Preparation method of methyl cyclohexanediamine
By using Ru/MgAlO catalyst and optimizing reaction conditions, the problem of catalyst deactivation during the hydrogenation of MTDA to prepare methylcyclohexanediamine was solved, and a catalyst with high selectivity and long life was achieved, which is suitable for industrial production.
Patent Information
- Application Number
- CN202410845286.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-06-19
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-29
AI Technical Summary
There are deamination condensation side reactions in the existing process of hydrogenating MTDA to prepare methylcyclohexanediamine, which leads to catalyst deactivation, and the catalyst preparation cost is high, making it difficult to achieve high selectivity and stability.
The Ru/MgAlO catalyst was used to prepare the catalyst by co-precipitation method, and the reaction conditions (temperature, pressure, time) were optimized to suppress the condensation deamination side reaction and improve the selectivity of methylcyclohexanediamine and the stability of the catalyst.
It achieves high selectivity of methylcyclohexanediamine (>95%) and long catalyst life (20 cycles), reduces production costs, and is suitable for industrial-scale production.
Smart Images

Figure CN118851918A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of methylcyclohexanediamine preparation, and in particular relates to a method for preparing methylcyclohexanediamine. Background Art
[0002] Methylcyclohexanediamine (HTDA) is an important fine chemical that can be directly used as a raw material for epoxy resin curing agent. It has the properties of fast curing, low toxicity, water resistance, heat resistance and chemical corrosion resistance, and is widely used in coatings, adhesives and composite materials. HTDA can also be used as a raw material for detergents, pharmaceutical intermediates, dyes and methylcyclohexane diisocyanate, among which methylcyclohexane diisocyanate can be used to prepare aliphatic polyurethane, an important functional material with wide applications. HTDA is mainly produced by hydrogenating meta-toluenediamine (MTDA) raw material in an intermittent reactor.
[0003] Chinese patent CN106994344A discloses a catalyst for hydrogenating toluenediamine to prepare methylcyclohexanediamine, which uses alumina as a carrier and is impregnated with metal ruthenium and other active metals. The conversion rate of toluenediamine is higher than 99%, and the selectivity of methylcyclohexanediamine is higher than 92%. However, the solution has the problem of long reaction time and greatly increased production cost. Chinese patent CN105924359A discloses a supported metal catalyst and an inorganic salt auxiliary agent system for the preparation of methylcyclohexanediamine. The patent can reduce 70-95% of deamination byproducts by adding inorganic salt auxiliary agents such as sodium sulfate and sodium phosphate, and significantly improve the total yield of HTDA products, which can reach 90-97%. US Patent No. 4186145 discloses a MTDA hydrogenation catalyst, which uses manganese and chromium oxides or hydroxides as carriers and a precipitation method to prepare the catalyst. Under high temperature reaction, the catalyst has high selectivity, less deamination byproducts, and high stability, and is not easy to deactivate. However, the catalyst preparation process is complicated, and the preparation of the oxide carrier involves multiple precipitation, separation and washing processes, and the preparation cost is high. Chinese Patent No. CN102688757A discloses a catalyst for preparing cyclohexanediamine by hydrogenation of phenylenediamine under ammonia conditions. The catalyst consists of three parts: a main active component (Ru or Pd), an auxiliary agent and a carrier (Al2O3 or SiO2). Phenylenediamine can be highly active and highly selectively converted into a variety of amine products with cyclohexanediamine as the main product, but Al2O3 and SiO2 carriers have certain acidity, which will cause -NH2 to be more easily adsorbed on the hydrogenation active site than the benzene ring, resulting in a deamination side reaction, resulting in a decrease in the selectivity of the main product and a decrease in the activity of the catalyst, and even inactivation.
[0004] As can be seen from the above, deamination condensation side reactions will occur during the hydrogenation of MTDA to produce HTDA, generating impurities such as secondary amines and tertiary amines. In addition, if the acidity of the catalyst is too strong, the product HTDA molecules will also condense and deaminize to generate high-boiling impurities such as secondary amines, tertiary amines or cross-linked amines. These impurities are adsorbed and deposited on the catalyst surface, blocking the catalyst pores, covering the active sites, and causing the catalyst to deactivate rapidly. Therefore, designing a slightly alkaline catalyst with the ability to inhibit the condensation deamination side reaction and using it for the autoclave hydrogenation to produce HTDA has become a problem that needs to be solved urgently. Summary of the invention
[0005] In view of the shortcomings of the prior art, the technical problem to be solved by the present invention is to overcome the catalyst deactivation problem caused by the condensation deamination side reaction in the existing MTDA hydrogenation process to HTDA, and to propose a method for preparing methylcyclohexanediamine which can effectively inhibit the condensation deamination side reaction, has good catalytic activity and high selectivity for the methylcyclohexanediamine product.
[0006] In order to solve the technical problem, the technical solution adopted by the present invention is:
[0007] The invention provides a method for preparing methylcyclohexanediamine. Meta-toluenediamine is used as a raw material. Under the catalytic action of a catalyst, a hydrogenation reaction is carried out to generate methylcyclohexanediamine under the conditions of a reaction temperature of 120-230 DEG C, a H2 pressure of 3.0-10.0MPa, and a reaction time of 5-20h. The catalyst uses Ru as an active component and MgAlO as a carrier. The concentration of the meta-toluenediamine is 30-50%, and the amount of the catalyst used accounts for 3-10% of the amount of the meta-toluenediamine used.
[0008] Preferably, the content of Ru in the catalyst is 1-10% of the mass of the catalyst.
[0009] Preferably, the catalyst is prepared by the following method:
[0010] S1: dissolving a soluble metal ruthenium salt, magnesium nitrate and aluminum nitrate in water to form solution 1; dissolving sodium carbonate in water to form solution 2; the metal ruthenium salt is selected from ruthenium chloride or ruthenium acetylacetonate;
[0011] S2: Add solution 1 and solution 2 dropwise into water at the same time, stir at room temperature, wash and dry to obtain a solid powder;
[0012] S3: reducing the solid powder in a hydrogen atmosphere at 200-500° C. for 1-24 h to obtain a Ru / MgAlO catalyst.
[0013] Preferably, in S1, 76 g of magnesium nitrate hexahydrate, 30 g of aluminum nitrate nonahydrate and 5.8 g of hydrated ruthenium trichloride are weighed and dissolved in water to form solution 1.
[0014] Preferably, in S2, stirring is performed at room temperature for 1-24 hours, followed by washing with water and ethanol, respectively, and drying in a vacuum oven at 80-120° C. for 1-24 hours.
[0015] Preferably, in S2, stirring is performed at room temperature for 8-15 hours.
[0016] Preferably, in S3, the reduction is carried out in a hydrogen atmosphere at 300-400° C. for 1-24 h.
[0017] Preferably, m-toluenediamine is used as the raw material, and at least one of N,N-dimethylformamide, N,N-dimethylacetamide, tetrahydrofuran, isopropanol, toluene, methanol and triethylamine is used as the organic solvent; the mass fraction of the m-toluenediamine is 3-20%.
[0018] Preferably, the mass fraction of the meta-toluenediamine is 4-15%.
[0019] Preferably, the reaction temperature is 150-200° C., the H 2 pressure is 5.0-9.0 MPa, and the reaction time is 7-12 h.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] The invention provides a method for preparing methylcyclohexanediamine, wherein a Ru-based catalyst prepared by a simple coprecipitation method is used as a catalyst, and reaction conditions (including reaction temperature, H2 pressure, and reaction time) are optimized, so that condensation deamination side reactions are effectively suppressed, and MTDA is prepared into HTDA by highly selective hydrogenation, with a conversion rate of more than 99%, a selectivity of more than 95%, and the catalyst can be cycled and maintained stable for 20 times. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is the gas phase spectrum provided in Example 1 of the present invention. DETAILED DESCRIPTION
[0023] The technical scheme in the specific embodiment of the present invention is described in detail and completely below. Obviously, the described embodiment is only a part of the specific implementation of the overall technical scheme of the present invention, rather than all implementations. Based on the overall concept of the present invention, all other embodiments obtained by ordinary technicians in this field fall within the scope of protection of the present invention.
[0024] The invention provides a method for preparing methylcyclohexanediamine, wherein m-toluenediamine is used as a raw material, and a hydrogenation reaction is carried out under the catalytic action of a catalyst under the conditions of a reaction temperature of 120-230° C., a H2 pressure of 3.0-10.0 MPa, and a reaction time of 5-20 hours to generate methylcyclohexanediamine; the catalyst uses Ru as an active component and MgAlO as a carrier; the concentration of the m-toluenediamine is 30-50%, and the amount of the catalyst accounts for 3-10% of the amount of the m-toluenediamine. It should be noted that the amount of the raw material (m-toluenediamine) needs to be determined according to the reaction container, and the concentration of the raw material is 30-50% determined by the above technical solution. The preparation method of methylcyclohexanediamine limits the type of catalyst. The catalyst uses MgAlO as a carrier, and metal Ru is in-situ doped during the coprecipitation synthesis process, and then reduced to obtain a Ru-based metal catalyst with high specific surface area, high metal dispersion and alkalinity. The MgAlO carrier material has the advantages of high specific surface area, unique pore structure and excellent stability, providing an excellent place for the reaction, which is conducive to the diffusion of MTDA to the active site and accelerating the hydrogenation reaction. The MgAlO carrier makes the catalyst alkaline as a whole, avoids the addition of additional inhibitors, inhibits the deamination condensation side reaction during the MTDA hydrogenation process, and obtains a highly selective HTDA product. Metal Ru salt is added during the synthesis of Ru / MgAlO, and the metal Ru is highly dispersed or embedded in the MgAlO carrier produced by coprecipitation through coordination with Al, and the metal component in the catalyst is firmly stabilized, which can improve the catalyst stability.
[0025] The above-mentioned preparation method of methylcyclohexanediamine also defines the preparation conditions (including reaction temperature, H2 pressure, and reaction time). It can be understood that the reaction temperature can also be 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, 190°C, 200°C, 210°C, 220°C and any point value within the range thereof; the H2 pressure can also be 4.0MPa, 5.0MPa, 6.0MPa, 7.0MPa, 8.0MPa, 9.0MPa and any point value within the range thereof; the reaction time can also be 10h, 15h and any point value within the range thereof. It should be noted that the catalytic reaction process is not only closely related to the catalyst, but also closely related to the reaction conditions (especially reaction temperature and pressure). The present invention adopts Ru / MgAlO catalyst for catalytic reaction, and cooperates with the reaction conditions so that the catalyst exhibits excellent catalytic performance in the MTDA hydrogenation to HTDA reaction, with a conversion rate of >99% and a selectivity of >95%. The catalyst can maintain stability for 20 cycles and is suitable for industrial-scale production.
[0026] In a preferred embodiment, the content of Ru in the catalyst is 1-10% of the mass of the catalyst. The technical solution specifically limits the content of Ru because the Ru component is the active site for hydrogenation of the benzene ring. Too little Ru content will lead to insufficient hydrogenation, and too much Ru content will lead to high catalytic costs. Therefore, a suitable Ru content is required to ensure that the reaction proceeds and control the reaction catalytic cost. It is understandable that the content of Ru can also be 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9% and any point value within the range.
[0027] In a preferred embodiment, the catalyst is prepared by the following method:
[0028] S1: dissolving a soluble metal ruthenium salt, magnesium nitrate and aluminum nitrate in water to form solution 1; dissolving sodium carbonate in water to form solution 2; the metal ruthenium salt is selected from ruthenium chloride or ruthenium acetylacetonate;
[0029] S2: Add solution 1 and solution 2 dropwise into water at the same time, stir at room temperature, wash and dry to obtain a solid powder;
[0030] S3: reducing the solid powder in a hydrogen atmosphere at 200-500°C for 1-24h to obtain a Ru / MgAlO catalyst. It is understood that the temperature may also be 250°C, 300°C, 350°C, 400°C, 450°C and any point value within the range.
[0031] In the preparation method of the above catalyst, the alkaline carrier MgO is directly used as the main material, a small amount of Al2O3 is introduced during the synthesis process, and the Ru active component is doped in situ to form a Ru / MgAlO catalyst. Among them, Al2O3 is used to adjust the surface acidity and alkalinity of the catalyst, while increasing the surface area of the carrier and promoting the dispersion of the active component on the carrier to adapt to the hydrogenation reaction of meta-toluenediamine. Compared with Al2O3 or SiO2 carriers, MgAlO has moderate acidity and alkalinity, which can greatly avoid the phenomenon that -NH2 is more easily adsorbed on the hydrogenation active site, and the benzene ring is adsorbed on the metal active site for hydrogenation to generate methylcyclohexanediamine. In the catalytic reaction process, the characteristics of the catalyst such as high specific surface area, high dispersion of metal components and partial alkalinity are combined to promote the autoclave hydrogenation reaction of meta-toluenediamine, inhibit the condensation deamination side reaction, improve the stability of the catalyst and the selectivity of the methylcyclohexanediamine product, and after the catalyst is circulated 20 times, the conversion rate of meta-toluenediamine is still>99%, and the selectivity of methylcyclohexanediamine is>95%, which can be suitable for industrial production.
[0032] In a preferred embodiment, 76 g of magnesium nitrate hexahydrate, 30 g of aluminum nitrate nonahydrate and 5.8 g of hydrated ruthenium trichloride are weighed and dissolved in water to form a solution 1.
[0033] In a preferred embodiment, in S2, stirring is performed at room temperature for 1-24 hours, followed by washing with water and ethanol, respectively, and drying in a vacuum oven at 80-120° C. for 1-24 hours. In a preferred embodiment, in S2, stirring is performed at room temperature for 8-15 hours. In a preferred embodiment, in S3, reduction is performed at 300-400° C. in a hydrogen atmosphere for 1-24 hours.
[0034] In a preferred embodiment, m-toluenediamine is used as a raw material, and at least one of N,N-dimethylformamide, N,N-dimethylacetamide, tetrahydrofuran, isopropanol, toluene, methanol, and triethylamine is used as an organic solvent; the mass fraction of m-toluenediamine is 3-20%. This technical solution specifically defines the solvent composition because the solvent defined in this embodiment can ensure the full dissolution of the reaction components and avoid the occurrence of other side reactions. It is understandable that the mass fraction of m-toluenediamine can also be 5%, 10%, 15%, and any point value within the range thereof.
[0035] In a preferred embodiment, the mass fraction of the meta-toluenediamine is 4-15%. It is understandable that the mass fraction of the meta-toluenediamine can also be 6%, 8%, 10%, 12%, 14% and any value within the range.
[0036] In a preferred embodiment, the reaction temperature is 150-200° C., the H 2 pressure is 5.0-9.0 MPa, and the reaction time is 7-12 h.
[0037] In order to more clearly and in detail introduce a method for preparing methylcyclohexanediamine provided by an embodiment of the present invention, it will be described below in conjunction with specific examples.
[0038] Example 1
[0039] Weigh 76g of magnesium nitrate hexahydrate, 30g of aluminum nitrate nonahydrate and 5.8g of hydrated ruthenium trichloride and dissolve them in 200mL of water, which is recorded as solution 1. Weigh 98g of sodium carbonate and dissolve them in 200mL of water, which is recorded as solution 2. Add solution 1 and solution 2 dropwise into 300mL of water at the same time, stir at room temperature for 12h, then wash with water and ethanol respectively, and dry in a vacuum oven at 100°C for 12h. The solid powder obtained by drying is placed in a tubular furnace and reduced at 400°C in a hydrogen atmosphere for 12h to obtain Ru / MgAlO catalyst 1.
[0040] The hydrogenation reaction of m-toluenediamine was evaluated in a batch reactor. 50 g of m-toluenediamine, 1.5 g of catalyst 1 and 150 mL of isopropanol were charged into the reactor. The reactor was tightened and hydrogen was introduced. The reaction temperature was 170°C, the H2 reaction pressure was 8 MPa, and the reaction time was 12 h.
[0041] The reaction product solution was analyzed by gas chromatography. After 20 cycles of the catalyst, the conversion rate of m-toluenediamine was still 99%, and the selectivity of methylcyclohexanediamine was 95.1%. The gas chromatography spectrum is shown in Figure 1 shown.
[0042] Example 2
[0043] 76 g of magnesium nitrate hexahydrate, 30 g of aluminum nitrate nonahydrate and 5.8 g of ruthenium acetylacetonate were weighed and dissolved in 200 mL of water, which was recorded as solution 1. 98 g of sodium carbonate was weighed and dissolved in 200 mL of water, which was recorded as solution 2. Solution 1 and solution 2 were simultaneously added dropwise to 300 mL of water, stirred at room temperature for 12 h, then washed with water and ethanol respectively, and dried in a vacuum oven at 100 ° C for 12 h. The solid powder obtained by drying was placed in a tubular furnace and reduced at 400 ° C for 12 h in a hydrogen atmosphere to obtain Ru / MgAlO catalyst 2.
[0044] The hydrogenation reaction of m-toluenediamine was evaluated in a batch reactor. 50 g of m-toluenediamine, 1.5 g of catalyst 2 and 150 mL of isopropanol were loaded into the reactor. The reactor was tightened and hydrogen was introduced. The reaction temperature was 170°C, the H2 reaction pressure was 8 MPa, and the reaction time was 12 h.
[0045] The reaction product solution was analyzed by gas chromatography. After 20 cycles of the catalyst, the conversion rate of m-toluenediamine was 97%, and the selectivity of methylcyclohexanediamine was 93.5%.
[0046] Example 3
[0047] 76 g of magnesium nitrate hexahydrate, 30 g of aluminum nitrate nonahydrate and 2.9 g of hydrated ruthenium trichloride were weighed and dissolved in 200 mL of water, which was recorded as solution 1. 98 g of sodium carbonate was weighed and dissolved in 200 mL of water, which was recorded as solution 2. Solution 1 and solution 2 were simultaneously added dropwise to 300 mL of water, stirred at room temperature for 12 h, then washed with water and ethanol respectively, and dried in a vacuum oven at 100° C. for 12 h. The solid powder obtained by drying was placed in a tubular furnace and reduced at 400° C. in a hydrogen atmosphere for 12 h to obtain the Ru / MgAlO catalyst 3.
[0048] The hydrogenation reaction of m-toluenediamine was evaluated in a batch reactor. 50 g of m-toluenediamine, 1.5 g of catalyst 3 and 150 mL of tetrahydrofuran were charged into the reactor. The reactor was tightened and hydrogen was introduced. The reaction temperature was 170°C, the H2 reaction pressure was 8 MPa, and the reaction time was 12 h.
[0049] The reaction product solution was analyzed by gas chromatography. After 20 cycles of the catalyst, the conversion rate of m-toluenediamine was 96%, and the selectivity of methylcyclohexanediamine was 90.1%.
[0050] Example 4
[0051] The hydrogenation reaction of m-toluenediamine was evaluated in a batch reactor. 30 g of m-toluenediamine, 1.5 g of catalyst 1 and 150 mL of isopropanol were charged into the reactor. The reactor was tightened and hydrogen was introduced. The reaction temperature was 170°C, the H2 reaction pressure was 8 MPa, and the reaction time was 12 h.
[0052] The reaction product solution was analyzed by gas chromatography. After the catalyst was circulated 20 times, the conversion rate of m-toluenediamine was still 99%, and the selectivity of methylcyclohexanediamine was 97%.
[0053] Example 5
[0054] The hydrogenation reaction of m-toluenediamine was evaluated in a batch reactor. 70 g of m-toluenediamine, 1.5 g of catalyst 1 and 150 mL of isopropanol were charged into the reactor. The reactor was tightened and hydrogen was introduced. The reaction temperature was 170°C, the H2 reaction pressure was 8 MPa, and the reaction time was 12 h.
[0055] The reaction product solution was analyzed by gas chromatography. After the catalyst was circulated 20 times, the conversion rate of m-toluenediamine was still 92%, and the selectivity of methylcyclohexanediamine was 90.5%.
[0056] Example 6
[0057] The hydrogenation reaction of m-toluenediamine was evaluated in a batch reactor. 50 g of m-toluenediamine, 0.9 g of catalyst 1 and 150 mL of isopropanol were charged into the reactor. The reactor was tightened and hydrogen was introduced. The reaction temperature was 170°C, the H2 reaction pressure was 8 MPa, and the reaction time was 12 h.
[0058] The reaction product solution was analyzed by gas chromatography. After 20 cycles of the catalyst, the conversion rate of m-toluenediamine was still 89%, and the selectivity of methylcyclohexanediamine was 89.7%.
[0059] Example 7
[0060] The hydrogenation reaction of m-toluenediamine was evaluated in a batch reactor. 50 g of m-toluenediamine, 3.5 g of catalyst 1 and 150 mL of isopropanol were charged into the reactor. The reactor was tightened and hydrogen was introduced. The reaction temperature was 170°C, the H2 reaction pressure was 8 MPa, and the reaction time was 12 h.
[0061] The reaction product solution was analyzed by gas chromatography. After 20 cycles of the catalyst, the conversion rate of m-toluenediamine was still 99%, and the selectivity of methylcyclohexanediamine was 96.8%. The catalytic reaction conditions and reaction results of Examples 1-7 are shown in Table 1.
[0062] Table 1 Catalytic reaction conditions and reaction results of Examples 1-7
[0063]
[0064] From the results in Table 1, it can be found that, considering the Ru component raw material, hydrated ruthenium trichloride is more suitable for the reaction system. The amount of Ru component added was screened. If the Ru content was low, the hydrogenation reaction was insufficient and the benzene ring was not fully hydrogenated. The amount of MTDA added was screened. It was found that as the raw material increased, the reaction effect gradually became worse.
[0065] Comparative Example 1
[0066] The hydrogenation reaction of m-toluenediamine was evaluated in a batch reactor. 50 g of m-toluenediamine, 1.5 g of catalyst 1 and 150 mL of tetrahydrofuran were charged into the reactor. The reactor was tightened and hydrogen was introduced. The reaction temperature was 110°C, the H2 reaction pressure was 8 MPa, and the reaction time was 12 h.
[0067] The reaction product solution was analyzed by gas chromatography. After the catalyst was circulated 20 times, the conversion rate of m-toluenediamine was 78%, and the selectivity of methylcyclohexanediamine was 75%.
[0068] Comparative Example 2
[0069] The hydrogenation reaction of m-toluenediamine was evaluated in a batch reactor. 50 g of m-toluenediamine, 1.5 g of catalyst 1 and 150 mL of tetrahydrofuran were charged into the reactor. The reactor was tightened and hydrogen was introduced. The reaction temperature was 240°C, the H2 reaction pressure was 8 MPa, and the reaction time was 12 h.
[0070] The reaction product solution was analyzed by gas chromatography. After 20 cycles of the catalyst, the conversion rate of m-toluenediamine was 99%, and the selectivity of methylcyclohexanediamine was 78.6%.
[0071] Comparative Example 3
[0072] The hydrogenation reaction of m-toluenediamine was evaluated in a batch reactor. 50 g of m-toluenediamine, 1.5 g of catalyst 1 and 150 mL of tetrahydrofuran were charged into the reactor. The reactor was tightened and hydrogen was introduced. The reaction temperature was 170°C, the H2 reaction pressure was 2 MPa, and the reaction time was 12 h.
[0073] The reaction product solution was analyzed by gas chromatography. After 20 cycles of the catalyst, the conversion rate of m-toluenediamine was 64.2%, and the selectivity of methylcyclohexanediamine was 62.1%.
[0074] Comparative Example 4
[0075] The hydrogenation reaction of m-toluenediamine was evaluated in a batch reactor. 50 g of m-toluenediamine, 1.5 g of catalyst 1 and 150 mL of tetrahydrofuran were charged into the reactor. The reactor was tightened and hydrogen was introduced. The reaction temperature was 170°C, the H2 reaction pressure was 11 MPa, and the reaction time was 12 h.
[0076] The reaction product solution was analyzed by gas chromatography. After 20 cycles of the catalyst, the conversion rate of m-toluenediamine was 99%, and the selectivity of methylcyclohexanediamine was 85.2%.
[0077] Comparative Example 5
[0078] 76 g of magnesium nitrate hexahydrate, 30 g of aluminum nitrate nonahydrate and 5.8 g of hydrated nickel chloride were weighed and dissolved in 200 mL of water, which was recorded as solution 1. 98 g of sodium carbonate was weighed and dissolved in 200 mL of water, which was recorded as solution 2. Solution 1 and solution 2 were simultaneously added dropwise to 300 mL of water, stirred at room temperature for 12 h, then washed with water and ethanol respectively, and dried in a vacuum oven at 100° C. for 12 h. The solid powder obtained by drying was placed in a tubular furnace and reduced at 400° C. in a hydrogen atmosphere for 12 h to obtain Ni / MgAlO catalyst 4.
[0079] The hydrogenation reaction of m-toluenediamine was evaluated in a batch reactor. 50 g of m-toluenediamine, 1.5 g of catalyst 4 and 150 mL of tetrahydrofuran were charged into the reactor. The reactor was tightened and hydrogen was introduced. The reaction temperature was 170°C, the H2 reaction pressure was 8 MPa, and the reaction time was 12 h.
[0080] The reaction product solution was analyzed by gas chromatography. After 20 cycles of the catalyst, the conversion rate of m-toluenediamine was 95%, and the selectivity of methylcyclohexanediamine was 85.7%.
[0081] Comparative Example 6
[0082] 5.8 g of hydrated ruthenium trichloride was added to 100 mL of deionized water and stirred thoroughly. Then 10 g of Al2O3 was added to the above solution and stirred for 4 h. 1 mol / L NaOH solution was added to adjust the pH value to about 10, and stirring was continued for 4 h. The mixture was allowed to stand, filtered, and washed with deionized water. The solid powder obtained by drying was placed in a tubular furnace and reduced at 400 °C in a hydrogen atmosphere for 12 h to obtain Ru / Al2O3 catalyst 5.
[0083] The hydrogenation reaction of m-toluenediamine was evaluated in a batch reactor. 50 g of m-toluenediamine, 1.5 g of catalyst 5 and 150 mL of tetrahydrofuran were charged into the reactor. The reactor was tightened and hydrogen was introduced. The reaction temperature was 170°C, the H2 reaction pressure was 8 MPa, and the reaction time was 12 h.
[0084] The reaction product solution was analyzed by gas chromatography. After 20 cycles of the catalyst, the conversion rate of m-toluenediamine was 92.2%, and the selectivity of methylcyclohexanediamine was 89.7%. The catalytic reaction conditions and reaction results of Comparative Examples 1-6 are shown in Table 2.
[0085] Table 2 Comparative Examples 1-6 Catalytic Reaction Conditions and Reaction Results
[0086]
[0087] From the results in Table 2, it can be found that too high temperature will promote the conversion of raw material MTDA, but at the same time it will generate highly polymerized impurities, reducing the selectivity of the target product HTDA. High pressure will promote the conversion of m-phenylenediamine, but at the same time it will generate more deamination byproducts, reducing the selectivity of the main product. In addition, it was found that the selectivity of the HTDA product was not high when using Ru / Al2O3 catalyst. The reason is that the Al2O3 carrier has a certain acidity, which will cause -NH2 to be more easily adsorbed on the hydrogenation active site than the benzene ring, resulting in a deamination side reaction, resulting in a decrease in the selectivity of the main product.
Claims
1. A method for preparing methylcyclohexanediamine, characterized in that: Taking m-toluenediamine as raw material, under the catalytic action of a catalyst, a hydrogenation reaction occurs to generate methylcyclohexanediamine at a reaction temperature of 120-230° C., a H2 pressure of 3.0-10.0 MPa, and a reaction time of 5-20 h; the catalyst has Ru as an active component and MgAlO as a carrier; The concentration of the meta-toluenediamine is 30-50%, and the amount of the catalyst used accounts for 3-10% of the amount of the meta-toluenediamine used.
2. The method for preparing methylcyclohexanediamine according to claim 1, characterized in that: The content of Ru in the catalyst is 1-10% of the mass of the catalyst.
3. The method for preparing methylcyclohexanediamine according to claim 1, characterized in that: The catalyst is prepared by the following method: S1: dissolving a soluble metal ruthenium salt, magnesium nitrate and aluminum nitrate in water to form solution 1; dissolving sodium carbonate in water to form solution 2; the metal ruthenium salt is selected from ruthenium chloride or ruthenium acetylacetonate; S2: Add solution 1 and solution 2 dropwise into water at the same time, stir at room temperature, wash and dry to obtain a solid powder; S3: reducing the solid powder in a hydrogen atmosphere at 200-500° C. for 1-24 h to obtain a Ru / MgAlO catalyst.
4. The method for preparing methylcyclohexanediamine according to claim 3, characterized in that: In the S1, 76 g of magnesium nitrate hexahydrate, 30 g of aluminum nitrate nonahydrate and 5.8 g of hydrated ruthenium trichloride are weighed and dissolved in water to form a solution 1.
5. The method for preparing methylcyclohexanediamine according to claim 3, characterized in that: In the S2, the mixture is stirred at room temperature for 1-24 hours, then washed with water and ethanol respectively, and dried in a vacuum oven at 80-120° C. for 1-24 hours.
6. The method for preparing methylcyclohexanediamine according to claim 5, characterized in that: In the S2, stir at room temperature for 8-15h.
7. The method for preparing methylcyclohexanediamine according to claim 3, characterized in that: In the S3, reduction is carried out in a hydrogen atmosphere at 300-400° C. for 1-24 h.
8. The method for preparing methylcyclohexanediamine according to claim 1, characterized in that: Meta-toluenediamine is used as a raw material, and at least one of N,N-dimethylformamide, N,N-dimethylacetamide, tetrahydrofuran, isopropanol, toluene, methanol and triethylamine is used as an organic solvent; the mass fraction of the meta-toluenediamine is 3-20%.
9. The method for preparing methylcyclohexanediamine according to claim 8, characterized in that: The mass fraction of the meta-toluenediamine is 4-15%.
10. The method for preparing methylcyclohexanediamine according to claim 1, characterized in that: The reaction temperature is 150-200° C., the H 2 pressure is 5.0-9.0 MPa, and the reaction time is 7-12 h.
Citation Information
Cited By
Monatomic noble metal catalyst as well as preparation method and application thereof
CN119746851A