Glass powder for copper conductive paste as well as preparation method and application of glass powder

By optimizing the composition and proportion of glass powder, the wettability and bonding force of glass in multilayer ceramic capacitors are improved, the problems of insufficient bonding force and acid resistance in the existing technology are solved, and lower dielectric loss and better High durability, suitable for high performance requirements of multilayer ceramic capacitors.

CN118851579APending Publication Date: 2024-10-29NANCHONG THREE CIRCLE ELECTRONICS +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410842578.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

The glass powder used for copper conductive paste in existing multilayer ceramic capacitors has insufficient bonding strength and acid resistance, and there are few studies on dielectric properties and application range, making it unable to meet increasingly higher performance requirements.

Method used

Using glass powder composed of SiO2, Al2O3, BaO, B2O3, alkali metal oxides and alkaline earth metal oxides, the wettability of the glass can be improved by adjusting the proportion and adding appropriate amounts of Al2O3, CuO, TiO2, MnO2, V2O5 and other ingredients. , bonding strength and acid resistance, and reduce dielectric loss.

Benefits of technology

It achieves a good connection between glass, copper powder and matrix, reduces dielectric loss, improves the durability and reliability of multilayer ceramic capacitors, and is suitable for medium-high voltage, medium-high capacity multilayer ceramic capacitors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118851579A_ABST
    Figure CN118851579A_ABST
Patent Text Reader

Abstract

The invention discloses glass powder for copper conductive paste and a preparation method and application thereof, and relates to the technical field of multilayer ceramic capacitors. The glass powder is prepared from the following components in parts by weight in terms of oxide: 3 to 45 parts of SiO2, 3 to 12 parts of Al2O3, 3 to 50 parts of BaO, 12 to 25 parts of B2O3, 1 to 11 parts of alkali metal oxide and 2.5 to 10 parts of alkaline earth metal oxide, the alkali metal oxide is a compound of alkali metal oxide A and Li2O, and the alkali metal oxide A is at least one of Na2O and K2O; the alkaline earth metal oxide is a compound of MgO, CaO and SrO. After the copper conductive paste prepared from the glass powder is sintered, the dielectric loss is effectively reduced, and the dielectric property of a multilayer ceramic capacitor is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of multilayer ceramic capacitors, in particular to glass powder for copper conductive paste and a preparation method and application thereof. Background Art

[0002] The copper conductive paste for the terminal electrode of multilayer ceramic capacitor (MLCC) is generally composed of a functional phase, a bonding phase and an organic carrier. Among them, the functional phase is conductive copper powder, the organic carrier is composed of some organic solvents and polymers, and the bonding phase is mainly glass powder. In a few cases, a certain amount of oxide is added, which determines the bonding ability of copper powder, glass powder, ceramic matrix, etc. in the copper terminal electrode.

[0003] At present, the glass powders commonly used in the copper conductive paste of the terminal electrodes of multilayer ceramic capacitors mainly include PbO-B2O3-SiO2 lead glass, Bi2O3-B2O3-SiO2 bismuth glass, CaO-B2O3-SiO2-BaO borate glass, ZnO-B2O3-SiO2 glass, etc. PbO-B2O3-SiO2 lead glass has high resistance, low dielectric loss, low softening temperature, and good chemical stability, but Pb is highly toxic. Bi2O3-B2O3-SiO2 bismuth glass has low softening temperature and good chemical stability, but the cost is high, bismuth is easy to precipitate, and the acid resistance is poor. Poor acid resistance will lead to nickel plating, and nickel plating affects the durability of multilayer ceramic capacitor products. CaO-B2O3-SiO2-BaO borate glass can only achieve low melting point by adding alkali metal, alkaline earth metal or heavy metal ions, thereby reducing the melting temperature and homogenizing the glass components. However, this type of glass has unstable chemical properties, large thermal expansion coefficient and easy phase separation. ZnO-B2O3-SiO2 glass is mainly composed of ZnO, and excessive Zn content will cause the glass to easily crystallize and form zinc oxide, which is easily reduced to zinc when sintered in N2 atmosphere. The melting point of zinc is about 420℃, which can easily lead to the loss of multilayer ceramic capacitor products and deterioration of insulation resistance performance.

[0004] To improve the bonding strength and acid resistance of glass, the composition of glass powder for copper conductive paste has been improved in this field. By adding a specific amount of TiO2 and CaO, CN 108137388 A can prepare a dense electrode film with extremely high acid resistance. CN 110582813 A adds 9wt% < X < 50wt% lead-free glass powder, which is B-Si-Zn system glass or Zn-V system glass. It can also be sintered densely at 750 °C, has sufficient bonding strength, and excellent electrical conductivity. CN110423013 A reduces the sintering temperature of copper conductive paste by adding V2O5; V can increase the insulation resistance and reliability of the BaTiO3 ceramic matrix, and at the same time does not damage the BaTiO3 structure, and a beneficial reaction is carried out, thereby further improving the adhesion. CN100583326C provides an ideal glass composition by adding a mixture composed of components such as SiO2, ZnO, B2O3, Co3O4, etc. The presence of ZnO promotes the adhesion of the end electrode ink to the BaTiO3 substrate, and the ratio of B2O3 to SiO2 is considered to play an important role in copper densification. However, in the above studies, the main component glass system with V2O5 added, although the bonding strength of the matrix is improved, the stability of the V2O5-based glass is poor and the acid resistance is not good; after adding ZnO as the main component to the glass powder, the crystallization ability of the glass will increase, affecting the uniformity of the glass, and at the same time reducing the acid resistance of the glass. At the same time, the above studies only focus on aspects such as the bonding strength and acid resistance of glass, and there is less research on dielectric properties and application scope. To meet the increasingly high performance requirements of copper conductive paste, it is necessary to develop glass powder with more comprehensive properties. Summary of the Invention

[0005] The purpose of the present invention is to overcome the deficiencies of the prior art and provide a glass powder for copper conductive paste, its preparation method and application.

[0006] To achieve the above purpose, the technical solutions adopted by the present invention are as follows:

[0007] A glass powder for copper conductive paste, the glass powder contains the following components in parts by weight based on oxides: 3-45 parts of SiO2, 3-12 parts of Al2O3, 3-50 parts of BaO, 12-25 parts of B2O3, 1-11 parts of alkali metal oxide, 2.5-10 parts of alkaline earth metal oxide; the alkali metal oxide is a compound of alkali metal oxide A and Li2O, and the alkali metal oxide A is at least one of Na2O and K2O; the alkaline earth metal oxide is a compound of MgO, CaO, and SrO.

[0008] The present invention adds Ba 2+ , Ba 2+As a typical network exosome ion, it can reduce the viscosity of glass, thereby improving the wettability with metal powder. The better the wettability, the smaller the wetting angle, the denser the seal, and can prevent the subsequent electroplating solution from contacting the porcelain body of the multilayer ceramic capacitor through the end pores and causing the porcelain body to fail. At the same time, the good wettability of the glass allows the glass to have a certain corrosive effect on the porcelain body, allowing the inner electrode to be better exposed and form a sufficient electrical connection with the outer electrode, thereby reducing the dielectric loss of the product. At the same time, the reaction transition layer formed between the glass and the porcelain body can form a good transition and mechanical connection between the outer electrode and the porcelain body, thereby improving the bonding force between the end and the porcelain body and improving the reliability of the product. The glass powder of the present invention contains 3-50 parts of BaO. When the BaO content is too low, the wettability with metal powder is poor and the sealing performance is poor. When it is too high, it will hinder the formation of glass. Sr 2+ , Ca 2+ Mg 2+ Alkaline earth metal elements are all network exosome ions. The refractive index, molar volume, thermal expansion coefficient and resistivity of glass increase with the increase of ion radius, while dielectric loss, hardness and high temperature viscosity decrease with the increase of ion radius. Therefore, by adjusting the ratio of the above three elements, a thermal expansion coefficient consistent with the matrix can be obtained, the viscosity in the high temperature zone and the low temperature zone can be reduced, thereby reducing the stress of the bonding layer between glass and matrix and improving the durability of multilayer ceramic capacitors. Si is a network former and is the basic structural unit of glass. Si-O forms a three-dimensional space network with high rigidity and is not easy to expand. The [SiO4] structure determines the viscosity of fused quartz glass, high mechanical strength, small thermal expansion coefficient, heat resistance, good dielectric properties and chemical stability. Therefore, in the glass powder of the present invention, the preferred weight of SiO2 is 3-45 parts. When the weight of SiO2 is too low, the mechanical strength, heat resistance, dielectric properties and chemical stability of the glass are poor. When it is too high, the viscosity of the glass is too high, which will lead to poor wettability with copper powder and too high sintering temperature.

[0009] BO forms a [BO3] layered or chain structure. When there is too much free oxygen in the glass, [BO3] is converted into [BO4], so that the layered structure of boron is converted into a frame structure, creating conditions for B2O3 and SiO2 to form a uniform glass. Therefore, in the glass powder of the present invention, the weight of B2O3 is preferably 12-25 parts. When the content of B2O3 is too low, it is difficult to form glass. When it is too high, due to the increase of boron oxygen triangles, the expansion coefficient (CTE) of the glass increases, resulting in the failure of the thermal expansion coefficient between the terminal electrode and the porcelain body, which deteriorates the thermal shock resistance, long-term reliability, aging life, etc. of the product.

[0010] At the same time, the present invention also adds an appropriate amount of Al2O3 to adjust the symmetric relationship of [SiO4], [BO4], and [BO3], adjust the thermal expansion coefficient of the glass, adapt to the ceramic body of the multilayer ceramic capacitor with different thermal expansion coefficients, and solve the failure problem between the terminal electrode and the ceramic body. Preferably, the weight of Al2O3 in the glass powder is 3-12 parts. As an intermediate oxide in the glass, Al2O3 can reduce the crystallization tendency of the glass, enhance the glass structure, and improve the stability and mechanical strength of the glass. When the Al2O3 content is higher than 12 parts, it will increase the viscosity of the glass, increase the softening point of the glass, and reduce the wettability of the glass and the substrate. When it is less than 3 parts, the chemical stability of the glass is poor.

[0011] Among the alkali metal oxides, Na2O and K2O play a role in breaking the network, and Li2O plays a role in agglomeration. The compounding of alkali metal oxide A and Li2O can produce a mixed alkali effect, thereby improving the ion diffusion, chemical stability and electrical properties of the glass.

[0012] Preferably, the mass ratio of alkali metal oxide A to Li2O in the alkali metal oxide is (0.1-5):1.

[0013] When the ratio of each component in the alkali metal oxide meets the above limitations, the dielectric loss is lower and the chemical stability is better; when the ratio of each component in the alkaline earth metal oxide meets the above limitations, the thermal expansion coefficient of the glass can be synergistically adjusted, the viscosity in the high temperature zone and the low temperature zone can be further reduced, the stress of the bonding layer between the glass and the substrate can be reduced, and the durability of the multilayer ceramic capacitor can be further improved.

[0014] Preferably, the mass ratio of MgO, CaO and SrO in the alkaline earth metal oxide is (0.1-5):(0.1-5):1.

[0015] When the proportions of the components in the alkaline earth metal oxide meet the above limitations, the dielectric loss is lower and the chemical stability is better.

[0016] Preferably, the mass ratio of BaO to alkaline earth metal oxide is (5-10):1.

[0017] The present invention has found through experiments that when the mass ratio of BaO to alkaline earth metal oxide meets the above-mentioned limitation, good glass wettability, appropriate linear expansion coefficient, and high copper end density can be guaranteed, while the crystallization tendency can be reduced, and good bonding strength between the copper end and the porcelain body and resistance to corrosion by electroplating solution can be guaranteed, thereby improving the reliability of the product.

[0018] Preferably, the glass powder further comprises at least one of CuO, Cu2O, TiO2, MnO2, V2O5, and ZnO.

[0019] Preferably, the glass powder for copper conductive paste has at least one of the following characteristics (a)-(e):

[0020] (a) the weight portion of CuO in the glass powder is 0-8 parts, and the weight portion of Cu2O is 0-8 parts;

[0021] CuO or Cu2O is added to the glass powder and applied to the copper conductive paste. When sintered in a reducing atmosphere, CuO or Cu2O is converted into Cu particles, which are evenly distributed on the surface of the gushing glass, playing the same cathode role as the Cu powder in the copper conductive paste, so that the Ni plating layer in the subsequent multilayer ceramic capacitor is evenly diffused to form a plating film, improving the problem of poor electroplating. When the weight of CuO or Cu2O is too high, the glass is easy to separate into phases, reducing chemical stability;

[0022] (b) The weight portion of TiO2 in the glass powder is 0-5 parts. Adding TiO2 to the glass powder helps to improve the acid resistance of the glass. When the weight portion of TiO2 is higher than 5 parts, the glass will be easily crystallized and the softening point will rise sharply.

[0023] (c) the weight portion of MnO2 in the glass powder is 0-10 parts, and the addition of MnO2 in the glass powder helps the formation of glass. When the weight portion of MnO2 is higher than 10 parts, the viscosity behavior of the glass at high temperature becomes unstable;

[0024] (d) The weight portion of V2O5 in the glass powder is 0-20 parts. Adding a small amount of V2O5 to the glass powder can reduce the sintering temperature and improve the bonding strength with the substrate. When the weight portion of V2O5 is too high, the stability of the glass is poor and the acid resistance is poor;

[0025] (e) Preferably, the weight proportion of ZnO in the glass powder is 0-30 parts. Adding a small amount of ZnO to the glass powder can enhance the bonding strength between the glass and the substrate. When the weight proportion of ZnO is higher than 30 parts, the glass is prone to crystallization, the uniformity of the glass deteriorates, and the acid resistance of the glass also deteriorates.

[0026] The present invention also provides a method for preparing the above-mentioned glass powder for copper conductive paste, comprising the following steps:

[0027] (1) Weighing each component in proportion, mixing them evenly and then sieving them to obtain a mixed material;

[0028] (2) keeping the mixture at 900-1200° C. for 1-2 hours and cooling;

[0029] (3) The cooled glass is crushed into a particle size of 1 μm-5 μm to obtain the glass powder.

[0030] The invention also provides application of the glass powder in preparing a multilayer ceramic capacitor.

[0031] After sintering, the copper conductive paste prepared by the glass powder of the present invention effectively reduces the dielectric loss and improves the dielectric performance of the multilayer ceramic capacitor while ensuring the density of the film strip, the bonding strength between the terminal electrode and the substrate, and the acid resistance.

[0032] The glass powder of the present invention has a wide range of applications and can be used on multilayer ceramic capacitors of medium-high voltage, medium-high capacitance and COG specifications. The prepared copper conductive paste can be used on all sizes of 0201, 0402, 0603, 0805 and 1206.

[0033] Compared with the prior art, the present invention has the following beneficial effects:

[0034] The present invention adds Ba 2+ , Sr 2+ , Ca 2+ Mg 2+ Alkaline earth metals, while ensuring the tight structure of the glass, adjust the thermal expansion coefficient of the glass to be consistent with the matrix, improve the matching with the matrix, and enhance the bonding strength between the glass and the matrix, which is beneficial to reduce the dielectric loss of the product.

[0035] The present invention can ensure good wettability between glass, copper powder and substrate by adjusting the ratio of Si and B elements in the glass, change the softening point of the glass, and ensure its chemical stability, so that it can be well connected with copper powder and substrate, and the glass powder can be used in multilayer ceramic capacitors of different specifications. At the same time, the present invention also adds appropriate Al2O3 as an intermediate oxide to adjust the symmetric relationship of [SiO4], [BO4], and [BO3], and adds appropriate alkali metals such as Li2O and Na2O and K2O to reduce the high-temperature viscosity of the glass melt, increase the oxygen content to make [BO3] transform to [BO4], thereby stabilizing the glass structure. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 This is a topographical image of the end of a multilayer ceramic capacitor prepared using the glass powder described in Comparative Example 1;

[0037] Figure 2 This is a morphology diagram of the end of a multilayer ceramic capacitor prepared using the glass powder described in Example 6. DETAILED DESCRIPTION

[0038] To better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with the accompanying drawings and specific embodiments. Those skilled in the art should understand that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0039] In the examples, the experimental methods used are conventional methods unless otherwise specified, and the materials, reagents, etc. used are all commercially available unless otherwise specified.

[0040] Embodiment 1-11

[0041] The embodiments of the glass powder for copper conductive paste of the present invention, the formulas of embodiments 1-11 are shown in Table 1, and the preparation method comprises the following steps:

[0042] (1) Weighing each oxide raw material according to the mass percentage in Table 1, mixing them evenly and then sieving them to obtain a mixed material;

[0043] The mixing equipment can be at least one of a rotary (V-type, double cone type, three-dimensional type) mixer, a disk type (moving disk type, fixed disk type) mixer, and a paddle type mixer; the mixing equipment used in the present invention is a V-type mixer;

[0044] (2) adding the mixture into a crucible, keeping the temperature at 900-1200° C. for 1-2 hours, and then rapidly cooling the molten glass; in the specific operation of the present invention, keeping the temperature at 1100° C. for 1 hour, and then rapidly cooling the molten glass;

[0045] The crucible can be at least one of a ceramic crucible (quartz, corundum, zirconium corundum, zirconium quartz, mullite, clay, etc.), a metal crucible (platinum, platinum-gold alloy, platinum-rhodium alloy, etc.) and other ceramic-metal composite crucibles, and the cooling treatment method can be at least one of water quenching, rolling mill, copper plate, wire drawing, and mold cooling molding; the crucible used in the present invention is a quartz crucible, and the cooling treatment method is rolling mill cooling,

[0046] (3) The cooled glass is crushed and sieved to obtain glass powder with a particle size of 1 μm-5 μm.

[0047] Among them, the mass ratio of MgO, CaO and SrO is 2.5:2.5:1, and the mass ratio of Li2O, Na2O and K2O is 1:2:1.

[0048] Embodiments 12 to 15

[0049] The embodiments of the glass powder for copper conductive paste according to the present invention, embodiments 12 to 15 are different from embodiment 1 only in that the mass ratios of MgO, CaO, and SrO in the alkaline earth metal oxides in the glass powder are different. The mass ratio of MgO, CaO, and SrO in embodiment 12 is 0.1:0.1:1; the mass ratio of MgO, CaO, and SrO in embodiment 13 is 5:5:1; the mass ratio of MgO, CaO, and SrO in embodiment 14 is 7:5:1; in embodiment 15, the alkaline earth metal oxides include only two types, MgO and SrO, and the mass ratio is 1:1.

[0050] Embodiments 16 to 18

[0051] The embodiments of the glass powder for copper conductive paste according to the present invention, embodiments 16 to 18 are different from embodiment 1 only in that the mass ratios of Li2O, Na2O, and K2O in the alkali metal oxides in the glass powder are different. In embodiment 16, the mass ratio of Li2O, Na2O, and K2O is 1:3:2; in embodiment 17, K2O is not contained, and the mass ratio of Li2O and Na2O is 1:0.1; in embodiment 18, the mass ratio of Li2O, Na2O, and K2O is 1:3:3.

[0052] Comparative Example 1

[0053] A glass powder for copper conductive paste, the formula of which is shown in Table 1, and the preparation method is the same as that of Example 1.

[0054] The terminal electrodes of the multilayer ceramic capacitor are prepared using the above glass powder, and the preparation method is as follows:

[0055] (1) dissolving 10 parts by weight of glass powder, 70 parts by weight of copper powder and 5 parts by weight of an organic resin binder in 15 parts by weight of an alcohol solvent, and kneading the mixture in a roller mill to prepare a conductive paste; wherein the organic resin binder is ethyl cellulose and the alcohol solvent is pine alcohol;

[0056] (2) The terminal part of the multilayer ceramic capacitor with an internal nickel electrode is immersed in the conductive paste, and then dried at 120°C for 20 minutes. After drying, it is sintered in a nitrogen furnace with an oxygen concentration of 50 ppm. The sintering temperature is 820°C and the sintering time is 1 hour to obtain a terminal electrode with a thickness of 40 μm.

[0057] The performance test of the multilayer ceramic capacitor prepared as above was carried out. The specific test method is as follows. The test results of dielectric loss and bonding strength are shown in Table 2. The test results of glass density of Comparative Example 1 and Example 6 are shown in Table 2. Figure 1 , Figure 2 As shown:

[0058] (1) Dielectric loss: loss tangent, the ratio of active power lost in the resistor to reactive power stored in the capacitor at frequencies of 800 MHz to 40 GHz;

[0059] (2) Bonding strength between glass and substrate (tensile strength): Two iron wires are welded on both sides of the copper end, and the welding point is pulled apart using a tensile testing machine. The tensile strength is evaluated based on the magnitude of the tensile force and the position where the copper end falls off;

[0060] (3) Glass density: After DPA curing, the copper end section was polished and ground, the SEM morphology was tested, and the depth of nickel plating liquid penetrating into the copper end was measured.

[0061] Table 1

[0062]

[0063]

[0064] Table 2

[0065] Dielectric loss %(X5R) Dielectric loss %(COG) Tensile strength kgf(COG) Tensile strength kgf(X5R) Example 1 4 0.01 4.5 5 Example 2 4.2 0.01 4.4 4.8 Example 3 4 0.01 4.3 4.8 Example 4 5.4 0.02 2.8 3.4 Example 5 5.8 0.02 2.3 3.2 Example 6 7 0.02 4.5 4.9 Example 7 4.5 0.02 5 5.2 Example 8 4 0.01 3.3 3.8 Example 9 4 0.01 3.0 3.5 Example 10 4 0.01 3.5 3.9 Embodiment 11 4.5 0.02 4.2 4.7 Example 12 4.1 0.01 4.2 4.8 Embodiment 13 4.3 0.01 4.2 4.7 Embodiment 14 7.5 0.03 1.0 2.0 Embodiment 15 7.5 0.03 0.5 1.2 Example 16 4.4 0.01 4.2 4.7 Embodiment 17 4.4 0.01 4.0 4 Embodiment 18 7 0.03 1.7 2.8 Comparative Example 1 8 0.03 0.7 1.0

[0066] As can be seen from Table 2, compared with ordinary glass powder (Comparative Example 1), the glass powder of the present invention is more conducive to reducing the dielectric loss of multilayer ceramic capacitors, and the tensile strength is significantly improved. From the comparison of the glass powders of Examples 1-5, it can be seen that in the glass powder of the present invention, when the ratio of BaO to alkaline earth metal oxide is in the preferred range, it can not only ensure good glass wettability, suitable linear expansion coefficient and copper end density, but also reduce the crystallization trend and improve the reliability of the product, especially when the mass ratio of BaO to alkaline earth metal oxide is preferably in the range of (5-10): 1, the product has better tensile strength and dielectric loss. From the comparison of the glass powders obtained in Examples 1-11 and 12-15, it can be seen that the Sr in the alkaline earth metal oxide in its composition 2+ , Ca 2+ Mg 2+ The three alkaline earth metal elements have some influence on the refractive index, molar volume, thermal expansion coefficient, etc. of the glass. When the mass ratio of the three oxides is adjusted within the preferred range of (0.1-5): (0.1-5): 1, the comprehensive performance of the product is better. Among the alkali metal oxides in the glass powder of the present invention, Na2O and K2O play a role in disconnecting the network, and Li2O plays a role in agglomerating. The compounding of alkali metal oxide A and Li2O can produce a mixed alkali effect, thereby improving the ion diffusion, chemical stability and electrical properties of the glass. When the mass ratio of Na2O, K2O and Li2O is preferably (0.1-5): 1, as shown in Example 1 and Examples 16-18, the dielectric loss of the product is lower and the chemical stability is better. The components in the alkaline earth metal oxide can synergistically adjust the thermal expansion coefficient of the glass, further reduce the viscosity in the high temperature zone and the low temperature zone, reduce the stress of the bonding layer between the glass and the substrate, and further improve the durability of the multilayer ceramic capacitor.

[0067] Comparative Example 1 uses ordinary glass powder ( Figure 1 ) and the glass powder of Example 6 ( Figure 2 ) It can be seen from the morphology of the end prepared by the glass powder of the present invention that the density of the end can be improved, the connection between the glass and the substrate is better, the electroplating will not nickel infiltrate, the durability of the capacitor is improved, and the dielectric loss is reduced.

[0068] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A glass powder for copper conductive paste, It is characterized in that The glass powder comprises the following components in parts by weight based on oxides: SiO 2 3-45 parts, Al 2 O 3 3-12 parts, BaO 3-50 parts, B 2 O 3 12-25 parts, alkali metal oxide 1-11 parts, alkaline earth metal oxide 2.5-10 parts; the alkali metal oxide is alkali metal oxide A and Li 2 O, the alkali metal oxide A is Na 2 O and K 2 O; the alkaline earth metal oxide is a compound of MgO, CaO and SrO.

2. The glass powder for copper conductive paste according to claim 1, It is characterized in that The alkali metal oxide A and Li 2 The mass ratio of O is (0.1-5):

1.

3. The glass powder for copper conductive paste according to claim 1, It is characterized in that The mass ratio of MgO, CaO and SrO in the alkaline earth metal oxide is (0.1-5):(0.1-5):

1.

4. The glass powder for copper conductive paste according to claim 1, It is characterized in that The mass ratio of the BaO to the alkaline earth metal oxide is (5-10):

1.

5. The glass powder for copper conductive paste according to any one of claims 1 to 4, It is characterized in that The glass powder further comprises CuO, Cu 2 O、TiO 2 、MnO 2 、V 2 O 5 , ZnO or at least one of the above.

6. The glass powder for copper conductive paste according to claim 5, It is characterized in that Having at least one of the following features (a)-(e): (a) The weight percentage of CuO in the glass powder is 0-8 parts, Cu 2 The weight portion of O is 0-8 parts; (b) TiO in the glass powder 2 The weight portion is 0-5 parts; (c) MnO in the glass powder 2 The weight portion is 0-10 parts; (d) V in the glass powder 2 O 5 The weight portion is 0-20 parts; (e) The weight proportion of ZnO in the glass powder is 0-30 parts.

7. A method for preparing glass powder for copper conductive paste according to any one of claims 1 to 6, It is characterized in that The following steps are involved: (1) Weighing each component in proportion, mixing them evenly and then sieving them to obtain a mixed material; (2) keeping the mixture at 900-1200° C. for 1-2 hours and cooling; (3) The cooled glass is crushed into a particle size of 1 μm-5 μm to obtain the glass powder.

8. Use of the glass powder for copper conductive paste according to any one of claims 1 to 7 in preparing multilayer ceramic capacitors.