Triglycidyl 4-amino-3-methylphenol epoxy resin as well as preparation method and application thereof
By using 4-amino-3-methylphenol and a composite catalyst to increase the conversion rate of amino active hydrogen in the etherification grafting reaction, the problem of low conversion efficiency of amino active hydrogen in the preparation of triglycidyl aminophenol epoxy resin is solved , achieving resin preparation with high purity, high temperature stability and long storage period, suitable for electronic equipment and aerospace materials.
Patent Information
- Application Number
- CN202410860453.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-06-28
AI Technical Summary
The existing triglycidyl aminophenol epoxy resin has low amino active hydrogen conversion efficiency during the preparation process, resulting in low product monomer purity, poor stability over time, and short storage time.
Using 4-amino-3-methylphenol as the monomer, and using a composite catalyst in the etherification grafting reaction, such as a composite catalyst of sodium hydroxide aqueous solution and quaternary ammonium salt, to control reasonable pressure, temperature and reaction conditions, Carry out etherification grafting and ring-closing reactions to improve the conversion rate of amino active hydrogen and the purity of the product.
It improves the monomer purity and storage time of triglycidyl 4-amino-3-methylphenol epoxy resin, enhances its high-temperature stability and hydrophobic properties, and extends the storage period of the product.
Smart Images

Figure BDA0004919090910000011 
Figure BDA0004919090910000021 
Figure BDA0004919090910000031
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of high temperature resistant and low water absorption epoxy resins, and in particular relates to a triglycidyl 4-amino-3-methylphenol epoxy resin and a preparation method and application thereof. Background Art
[0002] Triglycidyl epoxy resins include p-aminophenol epoxy resins and m-aminophenol epoxy resins, and the triglycidyl aminophenol epoxy resins reported in the prior art, such as triglycidyl m-aminophenol epoxy resin, have the following structural formula:
[0003] After being cured with methyl tetrahydrophthalic anhydride, the Tg value is 241°C and the impact strength is 16-20KJ / m 2 , bending strength 180 ~ 190MPa, tensile strength 50 ~ 70MPa.
[0004] Since triglycidyl aminophenol epoxy resin has the advantages of low viscosity, good wettability, high Tg value after curing, high strength, and impact resistance, it can be widely used in the fields of electronic adhesives and aerospace composite materials. Its synthesis is prepared by the corresponding aminophenol precursor (such as p-aminophenol, m-aminophenol, o-aminophenol) and epichlorohydrin through etherification grafting addition reaction, ring closure reaction and other steps. Since the amino group in the aminophenol precursor has two active hydrogens, it needs to be etherified with 2 molecules of epichlorohydrin for ring opening. In the existing process, the amino reaction is incomplete, and the presence of a small amount of amino active hydrogen has a negative impact on the stability of the finished product over time. During the storage process, the remaining small amount of amino active hydrogen will act as a catalyst, causing the ring opening of the epoxy group, thereby causing the product viscosity to increase during storage, and even gelation occurs, resulting in product failure. The existing products of this series, such as the brand AFG-90 / MF-3101L, are specially marked with a storage period of only half a year. Therefore, there is an urgent need to improve the process of such products, improve the conversion efficiency of amino active hydrogen, synthesize finished products with high monomer content, improve temporal stability, and increase product shelf life, which is of great significance to the application of such products.
[0005] In summary, the current preparation process of triglycidylaminophenol epoxy resin has technical problems such as low amino conversion efficiency, resulting in low purity of the final product, poor stability over time, and short product storage time. Summary of the invention
[0006] The purpose of the present invention is to solve the technical problems that the conversion efficiency of amino active hydrogen is low during the preparation process of the above-mentioned triglycidyl aminophenol epoxy resin, resulting in low monomer purity of the final product, poor stability over time, short product storage time and the like, and to provide a triglycidyl 4-amino-3-methylphenol epoxy resin, which has the characteristics of high amino active hydrogen conversion rate during the product preparation process, high monomer purity of the final product, good stability over time, long storage time, good high-temperature stability, low water absorption after curing, and the like, and a preparation method and application thereof.
[0007] The technical principle of the present application is that the molecular structure of 4-amino-3-methylphenol contains a methyl electron-donating group, which greatly reduces the reactivity of the monomer molecule. In addition, since the ortho position of the amino group is substituted by a methyl group, the reactivity of 4-amino-3-methylphenol is even lower. There is also the defect that the active hydrogen of the amino group is not completely reacted in the etherification grafting reaction, and the purity of the finished monomer will be lower. However, combined with the synergistic effect of using a special catalyst in the preparation process and controlling reasonable pressure, temperature and other means during the reaction process, a triglycidyl 4-amino-3-methylphenol epoxy resin with high monomer purity, longer storage time and better hydrophobic properties can be synthesized in the end.
[0008] The technical solution of this application In the first aspect, the present application provides a triglycidyl 4-amino-3-methylphenol epoxy resin, using the following technical solution: a triglycidyl 4-amino-3-methylphenol epoxy resin, the chemical structure of which is as follows:
[0009] The above-mentioned triglycidyl 4-amino-3-methylphenol epoxy resin contains methyl groups in its structure, so that the triglycidyl 4-amino-3-methylphenol epoxy resin has high purity, good storage stability and better hydrophobicity (low water absorption rate) when compared with p-aminophenol epoxy resin or m-aminophenol epoxy resin in addition to having considerable physical and chemical advantages. For example, the epoxy equivalent is distributed in 105-116 g / eq (p-aminophenol epoxy resin or m-aminophenol epoxy resin epoxy equivalent is distributed in 100-111 g / eq), the easily saponifiable chlorine is distributed in 47-98 ppm (p-aminophenol epoxy resin or m-aminophenol epoxy resin easily saponifiable chlorine is also distributed in 50-200 ppm), and the data after curing are: Tg value is 245-250°C, impact strength is 25-46 KJ / m 2 , bending strength is 178~198MPa, tensile strength is 70~80MPa, and its water absorption rate is ≤0.1%.
[0010] In a second aspect, the present application provides a method for preparing the above-mentioned triglycidyl 4-amino-3-methylphenol epoxy resin, and the reaction equation of the preparation process is as follows (wherein NaOH+quaternary ammonium salt represents a catalyst): That is, firstly, 4-amino-3-methylphenol monomer and epichlorohydrin are subjected to an etherification grafting reaction under the action of a catalyst to obtain a product A, namely, 4-amino-3-methylphenol chlorohydrin ether; the obtained 4-amino-3-methylphenol chlorohydrin ether is then subjected to a ring-closing reaction with NaOH to obtain a triglycidyl 4-amino-3-methylphenol epoxy resin; The NaOH can be replaced by KOH.
[0011] The following technical solutions are adopted: A preparation method of triglycidyl 4-amino-3-methylphenol epoxy resin comprises the following steps: firstly, 4-amino-3-methylphenol monomer and epichlorohydrin are subjected to etherification grafting reaction under the action of a catalyst; the obtained 4-amino-3-methylphenol chlorohydrin ether (product A) and sodium hydroxide are subjected to a ring-closing reaction under the conditions of a negative pressure of 0.07-0.09 MPa and a temperature of 30-50 DEG C to obtain 4-amino-3-methylphenol epoxy resin and sodium chloride; in order to further reduce the easily saponifiable chlorine in the resin, sodium hydroxide is added once more after the ring-closing reaction to carry out a refining reaction; and then purification and the like are carried out to finally obtain triglycidyl 4-amino-3-methylphenol epoxy resin with high purity and good storage stability.
[0012] The preparation method of the above-mentioned triglycidyl 4-amino-3-methylphenol epoxy resin comprises the following specific preparation steps: (1) Etherification grafting reaction In a container, 4-amino-3-methylphenol monomer, epichlorohydrin, a catalyst and solvent I are added in sequence, and three active groups in the 4-amino-3-methylphenol monomer (two active hydrogens of the amino group and one active hydrogen of the hydroxyl group) and epichlorohydrin are subjected to etherification grafting reaction in solvent I at a temperature of 30 to 70° C. for 3 to 8 hours to obtain a reaction solution containing 4-amino-3-methylphenol chlorohydrin ether; The temperature of the above-mentioned etherification grafting reaction process is preferably 30-55° C., mainly to reduce the side reactions caused by high temperature, which will eventually cause the purity of the triglycidyl 4-amino-3-methylphenol epoxy resin product to decrease and the epoxy equivalent to increase; the specific side reactions are shown in the following reaction equation (wherein NaOH+quaternary ammonium salt represents the catalyst): That is, epichlorohydrin is hydrolyzed in an alkaline environment, and the resulting glycidol further reacts with the 4-amino-3-methylphenol monomer to generate a by-product having a structural formula such as the product B in the above reaction equation, wherein R1, R2, and R3 in the structural formula may be -OH or -Cl, but R1, R2, and R3 cannot be -Cl at the same time, because when they are -Cl at the same time, they are the product A of the etherification grafting reaction, i.e., 4-amino-3-methylphenol chlorohydrin ether, and the by-product may further undergo a ring-closing reaction with NaOH, resulting in a reduction in the monomer purity of the final product, triglycidyl 4-amino-3-methylphenol epoxy resin, thereby affecting the quality; The catalyst is at least one of an alkali metal solution, an alkaline earth metal salt, a quaternary ammonium salt, ethyl triphenylphosphine acetate, and triphenylphosphine; The alkali metal solution is a sodium hydroxide aqueous solution, and the sodium hydroxide aqueous solution can be replaced by a potassium hydroxide aqueous solution; The alkaline earth metal salt is calcium chloride, magnesium sulfate or barium sulfate; The quaternary ammonium salt is methyl trioctyl ammonium chloride, didecyl dimethyl ammonium chloride, dioctyl dimethyl ammonium chloride, dimethyl dioctadecyl ammonium chloride, benzyl dimethyl octyl ammonium chloride, dodecyl trimethyl ammonium chloride, octadecyl trimethyl ammonium chloride, tetraethyl ammonium bromide, benzyl triethyl ammonium chloride, benzyl diethyl ammonium bromide or benzyl trimethyl ammonium bromide; Preferably, the catalyst is composed of a quaternary ammonium salt and an alkali metal solution: the quaternary ammonium salt is dodecyl trimethyl ammonium chloride, the alkali metal solution is a sodium hydroxide aqueous solution with a mass percentage concentration of 40-50%, and the amount of dodecyl trimethyl ammonium chloride and the sodium hydroxide aqueous solution with a mass percentage concentration of 40-50% is calculated by mass ratio, and the dodecyl trimethyl ammonium chloride: the sodium hydroxide aqueous solution with a mass percentage concentration of 40-50% is 1:28-30; Preferably, the amount of the sodium hydroxide aqueous solution with a mass percentage concentration of 40-50% in the composite catalyst is 1:0.53 according to the molar ratio of 4-amino-3-methylphenol to the sodium hydroxide aqueous solution with a mass percentage concentration of 40-50%. The catalyst in the present application is only exemplified by a composite catalyst obtained by compounding an aqueous sodium hydroxide solution in an alkali metal solution and dodecyltrimethylammonium chloride in a quaternary ammonium salt, but does not limit the use of the other various catalysts listed above alone or in combination; The above preferred etherification grafting reaction process uses two composite catalysts, which effectively overcomes the effect of poor reaction activity caused by the methyl group contained in the 4-amino-3-methylphenol monomer, thereby greatly improving the reaction efficiency of the etherification grafting reaction between the three active groups in the 4-amino-3-methylphenol monomer (two active hydrogens of the amino group and one active hydrogen of the hydroxyl group) and epichlorohydrin, thereby improving the yield of the 4-amino-3-methylphenol epoxy resin product, which can reach up to 98.7%; Preferably, the sodium hydroxide aqueous solution in the catalyst is added in 2 to 5 batches, and added again after each reaction for 30 minutes; more preferably, it is added in 4 batches. The reason for this may be that it is added every 30 minutes, so that the reaction system will not cause too much temperature fluctuation due to the change of the added materials, thereby making the etherification grafting reaction stable and effective; The above-mentioned 4-amino-3-methylphenol: epichlorohydrin: catalyst is used in a molar ratio of 4-amino-3-methylphenol: epichlorohydrin: catalyst of 1:6-15:0.1-0.6; In the above-mentioned etherification grafting reaction stage, the amount of epichlorohydrin used has little effect on the reaction efficiency of the grafting reaction in the etherification stage, and has little effect on the purity of the final product triglycidyl 4-amino-3-methylphenol epoxy resin. However, in a reactor of the same volume, if the molar number of epichlorohydrin increases while the total amount of feed remains unchanged, the feed amount of 4-amino-3-methylphenol is bound to decrease, thereby causing the yield of triglycidyl 4-amino-3-methylphenol epoxy resin to decrease. Therefore, in order to improve the maximum utilization rate of the reactor, the present application preferably uses 4-amino-3-methylphenol: epichlorohydrin, and the molar ratio of 4-amino-3-methylphenol: epichlorohydrin is 1:6 to 10; The solvent I is an alcohol ether cosolvent, and the alcohol ether cosolvent is at least one of ethanol, butanol, ethylene glycol, propylene glycol, isopropanol, ethylene glycol monomethyl ether, propylene glycol monomethyl ether, and tripropylene glycol monomethyl ether; in the present application, only isopropanol is used as an example, but the use of other solvents in the above-mentioned alcohol ether cosolvent is not limited; The amount of the solvent I is calculated according to the mass ratio of solvent I:epichlorohydrin, which is 10-30:100. The above-mentioned etherification grafting reaction time is 3 to 8 hours, and the reaction efficiency of the etherification grafting reaction of the 4-amino-3-methylphenol monomer can reach up to 98.9%. The higher the reaction efficiency of the etherification grafting reaction of the 4-amino-3-methylphenol monomer, the higher the conversion efficiency of the amino active hydrogen, which indicates that the preparation method of the triglycidyl 4-amino-3-methylphenol epoxy resin of the present application has a high conversion efficiency of the amino active hydrogen; Taking production efficiency into consideration, the reaction efficiency of the etherification grafting reaction of 4-amino-3-methylphenol monomer reaches 86.0-98.5% preferably within 3-6 hours; More preferably, when the reaction time is 4 to 6 hours, the conversion efficiency of the 4-amino-3-methylphenol monomer and the etherification grafting reaction efficiency of the 4-amino-3-methylphenol monomer can reach 95.0 to 98.5%; (2) Closed-loop reaction Controlling the negative pressure at 0.07-0.09 MPa and the temperature at 30-50° C., adding a sodium hydroxide aqueous solution to the reaction solution containing 4-amino-3-methylphenol chlorohydrin ether obtained in step (1), and then continuing to maintain the negative pressure at 0.07-0.09 MPa and the temperature at 30-50° C. to carry out a ring-closing reaction for 2-3 hours to obtain a reaction solution I containing triglycidyl 4-amino-3-methylphenol epoxy resin; the reaction solution I contains, in addition to the triglycidyl 4-amino-3-methylphenol epoxy resin, sodium chloride, unreacted epichlorohydrin, solvent I and by-products; The sodium hydroxide aqueous solution has a mass percentage concentration of 40 to 50%; The amount of the sodium hydroxide aqueous solution is calculated in molar ratio of 4-amino-3-methylphenol used in step (1) to sodium hydroxide in the sodium hydroxide aqueous solution used in the ring-closing reaction in the ratio of 1:2.0 to 2.7; The addition rate of the sodium hydroxide aqueous solution is controlled to be 1.25-2.25 g / min, that is, the mass of the sodium hydroxide aqueous solution added per minute is 1.25-2.25 g; If the catalyst in step (1) contains a potassium hydroxide aqueous solution, the sodium hydroxide aqueous solution used in the ring-closing reaction is replaced by a potassium hydroxide aqueous solution; In the above-mentioned closed-loop reaction, the amount and rate of sodium hydroxide solution added are controlled to ensure that the easily saponifiable chlorine after the closed-loop reaction is controlled within a reasonable level range. Combined with the following step (4), the refining reaction process controls the appropriate temperature and time of the refining reaction, and finally a triglycidyl 4-amino-3-methylphenol epoxy resin product with higher monomer purity and lower epoxy equivalent can be obtained. Analysis shows that the reason may be that the rate of addition of sodium hydroxide solution during the closed-loop reaction is too fast, which will cause a violent reaction, increase side reactions and thus affect the purity of the final resin product, while the addition rate is too slow, which will affect the production efficiency; in addition, too much sodium hydroxide solution added during the closed-loop reaction will cause the easily saponifiable chlorine to drop too low, and at the end of the refining reaction, it will cause the subsequent three wastes to increase and difficult to handle. If the amount of sodium hydroxide solution added is too little, the easily saponifiable chlorine content will be too high, which will lead to excessive use of sodium hydroxide solution in the refining reaction, resulting in increased costs; The above-mentioned ring-closing reaction is carried out under negative pressure, mainly to improve the utilization efficiency of the sodium hydroxide aqueous solution in the ring-closing reaction, reduce the waste of raw materials caused by hydrolysis of the raw material epichlorohydrin, and affect the quality of the final product triglycidyl 4-amino-3-methylphenol epoxy resin; Preferably, when the reaction temperature of the ring-closing reaction is 30-45° C., especially when the temperature is 40° C., the final triglycidyl 4-amino-3-methylphenol epoxy resin obtained under the same refining reaction conditions and the same purification conditions in the subsequent preparation process has a higher purity, and the purity can reach 92.1%; 1. After the ring-closing reaction in step (2) is completed, the pressure is adjusted to a negative pressure of 0.098 MPa, and the temperature is raised to 80-125° C. to remove solvent I and excess unreacted epichlorohydrin. When the amounts of unreacted epichlorohydrin and solvent I are both less than 500 ppm, solvent II is added and mixed uniformly to obtain a reaction solution II containing triglycidyl 4-amino-3-methylphenol epoxy resin; the reaction solution II contains, in addition to triglycidyl 4-amino-3-methylphenol epoxy resin, solvent II, sodium chloride, by-products, less than 500 ppm of epichlorohydrin and solvent I; The removal of the unreacted epichlorohydrin and solvent I can be detected by gas chromatography to determine the residual amounts of epichlorohydrin and solvent I in the reaction solution after the removal. The solvent II is at least one of toluene, xylene, butanone, and methyl isobutyl ketone; the solvent II in the present application is only toluene as an example, but the use of other solvents in the solvent II is not limited; The amount of solvent II added is calculated according to the mass ratio of solvent II to the theoretically obtained triglycidyl 4-amino-3-methylphenol epoxy resin, that is, the amount of solvent II added is 1 to 2.75 times the mass of the theoretically obtained triglycidyl 4-amino-3-methylphenol epoxy resin; The amount of triglycidyl 4-amino-3-methylphenol epoxy resin that should be obtained theoretically is calculated based on the reaction efficiency of the etherification grafting reaction of 4-amino-3-methylphenol used in step (1) being 100%, and the amount of triglycidyl 4-amino-3-methylphenol epoxy resin obtained under the condition that the ring-closing reaction is thorough; In each embodiment of the present application, only toluene is used as an example of solvent II, but the use of xylene, butanone, and methyl isobutyl ketone is not limited; (4) Refining reaction Since the molar ratio of the sodium hydroxide aqueous solution added in step (1) and step (2) to the 4-amino-3-methylphenol chlorohydrin ether is less than 3:1, a small amount of 4-amino-3-methylphenol chlorohydrin ether (the chlorine in the structure is called easily saponifiable chlorine) will remain and further ring closure is required to further improve the purity of the 4-amino-3-methylphenol epoxy resin; Adding a sodium hydroxide aqueous solution having a mass percentage concentration of 40 to 50% to the reaction solution II containing the triglycidyl 4-amino-3-methylphenol epoxy resin obtained in step (3) to carry out a refining reaction, wherein the refining reaction process is controlled at a temperature of 60 to 100° C. and a time of 2 to 9 hours to obtain a reaction solution after the refining reaction; the reaction solution after the refining reaction contains, in addition to the triglycidyl 4-amino-3-methylphenol epoxy resin, sodium chloride, solvent II (toluene) and a sodium hydroxide aqueous solution, etc.; The amount of the sodium hydroxide aqueous solution having a mass percentage concentration of 40 to 50% is 2 to 4 times the molar number of easily saponifiable chlorine in the triglycidyl 4-amino-3-methylphenol epoxy resin that should be obtained theoretically. The amount of the triglycidyl 4-amino-3-methylphenol epoxy resin that should be obtained theoretically is calculated based on the reaction efficiency of the etherification grafting reaction of 4-amino-3-methylphenol used in step (1) being 100%, and the amount of the triglycidyl 4-amino-3-methylphenol epoxy resin obtained under the condition that the ring-closing reaction is thorough; In the above-mentioned refining reaction process, if the reaction temperature is too high, the reaction process will be too fast, some aged resins will be produced, and the separation effect will be poor in the subsequent further purification process, and the purity of the final product triglycidyl 4-amino-3-methylphenol epoxy resin will also be reduced; and if the reaction temperature is too low, the reaction process will be too slow. Under the same refining reaction time, the final product triglycidyl 4-amino-3-methylphenol epoxy resin will have a high content of easily saponifiable chlorine; During the refining reaction, a too long reaction time will affect the production efficiency; while a too short reaction time will result in a high residual amount of easily saponifiable chlorine, which will affect the quality of the final product, triglycidyl 4-amino-3-methylphenol epoxy resin; Taking into account the content of easily saponifiable chlorine in the final triglycidyl 4-amino-3-methylphenol epoxy resin and the liquid separation in the purification process after the refining reaction, it is preferred that the refining reaction process is controlled at a temperature of 70 to 85° C. and a time of 2 to 5 hours for the refining reaction. After the reaction liquid after the refining reaction is purified under the same purification conditions, the final triglycidyl 4-amino-3-methylphenol epoxy resin has a content of easily saponifiable chlorine distributed in 47 to 98 ppm, and the liquid separation effect in the subsequent purification process is better; (5) Purification ①, adding water to the reaction solution after the purification reaction obtained in the above step (4), stirring and mixing, and then standing to separate the layers to obtain an organic phase consisting of a brine phase and a resin / solvent II, removing the lower brine phase to remove the byproduct salt, that is, to remove sodium chloride, to obtain an organic phase consisting of a resin / solvent II; The amount of water added is 3 to 6 times the mass of the byproduct sodium chloride theoretically produced by the etherification grafting reaction in step (1). To save water and energy consumption, the amount of water added is preferably 3 to 4.5 times; ②, adding a pH regulator to the organic phase composed of the resin / solvent II obtained in ①, controlling the pH value of the organic phase composed of the resin / solvent II to 5-7, then standing the liquid for separation, removing the lower aqueous phase, and obtaining an organic phase composed of the resin / solvent II with a pH value of 5-7; The pH regulator is one of phosphoric acid, sodium hydrogen phosphate, hydrochloric acid and oxalic acid; ③. Add water to the organic phase composed of resin / solvent II with a pH value of 5 to 7 obtained in ② and wash 1 to 3 times until there is no sodium chloride in the effluent, thereby obtaining a crude product containing triglycidyl 4-amino-3-methylphenol epoxy resin and solvent II; ④. The crude product containing triglycidyl 4-amino-3-methylphenol epoxy resin and solvent II obtained in ③ is controlled to have a negative pressure of 0.0985-0.099 MPa and a temperature of 125-140° C. to evaporate and remove solvent II to obtain triglycidyl 4-amino-3-methylphenol epoxy resin.
[0013] By adopting the above technical scheme, a composite catalyst is used in the etherification grafting stage, especially a composite catalyst containing an alkali metal solution, and the addition amount and addition rate of the sodium hydroxide aqueous solution are controlled during the ring-closing reaction, and the ring-closing reaction is controlled within a reasonable pressure range, and the temperature and time of the refining reaction process are controlled at the same time. The synergistic effect of the means such as the deterioration of the activity of the 4-amino-3-methylphenol monomer due to the addition of methyl groups and the incomplete reaction of the active hydrogen of the amino group are effectively overcome, and the reaction efficiency of the etherification grafting reaction between the active groups in the 4-amino-3-methylphenol monomer and epichlorohydrin is greatly improved, thereby improving the final The yield of triglycidyl 4-amino-3-methylphenol epoxy resin in the product can reach 98.7%, and the purity of triglycidyl 4-amino-3-methylphenol epoxy resin in the final product is also improved. In particular, when a catalyst composed of an alkali metal solution and a quaternary ammonium salt is used, especially a catalyst composed of an aqueous NaOH solution and dodecyltrimethylammonium chloride, it is tested that the purity of the triglycidyl 4-amino-3-methylphenol epoxy resin obtained above can reach up to 92.1%, meeting the requirement of being directly used in electronic equipment or aerospace materials, that is, no further purification is required.
[0014] Furthermore, in the preparation process, due to the use of the composite catalyst, the etherification grafting reaction temperature is controlled to be 30-55° C., and the reaction time is 3-6 hours, and the reaction efficiency of the etherification grafting reaction is 86.0-98.5%. In particular, when the etherification grafting reaction time is 4-6 hours, the reaction efficiency of the etherification grafting reaction is 95.0-98.5%, and the yield of the product is also the highest, ranging from 98.1-98.7%.
[0015] Furthermore, the sodium hydroxide aqueous solution in the composite catalyst used in the etherification grafting reaction in the preparation process is added in batches, especially in 4 batches, the reaction efficiency of the 4-amino-3-methylphenol monomer in the etherification grafting reaction is better, so that the purity of the final product is higher, which can reach 92.1%. Analysis shows that the reason may be that the addition is made every 30 minutes, which makes the fluctuation range of the temperature change in the system smaller, which is more conducive to the smooth progress of the etherification grafting reaction.
[0016] Furthermore, when the amount of sodium hydroxide aqueous solution used in the composite catalyst for the etherification grafting reaction in the preparation process is such that the molar ratio of 4-amino-3-methylphenol to sodium hydroxide in the sodium hydroxide aqueous solution is 1:0.53, the liquid separation condition in the purification stage of the preparation process is good, and the product purity is higher, reaching 92.1%.
[0017] Furthermore, in the closed-loop reaction of the preparation process, the addition amount and the addition rate of the sodium hydroxide aqueous solution are controlled, and the temperature of the refining reaction is controlled at 70-85° C. for 2-5 hours, which can ensure that the easily saponifiable chlorine after the refining reaction is controlled at 47-98 ppm. After further treatment, a triglycidyl 4-amino-3-methylphenol epoxy resin product with a purity of 90.0-92.1% and an epoxy equivalent of 105-116 g / eq is obtained.
[0018] Furthermore, the storage stability and high temperature stability of a triglycidyl 4-amino-3-methylphenol epoxy resin finally obtained by the above preparation method are as follows: At 15-30° C. and air humidity RH of 40-85%, the triglycidyl 4-amino-3-methylphenol epoxy resin is stored for 11-15 months, and the GPC spectrum distribution does not change, and the viscosity change rate at 25° C. is less than 10%, which indicates that the triglycidyl 4-amino-3-methylphenol epoxy resin has good storage stability; At the same time, the triglycidyl 4-amino-3-methylphenol epoxy resin was controlled to be baked at 190°C for 3 hours, and its purity was only reduced by 3% (from 92.1% to 89.1%), and the viscosity increase rate was 4%; relative to the commercially available triglycidyl p-aminophenol epoxy resin, its purity was reduced by 16% (from 72% to 56%) under the same conditions, and the viscosity increase rate was 34%; thus, it is shown that the triglycidyl 4-amino-3-methylphenol epoxy resin obtained by the preparation method of the present application has good high temperature stability and can withstand the influence of high environmental temperature on product performance. Therefore, the triglycidyl 4-amino-3-methylphenol epoxy resin obtained by the preparation method of the present application has relatively low requirements for storage environment temperature or temperature changes, which can also further prove that the triglycidyl 4-amino-3-methylphenol epoxy resin obtained by the preparation method of the present application has a technical effect of a long storage period.
[0019] In a third aspect, the present application provides an adhesive containing the above-mentioned triglycidyl 4-amino-3-methylphenol epoxy resin, and the specific technical scheme is as follows: An adhesive containing triglycidyl 4-amino-3-methylphenol epoxy resin, wherein the raw material composition and content thereof are, calculated by weight, 100 parts of triglycidyl 4-amino-3-methylphenol epoxy resin, 100-150 parts of curing agent, and 0.1-0.6 parts of accelerator, respectively; The curing agent is an acid anhydride curing agent, and the acid anhydride curing agent is one or more of methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, hexahydrophthalic anhydride, tetrahydrophthalic anhydride and methylnadic anhydride; The above-mentioned accelerator is imidazole, benzyldimethylamine, 2,4,6-tris(dimethylaminomethyl)phenol or o-hydroxybenzyldimethylamine; in this application, only methyltetrahydrophthalic anhydride as the curing agent and benzyldimethylamine as the accelerator are used as examples, and the use of the above-mentioned other curing agents and other accelerators in the adhesive containing triglycidyl 4-amino-3-methylphenol epoxy resin is not limited; The raw materials used in the above-mentioned adhesive containing triglycidyl 4-amino-3-methylphenol epoxy resin are stored separately, mixed when used, and then cured; The preparation method of the above-mentioned adhesive containing triglycidyl 4-amino-3-methylphenol epoxy resin comprises the following specific steps: First, add the above-mentioned triglycidyl 4-amino-3-methylphenol epoxy resin, curing agent and accelerator into a container in sequence, control the temperature at 20±2°C and stir and mix evenly to obtain an adhesive containing triglycidyl 4-amino-3-methylphenol epoxy resin.
[0020] The Tg, impact strength, flexural strength, tensile strength and hydrophobicity of the above-obtained adhesive containing triglycidyl 4-amino-3-methylphenol epoxy resin after curing are as follows: The curing is to control the temperature of the adhesive containing triglycidyl 4-amino-3-methylphenol epoxy resin to be 120° C. for curing for 2 hours and 160° C. for curing for 2 hours.
[0021] The Tg value after curing is 245-250°C, which shows that it has good high temperature resistance; Impact strength after curing: 25~46KJ / m 2 , bending strength 178 ~ 198MPa, tensile strength 70 ~ 80MPa, which shows that it has good anti-deformation performance; The water absorption after curing is ≤0.1%, which indicates that it has good hydrophobic properties; In summary, the adhesive containing triglycidyl 4-amino-3-methylphenol epoxy resin of the present application, after being cured using methyltetrahydrophthalic anhydride as a curing agent, not only has good Tg and anti-deformation properties, but also has better hydrophobic properties, and can be widely used in electronic equipment, automobiles and other product fields.
[0022] Beneficial technical effects of this application Compared with the existing technology, the beneficial technical effects of the technical solution of this application are as follows: The present invention discloses a method for preparing triglycidyl 4-amino-3-methylphenol epoxy resin. In the etherification grafting stage, two composite catalysts are preferably used, especially alkali metal solution and quaternary ammonium salt are composited, more especially sodium hydroxide aqueous solution and dodecyltrimethylammonium chloride are composited, especially when the alkali metal solution is added in batches, and the reaction efficiency of the etherification grafting reaction of 4-amino-3-methylphenol monomer monitored by GPC can reach more than 95.0%, up to 98.9%, and the yield of the final product can reach up to 98.7% under the synergistic effect of reasonable sodium hydroxide aqueous solution feeding amount and feeding rate, the temperature of the refining reaction process and other conditions in combination with the closed-loop reaction.
[0023] Furthermore, in the preparation method of a triglycidyl 4-amino-3-methylphenol epoxy resin of the present application, since the temperature of the etherification grafting reaction stage is 30 to 55° C., especially 40 to 50° C., the occurrence of side reactions is greatly reduced, and the number of by-products is reduced, so that the final finished product triglycidyl 4-amino-3-methylphenol epoxy resin has a higher purity. The purity of the final triglycidyl 4-amino-3-methylphenol epoxy resin can reach up to 92.1% through GPC monitoring, which can directly meet the use requirements of adhesives in electronic equipment, automobiles and other product fields, that is, it can be used directly without further purification, thereby reducing the energy consumption of the production process and relatively reducing the production cost.
[0024] Furthermore, the triglycidyl 4-amino-3-methylphenol epoxy resin obtained by the preparation method of a triglycidyl 4-amino-3-methylphenol epoxy resin in the present application contains a methyl group in the structure, so that the triglycidyl 4-amino-3-methylphenol epoxy resin has the same physical and chemical advantages as p-aminophenol epoxy resin or m-aminophenol epoxy resin, and also has better hydrophobic properties. The final triglycidyl 4-amino-3-methylphenol epoxy resin is cured with methyltetrahydrophthalic anhydride, and the Tg value is 245-250°C and the impact strength is 25-46KJ / m 2 , bending strength is 178~198MPa, tensile strength is 70~80MPa, and its water absorption rate is ≤0.1%.
[0025] Furthermore, the triglycidyl 4-amino-3-methylphenol epoxy resin obtained by the preparation method of a triglycidyl 4-amino-3-methylphenol epoxy resin of the present application has high purity and also has good high temperature stability and storage stability, and has relatively loose requirements on the storage environment temperature, and the storage period can reach 11 to 15 months without deterioration, while the storage period of the currently commercially available triglycidyl p-aminophenol epoxy resin or m-aminophenol epoxy resin is only half a year. DETAILED DESCRIPTION
[0026] The present application is further described in detail below in conjunction with specific embodiments, but the embodiments are not intended to limit the present application.
[0027] The raw materials used in each example of this application are as follows: The method for determining the performance index of the triglycidyl 4-amino-3-methylphenol epoxy resin product obtained in each embodiment of the present application is as follows: After the triglycidyl 4-amino-3-methylphenol epoxy resin is cured (curing method, methyltetrahydrophthalic anhydride is used as curing agent, benzyldimethylamine is used as accelerator; triglycidyl 4-amino-3-methylphenol epoxy resin, curing agent and accelerator are added to the container in sequence, stirred and mixed evenly at a constant temperature of 20±2°C, to obtain an adhesive containing triglycidyl 4-amino-3-methylphenol epoxy resin, and then the temperature is controlled to cure at 120°C for 2h and 160°C for 2h, and then Tg, strength, water absorption and other data can be tested): Method for determining Tg value: Detection is carried out by DSC method, as follows: 5 to 10 mg of the solidified material is weighed and placed in an aluminum crucible, and the heating rate is 10°C / min. After heating to 300°C, the temperature is lowered to 25°C at a rate of 20°C / min to eliminate the thermal history, and the temperature is again raised to 300°C at a program temperature of 10°C / min, and the glass transition temperature (Tg) is read.
[0028] The test method for impact strength is in accordance with GB / T 2567-2008; The test method for flexural strength is in accordance with GB / T 2567-2008; The test method for tensile strength is as follows: GB / T 2567-2008; The test method of water absorption rate of hydrophobic performance is as follows: the temperature is 85℃, the air RH humidity is 85%, and it is placed for 1000 hours. The weight difference before and after the test is large, the hydrophobic performance is poor, and the difference is small, the hydrophobic performance is good; Triglycidyl 4-amino-3-methylphenol epoxy resin: Purity determination method: characterized by gel permeation chromatography (GPC), according to GB / T 27843-2011, the name of the instrument used for determination is Waters high performance liquid chromatography, model Waters 1515; Determination method of epoxy equivalent: GB / T 4612-2008, instrument model: METTLER TOLEDO; Determination method of easily saponifiable chlorine: according to GB / T 4618.2-2008; The method for determining high temperature stability is as follows: The triglycidyl 4-amino-3-methylphenol epoxy resin was baked in an oven at 190°C for 3 hours, and the change in purity before and after baking was tested. Viscosity determination method: According to GB / T 10247-2008, a digital viscosity display meter (model: Brookfield DV2RT, USA) was used to test the viscosity at 25°C; Method for determining storage stability of triglycidyl 4-amino-3-methylphenol epoxy resin: By measuring the viscosity data of triglycidyl 4-amino-3-methylphenol epoxy resin just obtained after preparation and after storage at room temperature of 25°C, the time when the viscosity starts to increase is recorded as the storage period.
[0029] The reaction efficiency of the grafting reaction of the etherification section of 4-amino-3-methylphenol in the preparation process was determined by gel permeation chromatography (GPC). The instrument used for the determination was Waters high performance liquid chromatography, model Waters1515.
[0030] The calculation formula of the yield of triglycidyl 4-amino-3-methylphenol epoxy resin is as follows: Yield = actually obtained mass of triglycidyl 4-amino-3-methylphenol epoxy resin / theoretically produced mass of triglycidyl 4-amino-3-methylphenol epoxy resin × 100%.
[0031] Example 1 A triglycidyl 4-amino-3-methylphenol epoxy resin, the structural formula of which is shown below: The above-mentioned triglycidyl 4-amino-3-methylphenol epoxy resin is prepared by a method comprising the following steps: 1. Etherification grafting reaction In the four-mouthful round-bottomed flask of the 2000ml that agitator, mercury thermometer, nitrogen access tube, condenser tube and glass oil-water separator are housed, add 1124g epichlorohydrin successively, 337g solvent I, 166.7g 4-amino-3-methylphenol (theoretically should obtain the triglycidyl 4-amino-3-methylphenol epoxy resin of 388g), be warming up to 50 ℃ and keep 30min to dissolve 4-amino-3-methylphenol, then add the catalyst of 61g (adding for 4 times, each time at intervals of 30 minutes), then control the temperature to be 50 ℃ and carry out etherification grafting reaction 5h (starting timing from adding catalyst for the first time), obtain the reaction solution containing 4-amino-3-methylphenol chlorohydrin ether (product A); The above-mentioned 4-amino-3-methylphenol: epichlorohydrin: catalyst usage, calculated by molar ratio, 4-amino-3-methylphenol: epichlorohydrin: catalyst is 1:9:0.54; The 61g catalyst is compounded by 2g of dodecyltrimethylammonium chloride and 59g of a sodium hydroxide aqueous solution with a mass percentage concentration of 48.5%, that is, the amount of dodecyltrimethylammonium chloride and the sodium hydroxide aqueous solution with a mass percentage concentration of 48.5% is calculated according to the mass ratio of dodecyltrimethylammonium chloride: sodium hydroxide aqueous solution with a mass percentage concentration of 48.5% as 1:29.5; The above-mentioned 4-amino-3-methylphenol: sodium hydroxide in the catalyst is calculated by molar ratio, 4-amino-3-methylphenol: sodium hydroxide in the catalyst is 1:0.53; The solvent I is isopropanol; the amount added is calculated according to the mass ratio of solvent I:epichlorohydrin, which is 30:100; (2) Closed-loop reaction The reaction solution containing 4-amino-3-methylphenol chlorohydrin ether (product A) obtained in step (1) is adjusted to a pressure of negative pressure 0.089 MPa and a temperature of 40° C., and 247 g of a sodium hydroxide aqueous solution having a mass percent concentration of 48.5% is added within 2.5 h, i.e., the addition rate of the sodium hydroxide aqueous solution having a mass percent concentration of 48.5% is controlled to be 1.65 g / min, and then the pressure is continued to be maintained at a negative pressure of 0.089 MPa and a temperature of 50° C. for reaction for 1 h, to obtain a reaction solution I containing triglycidyl 4-amino-3-methylphenol epoxy resin; The amount of the sodium hydroxide aqueous solution with a mass percentage concentration of 48.5% is added in a molar ratio of 4-amino-3-methylphenol to the sodium hydroxide in the sodium hydroxide aqueous solution with a mass percentage concentration of 48.5% of 1:2.2; (3) Add 686 ml of solvent II toluene to the reaction solution I containing triglycidyl 4-amino-3-methylphenol epoxy resin obtained in step (2), stir and dissolve, then adjust the pressure to a negative pressure of 0.098 MPa and maintain the temperature at 120° C. for 2 hours to remove epichlorohydrin and solvent I, thereby obtaining a reaction solution II containing triglycidyl 4-amino-3-methylphenol epoxy resin; the solvent II is toluene, and the amount of toluene added is based on the mass ratio of toluene to the amount of 4-amino-3-methylphenol used in step (1) to obtain the triglycidyl 4-amino-3-methylphenol epoxy resin of 152:100; (4) Refining reaction Add 35 g of a sodium hydroxide aqueous solution having a mass percentage concentration of 48.5% to the reaction solution II containing the triglycidyl 4-amino-3-methylphenol epoxy resin obtained in step (3), control the temperature to 80° C. for a refining reaction for 2 h, and obtain a reaction solution after a refining reaction, which contains, in addition to the triglycidyl 4-amino-3-methylphenol epoxy resin, sodium chloride, solvent II (toluene), and a sodium hydroxide aqueous solution; The amount of the sodium hydroxide aqueous solution with a mass percentage concentration of 40-50% is 2.5 times the molar number of easily saponifiable chlorine in the theoretical triglycidyl 4-amino-3-methylphenol epoxy resin; (5) Purification ①, add 650 ml of water to the refined reaction solution obtained in step (4), mix well, and then let it stand for 30 minutes to separate the layers, to obtain an organic phase consisting of a brine phase and a resin / solvent II, remove the lower brine phase, and obtain an organic phase consisting of a resin / solvent II; ②, add 5% by mass oxalic acid aqueous solution to the organic phase composed of the resin / solvent II obtained in ① to adjust the pH value to 6, then remove the aqueous phase by layer to obtain an organic phase composed of the resin / solvent II with a pH value of 6; ③. Add water to the organic phase composed of resin / solvent II with a pH of 6 obtained in ② for washing, 50 ml of water is added each time, and there is no sodium chloride in the effluent of the washing value, to obtain a crude product containing triglycidyl 4-amino-3-methylphenol epoxy resin and solvent II; ④. Control the pressure to be negative pressure 0.0985-0.0995 MPa and the temperature to be 125-140°C, and vacuum-desolventize the crude product containing triglycidyl 4-amino-3-methylphenol epoxy resin and solvent II obtained in ③ to obtain the finished product of triglycidyl 4-amino-3-methylphenol epoxy resin.
[0032] The product obtained after vacuum removal of solvent II in the purification step ④ of the above step (5) was subjected to nuclear magnetic hydrogen spectrum measurement, and the data results of the measurement are as follows: ( 1H NMR, 400 MHz, CDCl3): 7.16-7.08 (dd, 1H, J = 7.6 Hz, 2 Hz, benzene ring hydrogen), 6.80-6.76 (d, 1H, J = 2 Hz, benzene ring hydrogen), 6.76-6.70 (dd, 1H, J = 7.6 Hz, 2 Hz, benzene ring hydrogen), 4.20-4.16 (dd, 1H, J = 8.4 Hz, 2.4 Hz), 3.94-3.90 (dd, 1H, J = 8.8Hz, 4.8Hz), 3.36-3.30 (m, 1H), 3.24-3.00 (m, 6H), 2.92-2.88 (t, 1H, J = 3.6H z), 2.76-2.72 (m, 1H), 2.70-2.66 (m, 2H), 2.45-2.42 (m, 2H), 2.36-2.32 (d, 3H, J = 3.6Hz).
[0033] It can be concluded from the above H NMR spectrum data that the product obtained after removing the solvent II toluene in the purification step ④ of step (5) of the above preparation process is triglycidyl 4-amino-3-methylphenol epoxy resin.
[0034] It has been determined that the reaction efficiency of the etherification grafting reaction of 4-amino-3-methylphenol in step (1) is 98.5%, the purity of the obtained triglycidyl 4-amino-3-methylphenol epoxy resin product is 92.1%, the viscosity is 813 cps / 25°C, and the storage period is 15 months when stored at 25°C and an air RH humidity of 75%, so the product has good storage stability.
[0035] The above triglycidyl 4-amino-3-methylphenol epoxy resin was baked at a temperature of 190° C. for 3 hours, and the purity was only reduced by 3% (from 92.1% to 89.1%). This shows that the triglycidyl 4-amino-3-methylphenol epoxy resin of the present application has good high temperature stability and can withstand the influence of high environmental temperature on product performance.
[0036] The above triglycidyl 4-amino-3-methylphenol epoxy resin, when combined with a curing agent and an accelerator, has a Tg value of 248°C and an impact strength of 40KJ / m after curing. 2 , the flexural strength is 189MPa, the tensile strength is 74MPa, and the water absorption rate is only 0.08%.
[0037] Example 2 A triglycidyl 4-amino-3-methylphenol epoxy resin, the preparation process of which is the same as that of Example 1, except that the catalyst I is dodecyltrimethylammonium chloride.
[0038] It was determined that the reaction efficiency of the etherification grafting reaction of 4-amino-3-methylphenol in step (1) of the preparation process was 82%, the purity of the obtained triglycidyl 4-amino-3-methylphenol epoxy resin was 86.0%, the viscosity was 854 cps / 25°C, and after curing, the Tg value was 238°C and the impact strength was 31 KJ / m 2 , the flexural strength is 185MPa, the tensile strength is 71MPa, and the water absorption is 0.09%.
[0039] The obtained triglycidyl 4-amino-3-methylphenol epoxy resin can be stored for 13 months at 25° C. and 75% RH.
[0040] Example 3 A triglycidyl 4-amino-3-methylphenol epoxy resin, the preparation process of which is the same as that of Example 1, except that the catalyst I is a sodium hydroxide aqueous solution with a mass percentage concentration of 48.5%.
[0041] The reaction efficiency of the etherification grafting reaction of 4-amino-3-methylphenol in step (1) of the preparation process was determined to be 75%. The purity of the obtained triglycidyl 4-amino-3-methylphenol epoxy resin was 82.0%, the viscosity was 892cps / 25°C, and after curing, the Tg value was 233°C and the impact strength was 24KJ / m 2 , the flexural strength is 181MPa, the tensile strength is 71MPa, and the water absorption is 0.1%.
[0042] The obtained triglycidyl 4-amino-3-methylphenol epoxy resin can be stored for 13 months without deterioration at 25° C. and 75% air RH humidity, and thus has good storage stability.
[0043] By comparing the above-mentioned Example 1, Example 2 and Example 3, it can be seen that the catalyst composed of two components in the etherification grafting reaction process can make the three active groups (two active hydrogens of amino group and one active hydrogen of hydroxyl group) in 4-amino-3-methylphenol monomer have a higher reaction efficiency of etherification grafting reaction with epichlorohydrin, which can reach 98.5% through GPC monitoring, while the reaction efficiency of the catalyst of the single component is only 75-82%. The reason for this may be that the catalyst after the two components are combined can effectively overcome the influence of the monomer reaction activity of 4-amino-3-methylphenol monomer due to the presence of methyl group, thereby greatly improving the reaction efficiency of the grafting reaction of the three active groups (two active hydrogens of amino group and one active hydrogen of hydroxyl group) in 4-amino-3-methylphenol monomer with epichlorohydrin.
[0044] Furthermore, by comparing the purity of the triglycidyl 4-amino-3-methylphenol epoxy resin obtained in the above-mentioned Example 1, Example 2, and Example 3, it can be seen that the purity of the triglycidyl 4-amino-3-methylphenol epoxy resin product finally obtained by using a catalyst composed of two components in the etherification grafting reaction is also higher, which can reach 92.1% through GPC monitoring, and the Tg value after curing is higher. However, the purity of the catalyst using a single component is only 82.0-86.0%, and the Tg value after curing will also be reduced.
[0045] Example 4 A triglycidyl 4-amino-3-methylphenol epoxy resin, the preparation process of which is the same as that of Example 1, except that the temperature of the etherification grafting reaction in step (1) is controlled to be 55°C.
[0046] It was determined that the reaction efficiency of the etherification grafting reaction of 4-amino-3-methylphenol in step (1) of the preparation process was 98.5%, the purity of the obtained triglycidyl 4-amino-3-methylphenol epoxy resin was 90.2%, and the Tg value after curing was 242°C.
[0047] Example 5 A triglycidyl 4-amino-3-methylphenol epoxy resin, the preparation process of which is the same as that of Example 1, except that the temperature of the etherification grafting reaction in step (1) is controlled to be 60°C.
[0048] It was determined that the reaction efficiency of the etherification grafting reaction of 4-amino-3-methylphenol in step (1) of the preparation process was 98.6%, the purity of the triglycidyl 4-amino-3-methylphenol epoxy resin finally obtained was 85.1%, and the Tg value after curing was 238°C.
[0049] Example 6 A triglycidyl 4-amino-3-methylphenol epoxy resin, the preparation process of which is the same as that of Example 1, except that the temperature of the etherification grafting reaction in the preparation step (1) is controlled to be 65°C.
[0050] It was determined that the reaction efficiency of the etherification grafting reaction of 4-amino-3-methylphenol was 98.5%, the purity of the finally obtained triglycidyl 4-amino-3-methylphenol epoxy resin was 82.0%, and the Tg value after curing was 236°C.
[0051] Example 7 A triglycidyl 4-amino-3-methylphenol epoxy resin, the preparation process of which is the same as that of Example 1, except that the temperature of the etherification grafting reaction in step (1) is controlled to be 70°C.
[0052] It was determined that the reaction efficiency of the etherification grafting reaction of 4-amino-3-methylphenol in step (1) of the preparation process was 98.6%, the purity of the triglycidyl 4-amino-3-methylphenol epoxy resin finally obtained was 79.1%, and the Tg value after curing was 234°C.
[0053] Example 8 A triglycidyl 4-amino-3-methylphenol epoxy resin, the preparation process of which is the same as that of Example 1, except that the temperature of the etherification grafting reaction in the preparation step (1) is controlled to be 30°C.
[0054] It was determined that the reaction efficiency of the etherification grafting reaction of 4-amino-3-methylphenol in step (1) of the preparation process was 91.0%, the purity of the obtained triglycidyl 4-amino-3-methylphenol epoxy resin was 88.0%, and the Tg value after curing was 240°C.
[0055] Example 9 A triglycidyl 4-amino-3-methylphenol epoxy resin, the preparation process of which is the same as that of Example 3, except that the temperature of the etherification grafting reaction in the preparation step (1) is controlled to be 40°C.
[0056] The reaction efficiency of the etherification grafting reaction of 4-amino-3-methylphenol was determined to be 95%, the purity of the obtained triglycidyl 4-amino-3-methylphenol epoxy resin was 90.7%, and the Tg value after curing was 245°C.
[0057] The epoxy equivalent values of the triglycidyl 4-amino-3-methylphenol epoxy resins obtained in Examples 1, 4 to 9 above were tested, and the results are shown in the following table: In the above-mentioned Examples 1, 4 to 9, when the temperature of the etherification grafting reaction process in step (1) of the preparation process is controlled at 50, 55, 60, 65, 70, 30, and 40°C, respectively, it can be seen from the purity, epoxy equivalent, and Tg data of the obtained triglycidyl 4-amino-3-methylphenol epoxy resin product that the temperature of the etherification grafting reaction process is preferably controlled at 30 to 55°C, more preferably 40-55°C. The reason for this may be that when the reaction process is controlled at a lower temperature, the occurrence of side reactions caused by high temperature can be avoided, thereby causing the purity of the final triglycidyl 4-amino-3-methylphenol epoxy resin product to decrease, that is, the epoxy equivalent to increase.
[0058] Example 10 A triglycidyl 4-amino-3-methylphenol epoxy resin, the preparation process of which is the same as that of Example 1, except that: a sodium hydroxide aqueous solution having a mass percentage of 48.5% in the composite catalyst used in the etherification grafting reaction of the preparation step (1) is added in 5 portions, once every 30 minutes of reaction.
[0059] It was determined that the reaction efficiency of the etherification grafting reaction of 4-amino-3-methylphenol in step (1) of the preparation process was 97.9%; the purity of the obtained triglycidyl 4-amino-3-methylphenol epoxy resin was 91.3%, the Tg value after curing was 245°C, and the impact strength was 36KJ / m 2 , flexural strength is 181MPa, tensile strength is 70MPa, and water absorption is 0.09%. The obtained triglycidyl 4-amino-3-methylphenol epoxy resin can be stored for 14 months at 25°C and air RH humidity of 75%.
[0060] Embodiment 11 A triglycidyl 4-amino-3-methylphenol epoxy resin, the preparation process of which is the same as that of Example 1, except that: a sodium hydroxide aqueous solution having a mass percentage of 48.5% of the composite catalyst used in the etherification grafting reaction of the preparation step (1) is added in three portions, once every 30 minutes of reaction.
[0061] It was determined that the reaction efficiency of the etherification grafting reaction of 4-amino-3-methylphenol in step (1) of the preparation process was 97.2%; the purity of the obtained triglycidyl 4-amino-3-methylphenol epoxy resin was 90.8%, the Tg value after curing was 244°C, and the impact strength was 35KJ / m 2 , flexural strength is 180MPa, tensile strength is 71MPa, and water absorption is 0.09%; the obtained triglycidyl 4-amino-3-methylphenol epoxy resin can be stored for 14 months at 25°C and air RH humidity of 75%.
[0062] Example 12 A triglycidyl 4-amino-3-methylphenol epoxy resin, a triglycidyl 4-amino-3-methylphenol epoxy resin, the preparation process of which is the same as that of Example 1, except that: The sodium hydroxide aqueous solution with a mass percentage of 48.5% of the composite catalyst used in the etherification grafting reaction of the preparation step (1) is added in two portions, once every 30 minutes of reaction.
[0063] It was determined that the reaction efficiency of the etherification grafting reaction of 4-amino-3-methylphenol in step (1) of the preparation process was 95.2%; the purity of the obtained triglycidyl 4-amino-3-methylphenol epoxy resin was 89.0%, the Tg value after curing was 242°C, and the impact strength was 33KJ / m 2 , flexural strength is 180MPa, tensile strength is 72MPa, and water absorption is 0.1%; the obtained triglycidyl 4-amino-3-methylphenol epoxy resin can be stored for 13 months at 25°C and air RH humidity of 75%.
[0064] In the above-mentioned Examples 1, 10 to 12, i.e., in the step (1) of the preparation process, the sodium hydroxide aqueous solution with a mass percentage of 48.5 in the catalyst formed by the composite of two components is added in 4, 5, 3 and 2 times, respectively, and added once every 30 minutes. By comparing the purity and Tg value of the triglycidyl 4-amino-3-methylphenol epoxy resin finally obtained in each Example, it can be seen that the purity and Tg value after curing when adding in 4 times are the best. The reason for this may be that adding in 4 times can not only improve the efficiency of the etherification grafting reaction, but also maintain a relatively stable temperature in the reaction system.
[0065] Embodiment 13 A triglycidyl 4-amino-3-methylphenol epoxy resin, the preparation process of which is the same as that of Example 1, except that the etherification grafting reaction in step (1) of the preparation process is controlled within 3 hours.
[0066] It has been determined that the reaction efficiency of the etherification grafting reaction of 4-amino-3-methylphenol in step (1) of the preparation process is 86.0%, and the yield of triglycidyl 4-amino-3-methylphenol epoxy resin is 95.5%; the obtained triglycidyl 4-amino-3-methylphenol epoxy resin can be stored for 12 months at 25° C. and air RH humidity of 75%.
[0067] Embodiment 14 A triglycidyl 4-amino-3-methylphenol epoxy resin, the preparation process of which is the same as that of Example 1, except that: The etherification grafting reaction in step (1) of the preparation process is controlled within 4 hours.
[0068] It has been determined that the reaction efficiency of the etherification grafting reaction of 4-amino-3-methylphenol in step (1) of the preparation process is 95.0%, and the yield of triglycidyl 4-amino-3-methylphenol epoxy resin is 98.1%; the obtained triglycidyl 4-amino-3-methylphenol epoxy resin can be stored for 13 months at 25° C. and an air RH humidity of 75%.
[0069] Embodiment 15 A triglycidyl 4-amino-3-methylphenol epoxy resin, the preparation process of which is the same as that of Example 1, except that: The etherification grafting reaction in step (1) of the preparation process is controlled within 6 hours.
[0070] The reaction efficiency of the etherification grafting reaction of 4-amino-3-methylphenol was determined to be 98.6%, and the yield of triglycidyl 4-amino-3-methylphenol epoxy resin was 98.0%; the obtained triglycidyl 4-amino-3-methylphenol epoxy resin could be stored for 14 months at 25° C. and an air RH humidity of 75%.
[0071] Example 16 A triglycidyl 4-amino-3-methylphenol epoxy resin, the preparation process of which is the same as that of Example 1, except that: The etherification grafting reaction in step (1) of the preparation process is controlled within 8 hours.
[0072] It has been determined that the reaction efficiency of the etherification grafting reaction of 4-amino-3-methylphenol in step (1) of the preparation process is 98.9%, and the yield of triglycidyl 4-amino-3-methylphenol epoxy resin is 96.5%; the obtained triglycidyl 4-amino-3-methylphenol epoxy resin can be stored for 12.8 months at 25° C. and air RH humidity of 75%.
[0073] The following table summarizes the reaction efficiency of the etherification grafting reaction, the yield of the obtained triglycidyl 4-amino-3-methylphenol epoxy resin and the storage time at 25° C. and air RH humidity of 75% under different etherification grafting reaction times in the above-mentioned Examples 1 and 13 to 16: It can be seen from the above table that when the time of the etherification grafting reaction is preferably 3 to 6 hours, the reaction efficiency of the etherification grafting reaction is 86.0 to 98.5%.
[0074] In order to take into account the production efficiency, the etherification grafting reaction time is preferably 4 to 6 hours, and the reaction efficiency of the etherification grafting reaction is 95.0 to 98.5%. At the same time, the yield of the product is also the highest, ranging from 98.1 to 98.7%.
[0075] The triglycidyl 4-amino-3-methylphenol epoxy resin finally obtained in the above-mentioned Examples 13 to 16 can be stored for 12, 13, 14, and 12.8 months at 25° C. and an air RH humidity of 75%, according to tests.
[0076] Embodiments 17 to 19 A triglycidyl 4-amino-3-methylphenol epoxy resin, the preparation process of which is the same as that of Example 1, except that: the amount of catalyst used in the etherification grafting reaction process in step (1) is different, that is, when the amounts of 4-amino-3-methylphenol and epichlorohydrin are the same as those in Example 1, the amount of catalyst used in Examples 17 to 19 is calculated according to the molar ratio of 4-amino-3-methylphenol:epichlorohydrin:catalyst (the ratio of dodecyltrimethylammonium chloride and sodium hydroxide aqueous solution with a mass percentage concentration of 48.5% in the catalyst is the same as that in Example 1) as shown in the following table: At the same time, the reaction efficiency of the etherification grafting reaction of 4-amino-3-methylphenol in step (1) of the preparation process, the purity and yield of the finally obtained triglycidyl 4-amino-3-methylphenol epoxy resin, and the storage time at 25° C. and air RH humidity of 75% are also listed in the following table; From the comparison of the reaction efficiency of the etherification stage grafting reaction in Examples 1, 17 to 19 in the above table and the purity of the finally obtained triglycidyl 4-amino-3-methylphenol epoxy resin, it can be seen that when the amounts of 4-amino-3-methylphenol and epichlorohydrin are the same and only the amount of the composite catalyst is different, the efficiency of the etherification stage grafting reaction is greatly affected. When the molar ratio of 4-amino-3-methylphenol: epichlorohydrin: catalyst is 1:9:0.54, the reaction efficiency of the etherification grafting reaction is the highest, the purity index of the final product is better, and the yield is the highest.
[0077] The triglycidyl 4-amino-3-methylphenol epoxy resins finally obtained in Examples 1, 17 to 19 in the above table can be stored for 11 to 15 months without deterioration at 25° C. and an air RH humidity of 75%, and the storage period is more than half a year.
[0078] Embodiments 20 to 22 A triglycidyl 4-amino-3-methylphenol epoxy resin, the preparation process of which is the same as that of Example 1, except that: in the preparation process step (1), the amounts of 4-amino-3-methylphenol and the catalyst are the same as those of Example 1, while the amount of epichlorohydrin is different, that is, the amount of epichlorohydrin in Examples 20 to 22 is calculated according to the molar ratio of 4-amino-3-methylphenol:epichlorohydrin:catalyst, as shown in the following table: The reaction efficiency of the etherification grafting reaction of 4-amino-3-methylphenol in step (1) of the preparation process, the purity and yield of the finally obtained triglycidyl 4-amino-3-methylphenol epoxy resin, and the storage time at 25° C. and air RH humidity of 75% are also listed in the following table; From the comparison of the reaction efficiency of the etherification stage grafting reaction of Examples 1, 22 to 24 in the above table and the purity of the finally obtained triglycidyl 4-amino-3-methylphenol epoxy resin, it can be seen that when the amount of epichlorohydrin is different, the reaction efficiency of the etherification stage grafting reaction is not greatly affected, and the purity of the final product is also very small. However, in a reactor of the same volume, if the molar number of epichlorohydrin increases, the feed amount of 4-amino-3-methylphenol is bound to decrease, thereby causing the output of triglycidyl 4-amino-3-methylphenol epoxy resin to become lower. Therefore, in order to maintain a considerable output, the preferred amount of 4-amino-3-methylphenol: epichlorohydrin is calculated in a molar ratio of 4-amino-3-methylphenol: epichlorohydrin to be 1:6 to 10.
[0079] The triglycidyl 4-amino-3-methylphenol epoxy resins finally obtained in the above Examples 1, 20 to 22 can be stored for 14 to 15 months at 25° C. and an air RH humidity of 75% without deterioration.
[0080] Embodiments 23 to 25 A triglycidyl 4-amino-3-methylphenol epoxy resin, the preparation process of which is the same as that of Example 1, except that the control temperature of the ring-closing reaction process in step (2) of Examples 23, 24, and 25 is 30° C., 45° C., and 50° C., respectively.
[0081] The content and purity of easily saponifiable chlorine of the triglycidyl 4-amino-3-methylphenol epoxy resin finally obtained in Examples 1 and 23 to 25 were measured. The results are shown in the following table: From the data on the content and purity of easily saponifiable chlorine in the triglycidyl 4-amino-3-methylphenol epoxy resin obtained in the above table, it can be seen that when the temperature is preferentially controlled at 30-45°C during the closed-loop reaction process, the content of easily saponifiable chlorine in the finished product is low and the product purity is higher, reaching 91.5-92.1%.
[0082] Embodiments 26 to 30 A triglycidyl 4-amino-3-methylphenol epoxy resin, the preparation process of which is the same as that of Example 1, except that: in the step (2) of Example 1 and Examples 26 to 30, the addition rate of the sodium hydroxide aqueous solution is controlled to be 1.65 g / min, 1.45 g / min, 1.85 g / min, 1.25 g / min, 2.05 g / min, and 2.25 g / min, respectively.
[0083] The content and purity of easily saponifiable chlorine of the triglycidyl 4-amino-3-methylphenol epoxy resin obtained in Examples 1, 26 to 30 were measured. The results are shown in the following table: From the easily saponifiable chlorine and purity data of triglycidyl 4-amino-3-methylphenol epoxy resin in the above table, it can be seen that when the drop rate of the sodium hydroxide aqueous solution with a mass percentage concentration of 48.5% is preferentially controlled to be 1.45-1.85 g / min during the closed-loop reaction process, the purity of the product is higher and can reach 91.7-92.1%.
[0084] Examples 31 to 34 A triglycidyl 4-amino-3-methylphenol epoxy resin, the preparation process of which is the same as that of Example 1, except that: in the ring-closing reaction process of step (2) of Examples 31 to 34, the amount of sodium hydroxide added is controlled, and the molar ratio of 4-amino-3-methylphenol to sodium hydroxide in the sodium hydroxide aqueous solution is 1:2.0, 1:2.3, 1:2.5, and 1:2.7 respectively; The separation conditions in the purification process ① of Examples 1 and 31 to 34 and the purity of the finally obtained triglycidyl 4-amino-3-methylphenol epoxy resin were observed. The results are shown in the following table: From the liquid separation condition in the purification process ① and the purity data of triglycidyl 4-amino-3-methylphenol epoxy resin in the above table, it can be seen that when the molar ratio of 4-amino-3-methylphenol: sodium hydroxide in the sodium hydroxide aqueous solution is 1:2.2-2.3, the liquid separation condition is good and the product purity is higher, reaching 91.8-92.1%.
[0085] Embodiments 35 to 38 A triglycidyl 4-amino-3-methylphenol epoxy resin, the preparation process of which is the same as that of Example 1, except that the control temperature of the refining reaction process in step (4) of Examples 35 to 38 is 60, 70, 85, and 100° C., respectively.
[0086] The liquid separation conditions in the purification process ① of Examples 1 and 35 to 38 and the content of easily saponifiable chlorine in the finally obtained triglycidyl 4-amino-3-methylphenol epoxy resin were observed. The results are shown in the following table: From the content of easily saponifiable chlorine in triglycidyl 4-amino-3-methylphenol epoxy resin in the above table, it can be seen that when the temperature is preferentially controlled at 70-85°C during the refining reaction process, the easily saponifiable chlorine in the resin after refining is lower, at 56-98 ppm, and the effect of the liquid separation condition in the preparation process is better.
[0087] Embodiments 39 to 42 A triglycidyl 4-amino-3-methylphenol epoxy resin, the preparation process of which is the same as that of Example 1, except that the control time of the refining reaction process in step (4) of Examples 39, 40, 41, and 42 is 3h, 5h, 7h, and 9h, respectively, that is, the control time of the refining reaction process is different.
[0088] The liquid separation conditions in the purification process ① of Examples 1 and 39 to 42 and the content of easily saponifiable chlorine in the finally obtained triglycidyl 4-amino-3-methylphenol epoxy resin were observed. The results are shown in the following table: From the content of easily saponifiable chlorine in triglycidyl 4-amino-3-methylphenol epoxy resin in the above table, it can be seen that when the refining reaction time is controlled at 2 to 5 hours, although the easily saponifiable chlorine content at the end of refining is equivalent to that at 7 to 9 hours, the effect of liquid separation in the purification process is better when the time is 2 to 5 hours.
[0089] Application Example 1 An adhesive containing the triglycidyl 4-amino-3-methylphenol epoxy resin obtained in Example 1, wherein the raw material composition and content thereof are, calculated by weight, 100 parts of the triglycidyl 4-amino-3-methylphenol epoxy resin obtained in Example 1, 125 parts of a curing agent, and 0.1 parts of an accelerator, respectively; The curing agent is methyltetrahydrophthalic anhydride; The above-mentioned accelerator is benzyl dimethylamine; The preparation method of the above-mentioned adhesive containing triglycidyl 4-amino-3-methylphenol epoxy resin comprises the following specific steps: The above-mentioned triglycidyl 4-amino-3-methylphenol epoxy resin, curing agent and accelerator are added into a container in sequence, and stirred and mixed evenly at a constant temperature of 20±2° C. to obtain an adhesive containing triglycidyl 4-amino-3-methylphenol epoxy resin.
[0090] The curing method of the adhesive containing triglycidyl 4-amino-3-methylphenol epoxy resin obtained above is as follows: the curing temperature and curing time are sequentially controlled to be 120° C. for 2 h and 160° C. for 2 h.
[0091] Comparative Example of Application Example 1 Triglycidyl p-aminophenol epoxy resin was used, the source was Shanghai Huayi Resin Co., Ltd., the product brand was AFG-90, and its chemical structure is as follows:
[0092] The triglycidyl 4-amino-3-methylphenol epoxy resin obtained in Example 1 is substituted for the triglycidyl 4-amino-3-methylphenol epoxy resin obtained in Example 1, and the rest is the same as in Example 1, and finally an adhesive containing triglycidyl p-aminophenol epoxy resin is obtained.
[0093] The curing method of the above-mentioned adhesive containing triglycidyl p-aminophenol epoxy resin is the same as the curing method in the above-mentioned application example 1.
[0094] Application Example 2 An adhesive containing the triglycidyl 4-amino-3-methylphenol epoxy resin obtained in Example 1, wherein the raw material composition and content used in its preparation are calculated by weight: the triglycidyl 4-amino-3-methylphenol epoxy resin obtained in Example 1, the curing agent, and the accelerator are 100 parts, 100 parts, and 0.3 parts, respectively; The curing agent is the same as that in Application Example 1; The above-mentioned accelerator is the same as that in Application Example 1.
[0095] The preparation method and curing method of the above-mentioned triglycidyl 4-amino-3-methylphenol epoxy resin obtained in Example 1 are the same as those in the above-mentioned Application Example 1.
[0096] Application Example 3 An adhesive containing triglycidyl 4-amino-3-methylphenol epoxy resin, wherein the raw materials used in its preparation are calculated by weight: triglycidyl 4-amino-3-methylphenol epoxy resin, curing agent, and accelerator are 100 parts, 150 parts, and 0.6 parts, respectively; The curing agent is the same as that in Application Example 1; The above-mentioned accelerator is the same as that in Application Example 1.
[0097] The Tg value, impact strength, flexural strength, tensile strength, and water absorption of the cured resin of the adhesive obtained in the above-mentioned Application Example 1 and the Application Control Example were measured; at the same time, the triglycidyl 4-amino-3-methylphenol epoxy resin used in Application Examples 1 to 3 of the present application and the triglycidyl p-aminophenol epoxy resin used in the control example of Application Example 1 were baked at a temperature of 190° C. for 3 hours, and the purity changes thereof were measured as shown in the following table: It can be seen from the above table that the adhesive prepared using the triglycidyl 4-amino-3-methylphenol epoxy resin of the present application has a higher Tg value and a lower water absorption rate after curing, and the triglycidyl 4-amino-3-methylphenol epoxy resin obtained in the present application has better high-temperature stability. Therefore, it is used in the bonding and sealing of electronic equipment and automobiles and other products that have high requirements for environmental temperature changes. After curing, it has higher high temperature resistance, lower water absorption and other properties.
[0098] In summary, the triglycidyl 4-amino-3-methylphenol epoxy resin of the present application, due to the synergistic effect of technical means such as the use of a composite catalyst in the etherification grafting reaction during the preparation process and the control of a specific ratio range, a specific feeding method, a reaction temperature, and a reaction time, the feeding amount of the sodium hydroxide aqueous solution in the closed-loop reaction stage, the feeding speed, and the pressure and temperature of the appropriate reaction process, and the control of the optimal reaction temperature and time in the refining reaction stage, the final triglycidyl 4-amino-3-methylphenol epoxy resin with high purity and long storage period is obtained. At the same time, after curing, it also has the characteristics of high temperature resistance and low water absorption. The adhesive prepared by using the adhesive can be widely used in the bonding and sealing of electronic equipment and automobiles and other products that have high requirements for environmental temperature and humidity changes.
[0099] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A triglycidyl 4-amino-3-methylphenol epoxy resin, Features Its structural formula is as follows:
2. A method for preparing a triglycidyl 4-amino-3-methylphenol epoxy resin as claimed in claim 1, Features The specific steps of the preparation process are as follows: (1) Etherification grafting reaction In a container, 4-amino-3-methylphenol, epichlorohydrin, a catalyst and solvent I are added in sequence, and then the temperature is controlled at 30-70° C. to react for 3-8 hours; The catalyst is at least one of an alkali metal solution, an alkaline earth metal salt, a quaternary ammonium salt, ethyl triphenylphosphine acetate, and triphenylphosphine; The alkali metal solution is an aqueous sodium hydroxide solution; The alkaline earth metal salt is calcium chloride, magnesium sulfate or barium sulfate; The quaternary ammonium salt is methyl trioctyl ammonium chloride, didecyl dimethyl ammonium chloride, dioctyl dimethyl ammonium chloride, dimethyl dioctadecyl ammonium chloride, benzyl dimethyl octyl ammonium chloride, dodecyl trimethyl ammonium chloride, octadecyl trimethyl ammonium chloride, tetraethyl ammonium bromide, benzyl triethyl ammonium chloride, benzyl diethyl ammonium bromide or benzyl trimethyl ammonium bromide; The above-mentioned 4-amino-3-methylphenol: epichlorohydrin: catalyst is used in a molar ratio of 4-amino-3-methylphenol: epichlorohydrin: catalyst of 1:6-15:0.1-0.6; The solvent I is an alcohol ether cosolvent, and the alcohol ether cosolvent is at least one of ethanol, butanol, ethylene glycol, propylene glycol, isopropanol, ethylene glycol monomethyl ether, propylene glycol monomethyl ether, and tripropylene glycol monomethyl ether; The amount of the solvent I is calculated by mass percentage, and the solvent I:epichlorohydrin is 10-30:100; (2) Closed-loop reaction Controlling the negative pressure at 0.07-0.09 MPa and the temperature at 30-50° C., adding a sodium hydroxide aqueous solution having a mass percentage concentration of 40-50% to the reaction solution after etherification and grafting obtained in step (1) to carry out a ring-closing reaction for 2-3 hours to obtain a reaction solution I containing triglycidyl 4-amino-3-methylphenol epoxy resin; The amount of the sodium hydroxide aqueous solution having a mass percentage concentration of 40 to 50% is calculated by molar ratio, and the molar ratio of 4-amino-3-methylphenol used in step (1) to the sodium hydroxide in the sodium hydroxide aqueous solution is 1:2.0 to 2.7; The addition rate of the sodium hydroxide aqueous solution with a mass percentage concentration of 40 to 50% is 1.25 to 2.25 g / min; (3) After the ring-closing reaction in step (2) is completed, the pressure is adjusted to a negative pressure of 0.098 MPa, and the temperature is raised to 80-125° C. to remove solvent I and excess unreacted epichlorohydrin. When the residual amounts of solvent I and unreacted epichlorohydrin are controlled to be less than 500 ppm, solvent II is added and mixed uniformly to obtain a reaction solution II containing triglycidyl 4-amino-3-methylphenol epoxy resin; The solvent II is at least one of toluene, xylene, butanone, and methyl isobutyl ketone, and the amount of solvent II added is 1 to 2.75 times the mass of the theoretically obtained triglycidyl 4-amino-3-methylphenol epoxy resin; (4) Refining reaction Adding a sodium hydroxide aqueous solution having a mass percentage concentration of 40 to 50% to the reaction solution II containing triglycidyl 4-amino-3-methylphenol epoxy resin obtained in step (3), controlling the temperature to 60 to 100° C. for a refining reaction for 2 to 9 hours, and obtaining a reaction solution after the refining reaction; The amount of the sodium hydroxide aqueous solution with a mass percentage concentration of 40 to 50% is 2 to 4 times the molar number of easily saponifiable chlorine in the reaction solution II containing triglycidyl 4-amino-3-methylphenol epoxy resin; (5) Purification ①, adding water to the reaction solution after the purification reaction obtained in the above step (4), stirring and mixing, and then standing to separate the layers to obtain an organic phase consisting of a brine phase and resin / solvent II, and removing the brine phase; The amount of water added is 3 to 6 times the mass of the byproduct sodium chloride theoretically produced after the ring-closing reaction in step (2); ②, adding a pH adjuster to the organic phase composed of the resin / solvent II obtained in ①, adjusting the pH value of the organic phase composed of the resin / solvent II to 5-7, and then separating the liquids, removing the aqueous phase, and obtaining an organic phase composed of the resin / solvent II with a pH value of 5-7; The pH regulator is one of phosphoric acid, sodium hydrogen phosphate, hydrochloric acid or oxalic acid; ③. Add water to the organic phase composed of resin / solvent II with a pH value of 5 to 7 obtained in ② and wash until there is no sodium chloride in the effluent, thereby obtaining a crude product containing triglycidyl 4-amino-3-methylphenol epoxy resin and solvent II; ④. The crude product containing triglycidyl 4-amino-3-methylphenol epoxy resin and solvent II obtained in ③ is heated in vacuum at a negative pressure of 0.0985-0.099 MPa and a temperature of 125-140° C. to remove solvent II, thereby obtaining triglycidyl 4-amino-3-methylphenol epoxy resin.
3. A method for preparing a triglycidyl 4-amino-3-methylphenol epoxy resin as claimed in claim 2, Features The amount of 4-amino-3-methylphenol:epichlorohydrin:catalyst in step (1) is calculated by molar ratio of 4-amino-3-methylphenol:epichlorohydrin:catalyst to be 1:6-10:0.1-0.
6.
4. A method for preparing a triglycidyl 4-amino-3-methylphenol epoxy resin as claimed in claim 3, Features The catalyst described in step (1) is composited by quaternary ammonium salt and alkali metal solution, wherein the quaternary ammonium salt is dodecyl trimethyl ammonium chloride, and the alkali metal solution is a sodium hydroxide aqueous solution with a mass percentage concentration of 40-50%; the consumption of dodecyl trimethyl ammonium chloride and the sodium hydroxide aqueous solution with a mass percentage concentration of 40-50% is calculated by mass ratio, and the ratio of dodecyl trimethyl ammonium chloride to the sodium hydroxide aqueous solution with a mass percentage concentration of 40-50% is 1:28-30.
5. A method for preparing a triglycidyl 4-amino-3-methylphenol epoxy resin as claimed in claim 3, Features The amount of sodium hydroxide in the catalyst described in step (1) is 1:0.53 according to the molar ratio of 4-amino-3-methylphenol to sodium hydroxide in a sodium hydroxide aqueous solution with a mass percentage concentration of 40-50%.
6. A method for preparing a triglycidyl 4-amino-3-methylphenol epoxy resin as claimed in claim 5, Features The sodium hydroxide aqueous solution with a mass percentage concentration of 40-50% of the catalyst in step (1) is added in 2-5 times, once every 30 minutes.
7. A method for preparing a triglycidyl 4-amino-3-methylphenol epoxy resin as claimed in claim 6, Features The sodium hydroxide aqueous solution with a mass percentage concentration of 40-50% in the catalyst described in step (1) is added in 4 portions.
8. A method for preparing a triglycidyl 4-amino-3-methylphenol epoxy resin as claimed in claim 7, Features During the etherification grafting reaction in step (1), the temperature is controlled at 30-55°C.
9. A method for preparing a triglycidyl 4-amino-3-methylphenol epoxy resin as claimed in claim 8, Features During the etherification grafting reaction in step (1), the temperature is controlled at 40-55°C.
10. A method for preparing a triglycidyl 4-amino-3-methylphenol epoxy resin as claimed in claim 9, Features During the etherification and grafting reaction in step (1), the etherification and grafting reaction time is 3 to 6 hours.
11. A method for preparing a triglycidyl 4-amino-3-methylphenol epoxy resin as claimed in claim 10, Features During the etherification and grafting reaction in step (1), the etherification and grafting reaction time is 4 to 6 hours.
12. A method for preparing a triglycidyl 4-amino-3-methylphenol epoxy resin as claimed in claim 11, Features During the ring-closing reaction of step (2), the addition rate of the sodium hydroxide aqueous solution with a mass percentage concentration of 40 to 50% is controlled to be 1.45 to 1.85 g / min, and the amount of the sodium hydroxide aqueous solution with a mass percentage concentration of 40 to 50% is calculated in a molar ratio of 4-amino-3-methylphenol used in the preparation process step (1): sodium hydroxide in the sodium hydroxide aqueous solution with a mass percentage concentration of 40 to 50% is 1:2.2 to 2.
3.
13. A method for preparing a triglycidyl 4-amino-3-methylphenol epoxy resin as claimed in claim 12, Features During the ring-closing reaction in step (2), the temperature was controlled at 40°C.
14. A method for preparing a triglycidyl 4-amino-3-methylphenol epoxy resin as claimed in claim 13, Features In step (3), the temperature of the refining reaction is controlled at 70 to 85° C. and the refining reaction is carried out for 2 to 5 hours.
15. An adhesive containing the triglycidyl 4-amino-3-methylphenol epoxy resin as claimed in claim 1, wherein the raw material composition and content used in its preparation are, by weight, 100 parts of triglycidyl 4-amino-3-methylphenol epoxy resin, 100-150 parts of curing agent, and 0.1-0.6 parts of accelerator, respectively; The curing agent is an acid anhydride curing agent, and the acid anhydride curing agent is one or more of methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, hexahydrophthalic anhydride, tetrahydrophthalic anhydride and methylnadic anhydride; The above-mentioned accelerator is imidazole, benzyldimethylamine, 2,4,6-tris(dimethylaminomethyl)phenol or o-hydroxybenzyldimethylamine; the raw materials used in the above-mentioned adhesive containing triglycidyl 4-amino-3-methylphenol epoxy resin are stored separately, and when used, the temperature is controlled at 20±2° C. for mixing, and then cured; The curing is to control the temperature to 120° C. for curing for 2 hours and 160° C. for curing for 2 hours.
Citation Information
Patent Citations
Preparation method of triglycidyl-meta-aminophenol epoxy resin
CN104478831A
Epoxy resin composition, epoxy resin cured product, prepreg and fiber-reinforced composite material
CN107949593A
Adhesive composition and adhesive sheet using the same
JP2011148864A
Cited By
Tetraglycidyl amine-containing epoxy resin composition as well as preparation method and application thereof
CN120795553A