heat load shrinkage temperature 600 ° C, slag ball content (particle size > 0.25mm) is 8.8%. The effect of cotton mineral product is obviously not as good as that of Example 3.
[0058] Comparative example 3.
[0059] The waste catalyst raw material used in the test was from an automobile parts factory in Shenyang, with a PtO2 content of 0.05%, a PdO content of 0.02%, a Rh2O3 content of 0.01%, an Al2O3 content of 40.24%, a SiO2 content of 22.46%, a MgO content of 5.41%, a CaO content of 1.5%, a Fe2O3 content of 2.34%, a TiO2 content of 2.52%, a MnO content of 0.18%, a ZnO content of 0.05%, a CuO content of 0.63%, and a C content of 1.0%. The raw material was smelted at 1300°C in a 100kVA DC arc furnace by a copper pyrometallurgical capture method to obtain slag, in which the Al2O3 content was 18.56%, the SiO2 content was 37.23%, the MgO content was 22.60%, the CaO content was 19.04%, and the Fe2O3 content was 0.662%. The C content in graphite powder is 85%, the SiO2 content in glass slag is 68.46%, the Al2O3 content in the slag-making agent copper slag is 3.05%, the SiO2 content is 24.41%, the MgO content is 5.29%, the CaO content is 20.95%, and the Fe2O3 content is 26.23%.
[0060] The slag is sent to the cooling tank, and the cooling water flow rate is set to 250L / min to ensure that the slag is cooled from 1300℃ to room temperature. The cooled slag is crushed by a crusher, and the particle diameter is controlled below 1.5mm to remove large impurities. The slag is further screened in a magnetic separator with a magnetic field strength of 8000Gs. The screened slag, graphite powder (6% of the slag mass), glass slag (15% of the slag mass) and copper slag (30% of the slag mass) are fully mixed and sent to a 1200KVA submerged arc furnace for secondary melting. The temperature is set to 1350℃, the melting time is 2 hours, and the oxygen flow rate is 25m 3 / min, to ensure that the residual impurities in the slag are fully dissolved. The molten slag is discharged from the electric furnace and flows into a high-speed rotating centrifuge (speed 4500r / min), where it is thrown out to form preliminary fibers. The thrown molten fibers are further stretched and refined by a glass wool fiberizer (speed 30m / s). The fiberized high-temperature mineral wool fibers are naturally cooled and transported to the automatic collection conveyor belt system, and the collection speed is controlled at 6m / min. Finally, the mineral wool fibers are compressed and packaged by an automatic packaging machine (packaging pressure 80KPa).
[0061] The final mineral wool product has a density of 90kg / m 3 , thermal conductivity 0.044W / (M 0 K), organic matter content 2.1%, heat load shrinkage temperature 600 ° C, slag ball content (particle size > 0.25mm) is 9.8%. The effect of cotton mineral product is obviously not as good as that of Example 1.
[0062] The present invention has disclosed and described the embodiments of the present invention in detail, but it should be emphasized that relational terms such as "first" and "second" are only used to distinguish entities or operations, and do not necessarily imply an actual relationship or order between them. In addition, the terms "include", "comprises" and their variations are intended to cover non-exclusive inclusion, so that a process, method, article or device involving a series of elements includes not only the listed elements, but also other elements not explicitly listed, as well as elements inherent to the process, method, article or device.
Claims
1. A method for preparing mineral wool by capturing waste automobile exhaust catalyst slag using copper pyrolysis, characterized in that: The following steps are involved: Step 1, pretreatment of waste automobile exhaust catalyst: remove pollutants on the surface of waste automobile exhaust catalyst, and use a crusher to crush it into particles with a diameter of less than 3 mm suitable for smelting, and set the sieve hole diameter of the screening machine to 2 mm to screen out the raw materials used in the test; Step 2, copper pyrometallurgical capture: the automobile exhaust catalyst pretreated in step 1 is sent into a 100kVA DC arc furnace, and precious metal components such as Pt, Pd, and Rh in the catalyst are captured by pyrometallurgical reduction smelting technology to generate slag; Step 3, cooling and crushing the slag: the slag produced by the copper pyrometallurgy in step 2 is sent to a cooling tank, the cooled slag is crushed by a crusher to control the particle diameter to be less than 1 mm, and the metal impurities in the slag are further removed by magnetic separation technology; the screened slag is transferred to a magnetic separator equipped with a vibrating screening system and an automatic collection device for processing, and the magnetic field strength is 8000Gs; Step 4, secondary high-temperature melting in a mineral heat furnace: the slag, graphite powder, glass slag and copper slag treated in step 3 are mixed and sent into a 1000KVA mineral heat furnace for secondary melting; during the melting process, oxygen is injected through the air intake system on the top of the furnace; Step 5, centrifugal blowing fiberization treatment: the molten slag in step 4 is discharged from the ore-fired electric furnace and flows into a high-speed rotating centrifuge to throw out the slag to form preliminary fibers; the thrown molten fibers are further stretched and refined by a high-pressure airflow through an air ejector; and mechanically stretched under the action of a glass wool fiberizer; Step 6, cooling and collecting mineral wool: the high-temperature mineral wool fibers after fiberization in step 5 are dropped from the outlet of the blowing device onto the cooling conveyor belt, and are rapidly cooled by the cooling fan and the spray device above the conveyor belt; the cooled mineral wool fibers are conveyed by the cooling conveyor belt to the automatic collection conveyor belt system; finally, the collected mineral wool fibers are compressed and packaged by the automatic packaging machine.
2. The method for preparing mineral wool by capturing waste automobile exhaust catalyst slag by copper pyrometallurgy according to claim 1, characterized in that: In the step 1, a dust collector is provided, and the dust collection efficiency is ≥ 99%.
3. The method for preparing mineral wool by capturing waste automobile exhaust catalyst slag by copper pyrometallurgy according to claim 1, characterized in that: In step 2, the smelting temperature is between 1200° C. and 1400° C., and the smelting time is 2 to 4 hours.
4. The method for preparing mineral wool by capturing waste automobile exhaust catalyst slag by copper pyrometallurgy according to claim 1, characterized in that: In step 2, during the smelting process, the high-temperature furnace gas generated by the DC electric arc furnace passes through a heat exchanger to exchange heat with the cold air entering the electric arc furnace, so that the cold air is preheated to 400° C. to 500° C. before entering the furnace; The heat exchanger cooling rate was 10°C / min.
5. The method for preparing mineral wool by capturing waste automobile exhaust catalyst slag by copper pyrometallurgy according to claim 1, characterized in that: In step 3, the cooling trough has dimensions of 5 meters in length, 2 meters in width, and 1.5 meters in depth, is made of refractory bricks, and the cooling water flow rate is set to 240L / min~270L / min.
6. The method for preparing mineral wool by capturing waste automobile exhaust catalyst slag by copper pyrometallurgy according to claim 1, characterized in that: In step 4, the amount of graphite powder added is 2% to 8% of the mass of the slag, the amount of limestone added is 2% to 20% of the mass of the slag, and the amount of slag-forming agent copper slag added is 10% to 50% of the mass of the slag.
7. The method for preparing mineral wool by capturing waste automobile exhaust catalyst slag by copper pyrometallurgy according to claim 1, characterized in that: In step 4, the temperature of the electric furnace is 1200°C to 1400°C, the melting time is controlled to be 1.5 hours to 2 hours; the flow rate of oxygen is 20m 3 / min~30m 3 / min.
8. The method for preparing mineral wool by capturing waste automobile exhaust catalyst slag by copper pyrometallurgy according to claim 1, characterized in that: In step 5, the centrifuge speed is 3000 r / min~5000 r / min; the air ejector pressure is 0.5 MPa~1.0 MPa; and the speed of the glass wool fiberizing machine is 20 m / s~40 m / s.
9. The method for preparing mineral wool by capturing waste automobile exhaust catalyst slag by copper pyrometallurgy according to claim 1, characterized in that: In step 6, the wind speed of the cooling fan is 15m / s~20m / s, and the cooling temperature is 20℃~30℃; the water flow rate of the spray device is 60L / min~70L / min, and the water temperature is 15℃~20℃.
10. The method for preparing mineral wool by capturing waste automobile exhaust catalyst slag by copper pyrometallurgy according to claim 1, characterized in that: In step 6, the collection speed of the automatic collection conveyor belt system is controlled between 5m / min and 7m / min, and the packaging pressure of the automatic packaging machine is 70KPa to 80KPa.