Ultralow-viscosity light-shielding acrylonitrile-butadiene-styrene composition as well as preparation method and application thereof
Through the shear thinning effect of the ultra-low viscosity acrylonitrile-butadiene-styrene composition and the combination of nano-metal powder, the fluidity and light shielding problems of traditional ABS materials in the processing of micro-thin light guide parts are solved, and high efficiency is achieved. Excellent light shielding effect and low cost production.
Patent Information
- Application Number
- CN202310462852.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-26
- Publication Date
- 2024-10-29
AI Technical Summary
Traditional ABS materials have problems such as insufficient thickness, poor fluidity and weak light guiding function in the application of light guide parts, making it difficult to process and form thin light guide parts.
Develop an ultra-low viscosity acrylonitrile-butadiene-styrene composition, which reduces the melt viscosity through the shear thinning effect and flow curve platform characteristics, and combines nanometal powder and high reflectivity light shielding agent to achieve ultra-low viscosity. Injection molding processing of thin structure and excellent light shielding effect.
It achieves the processing of light guide parts and excellent light shielding effect at extremely thin thickness, reduces manufacturing costs, and improves the market penetration and competitiveness of the technology.
Smart Images

Figure BDA0004201302250000081
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer materials, and in particular relates to an ultra-low viscosity light-shielding acrylonitrile-butadiene-styrene composition and a preparation method and application thereof. Background Art
[0002] Acrylonitrile Butadiene Styrene (ABS) is a graft copolymer of acrylonitrile, butadiene and styrene. It combines the chemical resistance and high surface hardness of acrylonitrile, the toughness of butadiene, and the coloring and good processability of styrene. It is widely used in the appearance parts of home appliances, automobiles, aviation and other fields.
[0003] The emerging contactless optical touch control is a booming technology with great advantages. It guides light directionally through parts and uses the amount and direction of light as action signals to control the device.
[0004] There is little research on this field specifically for existing materials, especially for the application and development of core light-guiding parts. Traditional ABS materials are almost all used in the field of traditional structural dimensions, and the thickness of parts is mostly around 2mm. Thinner wall thickness, such as 1mm thick parts, require a lot of injection pressure during molding (injection molding process) due to the large resistance of the melt, and it is even difficult to complete the molding process. The micron and nanometer thickness of the light-guiding parts is obviously far beyond the application scope of current materials. The thinner the part thickness, the less effect the material has on light and the weaker the light-guiding function. These are the problems that need to be solved in the application of traditional materials in the field of light-guiding. Summary of the invention
[0005] In order to solve the above technical defects, the purpose of the present invention is to provide an ultra-low viscosity light-shielding acrylonitrile-butadiene-styrene composition and a preparation method thereof, which is used in light-guiding ultra-thin structural parts. The "neck" shear thinning effect in ultra-thin thickness enables the resin to break through the traditional product thickness limit, and can be processed and formed in ultra-thin thickness parts with super fluidity, and has excellent light-shielding properties in ultra-thin thickness products.
[0006] The objective of the present invention is achieved through the following technical solutions:
[0007] The first object of the present invention is to provide an ultra-low viscosity light-shielding acrylonitrile-butadiene-styrene composition, which is made of the following components in parts by weight:
[0008] Acrylonitrile-butadiene-styrene resin: 58-90 parts,
[0009] Light diffuser: 3-15 parts,
[0010] Light shielding agent: 5-20 parts,
[0011] Light stabilizer: 0.5-2 parts,
[0012] Processing aids: 0.5-2 parts,
[0013] Metal powder: 0.5-3 parts;
[0014] The content of butadiene component in the acrylonitrile-butadiene-styrene resin is between 10% and 20%, and the relative density of the acrylonitrile-butadiene-styrene resin is between 1.02 and 1.05 g / cm 3 The melt viscosity index of the acrylonitrile-butadiene-styrene resin is ≤100 Pa.s at a shear rate of 1000 1 / s under the test conditions of 220°C and ≤2 Pa.s at a shear rate of 100000 1 / s.
[0015] The light diffuser is at least one of barium sulfate, calcium carbonate and silicon dioxide, and the particle size of the light diffuser is less than 0.5 micrometers. Furthermore, the light diffuser is a mixture of barium sulfate and calcium carbonate in a weight ratio of 2:1.
[0016] The light shielding agent is rutile titanium dioxide, and the titanium dioxide content thereof is greater than 96%.
[0017] The light stabilizer is at least one of a benzophenone light stabilizer, a benzotriazole light stabilizer, a benzotriazole light stabilizer, and a hindered amine light stabilizer.
[0018] The processing aid comprises a heat stabilizer and a lubricant; the heat stabilizer is selected from at least one of hindered phenol heat stabilizers, thioester heat stabilizers and phosphite heat stabilizers; the lubricant is selected from at least one of solid paraffin, liquid paraffin, low molecular weight polyethylene, stearic acid amide, methylene bis stearic acid amide and ethylene bis stearic acid amide.
[0019] The metal powder is at least one of aluminum powder, silver powder, iron powder, nickel powder and zinc powder; the particle size of the metal powder is 5nm-100nm, belonging to the nanometer level, and the shape is spherical.
[0020] A second object of the present invention is to provide a method for preparing the ultra-low viscosity light-shielding acrylonitrile-butadiene-styrene composition as described in the first object, comprising the following steps:
[0021] (1) Weighing 58 to 90 parts of acrylonitrile-butadiene-styrene resin, 3 to 15 parts of light diffusing agent, 5 to 20 parts of light shielding agent, 0.5 to 2 parts of light stabilizer, 0.5 to 2 parts of processing aid, and 0.5 to 3 parts of metal powder, and mixing them uniformly to obtain a mixed material;
[0022] (2) The mixed material is fed into a twin-screw extruder. Under the conveying and shearing action of the screw, the material is fully melted and compounded, and then extruded, drawn, cooled, and pelletized through a die head to obtain a final product. The screw temperature of the first zone of the twin-screw extruder is 190-210° C.; the screw temperature from the second zone to the die head is 210-250° C.; and the screw speed is 200-500 r / min.
[0023] The third object of the present invention is to provide an application of the ultra-low viscosity light-shielding acrylonitrile-butadiene-styrene composition as described in the first object in the light-guiding field, which can be used to prepare ultra-thin light-guiding structural parts, can complete injection molding processing for extremely thin thickness light-guiding parts, and realizes the processing completeness of light-guiding parts.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] (1) The present invention utilizes the shear thinning principle and the characteristics of the flow curve platform, and selects acrylonitrile-butadiene-styrene resin as the base resin, whose melt viscosity decreases under high shear and whose viscosity reaches the limit under a certain shear rate condition. In this way, the high shear effect generated under high-speed injection makes the viscosity of acrylonitrile-butadiene-styrene resin fully reduced and its fluidity rapidly improved, thus completing the injection molding process of ultra-thin structural parts. This solves the problem that due to the small cavity space of the thin-walled structure, the resistance of the melt flowing in it is large, resulting in slow flow, and some very thin structures are almost difficult to complete injection molding, resulting in short shots and incomplete injection.
[0026] (2) The ultra-low viscosity light-shielding acrylonitrile-butadiene-styrene composition provided by the present invention has an excellent light-shielding effect, thereby completing the functional realization of the light-guiding parts. The light-shielding agent involved in the technical disclosure of the present invention makes full use of the reflection principle and scattering principle of light, selects titanium dioxide with special components and content to improve the high reflection of light; selects a light diffusing agent with a special particle size and special components to improve the scattering effect of light, and finally achieves a light-shielding effect.
[0027] (3) The acrylonitrile-butadiene-styrene composition provided by the present invention is used for processing ultra-thin structure products, the thickness of which is micrometer or nanometer level, and the light shielding effect achieved by only using traditional material technology is not very excellent. The present invention introduces nano metal powder and cooperates with the rutile titanium dioxide light shielding agent of the present invention, and uses the metal powder to color the material to improve the glossiness of the material surface, thereby improving the light reflection effect; in addition, since the titanium dioxide crystal structure in the anatase titanium dioxide has a larger arrangement space, the photochemical properties of the small molecular water and oxygen on its surface are extremely active, and the metal atoms in the metal powder pigment are easily excited and transitioned on its surface; and the titanium dioxide crystal structure in the rutile titanium dioxide has a tighter arrangement space, and the metal powder pigment is easy to form a firm and dense skin on its surface, thereby improving the light shielding effect.
[0028] (4) The ultra-low viscosity light-shielding acrylonitrile-butadiene-styrene composition provided by the present invention not only realizes the feasibility of processing extremely thin light-guiding parts, but also greatly reduces the manufacturing cost. Compared with other processes such as electroplating and spraying, it improves the market penetration and competitiveness of the technology. DETAILED DESCRIPTION
[0029] The present invention is further described below in conjunction with embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.
[0030] In addition, unless otherwise specified, the preparation processes in the following embodiments are all conventional means in the prior art in the art, and therefore, they are not described in detail; the parts in the following embodiments are all parts by weight.
[0031] The models and suppliers of the reagents used in this embodiment and comparative example are as follows:
[0032] The acrylonitrile-butadiene-styrene resin is HG-203D from LG of South Korea, which is produced by an emulsion grafting method, and the melt viscosity index is 90 Pa.s at a shear rate of 1000 1 / s at 220°C and 0.9 Pa.s at a shear rate of 1000001 / s at 220°C.
[0033] The acrylonitrile-butadiene-styrene resin was 750 from Daqing Petrochemical.
[0034] The particle size of ultrafine barium sulfate is 0.4 micron (25000 mesh), and the supplier is CIMBAR in the United States;
[0035] The particle size of barium sulfate is 5.5 μm (2500 mesh), and the supplier is CIMBAR, USA;
[0036] The particle size of fine calcium carbonate is 0.4 microns (25000 mesh);
[0037] The particle size of calcium carbonate is 7.5 microns (2000 mesh).
[0038] The light shielding agent is selected from rutile titanium dioxide with the brand name R-771 produced by Bamon or anatase titanium dioxide with the brand name NA100 produced by Nanjing Titanium Dioxide Chemical Co., Ltd.
[0039] The light stabilizer is a mixture of a hindered amine light stabilizer (LA-944B from Changchun Chemical) and a benzotriazole light stabilizer (UV-360 from Changchun Chemical) at a weight ratio of LA-944B:UV-360=3:2.
[0040] The processing aid is a heat stabilizer which is a mixture of a hindered phenol heat stabilizer (AO-62A of Changchun Chemical Industry) and a phosphite heat stabilizer (2112B of Changchun Chemical Industry) in a weight ratio of AO-62A:2112B=1:2;
[0041] The lubricant is domestic EBS, commercially available.
[0042] The metal powder is nano silver powder produced by Nanjing Fengyue Nanotechnology Co., Ltd. It is spherical, with a particle size of 50nm and a silver-gray color.
[0043] The above reagents are only for illustrating the sources and components of the reagents used in the experiments of the present invention so as to fully disclose the information, and do not mean that the present invention cannot be realized by using other similar reagents or reagents provided by other suppliers.
[0044] Example 1
[0045] A method for preparing an ultra-low viscosity light-shielding acrylonitrile-butadiene-styrene composition comprises the following steps:
[0046] (1) 75.5 parts of HG-203D from LG, 10 parts of a mixture of ultrafine barium sulfate and fine calcium carbonate (weight ratio = 2:1), 12 parts of R-771, 0.5 parts of a light stabilizer, 0.5 parts of a processing aid (0.3 parts of a heat stabilizer, 0.2 parts of a lubricant), and 1.5 parts of metallic silver powder were mixed uniformly by high-speed stirring to obtain a mixed material;
[0047] (2) The mixed material is fed into a twin-screw extruder, fully melted and compounded under the conveying and shearing action of the screw, and then extruded through a die, drawn into strips, cooled, and pelletized.
[0048] Among them: the screw temperature of each section of the twin-screw extruder is: the temperature of zone 1 is controlled at 200℃, the temperature of each section from zone 2 to the die is controlled at 210℃ in zone 2, 230℃ in zone 3, 245℃ in zone 4, 245℃ in zone 5, 235℃ in zone 6, 235℃ in zone 7, 250 in die head, and the screw speed is 400r / min.
[0049] Comparative Example 1
[0050] A method for preparing an ultra-low viscosity light-shielding acrylonitrile-butadiene-styrene composition comprises the following steps:
[0051] (1) 75.5 parts of HG-203D from LG of South Korea, 10 parts of a mixture of ultrafine barium sulfate and fine calcium carbonate (weight ratio of the two = 2:1), 12 parts of NA100, 0.5 parts of a light stabilizer, 0.5 parts of a processing aid (0.3 parts of a heat stabilizer, 0.2 parts of a lubricant), and 1.5 parts of metallic silver powder were mixed uniformly by high-speed stirring to obtain a mixed material;
[0052] (2) The mixed material is fed into a twin-screw extruder, fully melted and compounded under the conveying and shearing action of the screw, and then extruded through a die, drawn into strips, cooled, and pelletized.
[0053] Among them: the screw temperature of each section of the twin-screw extruder is: the temperature of zone 1 is controlled at 200℃, the temperature of each section from zone 2 to the die is controlled at 210℃ in zone 2, 230℃ in zone 3, 245℃ in zone 4, 245℃ in zone 5, 235℃ in zone 6, 235℃ in zone 7, 250 in die head, and the screw speed is 400r / min.
[0054] Example 2
[0055] A method for preparing an ultra-low viscosity light-shielding acrylonitrile-butadiene-styrene composition comprises the following steps:
[0056] (1) 89.5 parts of HG-203D from LG of South Korea, 3 parts of a mixture of ultrafine barium sulfate and fine calcium carbonate (weight ratio of the two = 2:1), 5 parts of R-771, 1 part of a light stabilizer, 1 part of a processing aid (0.8 parts of a heat stabilizer, 0.2 parts of a lubricant), and 0.5 parts of metallic silver powder were mixed uniformly by high-speed stirring to obtain a mixed material;
[0057] (2) The mixed material is fed into a twin-screw extruder, fully melted and compounded under the conveying and shearing action of the screw, and then extruded through a die, drawn into strips, cooled, and pelletized.
[0058] Among them: the screw temperature of each section of the twin-screw extruder is: the temperature of zone 1 is controlled at 200℃, the temperature of each section from zone 2 to the die is controlled at 210℃ in zone 2, 230℃ in zone 3, 245℃ in zone 4, 245℃ in zone 5, 235℃ in zone 6, 235℃ in zone 7, 250 in die head, and the screw speed is 400r / min.
[0059] Comparative Example 2-1
[0060] A method for preparing an ultra-low viscosity light-shielding acrylonitrile-butadiene-styrene composition comprises the following steps:
[0061] (1) 89.5 parts of Daqing Petrochemical's 750, 3 parts of a mixture of ultrafine barium sulfate and fine calcium carbonate (weight ratio = 2:1), 5 parts of R-771, 1 part of a light stabilizer, 1 part of a processing aid (0.8 parts of a heat stabilizer, 0.2 parts of a lubricant), and 0.5 parts of metallic silver powder were mixed uniformly by high-speed stirring to obtain a mixed material;
[0062] (2) The mixed material is fed into a twin-screw extruder, fully melted and compounded under the conveying and shearing action of the screw, and then extruded through a die, drawn into strips, cooled, and pelletized.
[0063] Among them: the screw temperature of each section of the twin-screw extruder is: the temperature of zone 1 is controlled at 200℃, the temperature of each section from zone 2 to the die is controlled at 210℃ in zone 2, 230℃ in zone 3, 245℃ in zone 4, 245℃ in zone 5, 235℃ in zone 6, 235℃ in zone 7, 250 in die head, and the screw speed is 400r / min.
[0064] Comparative Example 2-2
[0065] A method for preparing an ultra-low viscosity light-shielding acrylonitrile-butadiene-styrene composition comprises the following steps:
[0066] (1) 90 parts of HG-203D from LG of South Korea, 3 parts of a mixture of ultrafine barium sulfate and fine calcium carbonate (weight ratio of the two = 2:1), 5 parts of R-771, 1 part of a light stabilizer, and 1 part of a processing aid (0.8 parts of a heat stabilizer and 0.2 parts of a lubricant) were mixed uniformly by high-speed stirring to obtain a mixed material;
[0067] (2) The mixed material is fed into a twin-screw extruder, fully melted and compounded under the conveying and shearing action of the screw, and then extruded through a die, drawn into strips, cooled, and pelletized.
[0068] Among them: the screw temperature of each section of the twin-screw extruder is: the temperature of zone 1 is controlled at 200℃, the temperature of each section from zone 2 to the die is controlled at 210℃ in zone 2, 230℃ in zone 3, 245℃ in zone 4, 245℃ in zone 5, 235℃ in zone 6, 235℃ in zone 7, 250 in die head, and the screw speed is 400r / min.
[0069] Example 3
[0070] A method for preparing an ultra-low viscosity light-shielding acrylonitrile-butadiene-styrene composition comprises the following steps:
[0071] (1) 58 parts of HG-203D from LG of South Korea, 15 parts of a mixture of ultrafine barium sulfate and fine calcium carbonate (weight ratio of the two = 2:1), 20 parts of R-771, 2 parts of a light stabilizer, 2 parts of a processing aid (1.8 parts of a heat stabilizer, 0.2 parts of a lubricant), and 3 parts of metallic silver powder were mixed uniformly by high-speed stirring to obtain a mixed material;
[0072] (2) The mixed material is fed into a twin-screw extruder, fully melted and compounded under the conveying and shearing action of the screw, and then extruded through a die, drawn into strips, cooled, and pelletized.
[0073] Among them: the screw temperature of each section of the twin-screw extruder is: the temperature of zone 1 is controlled at 200℃, the temperature of each section from zone 2 to the die is controlled at 210℃ in zone 2, 230℃ in zone 3, 245℃ in zone 4, 245℃ in zone 5, 235℃ in zone 6, 235℃ in zone 7, 250 in die head, and the screw speed is 400r / min.
[0074] Comparative Example 3
[0075] A method for preparing an ultra-low viscosity light-shielding acrylonitrile-butadiene-styrene composition comprises the following steps:
[0076] (1) 58 parts of HG-203D from LG, 15 parts of a mixture of barium sulfate and calcium carbonate (weight ratio = 2:1), 20 parts of R-771, 2 parts of a light stabilizer, 2 parts of a processing aid (1.8 parts of a heat stabilizer, 0.2 parts of a lubricant), and 3 parts of metallic silver powder were mixed uniformly by high-speed stirring to obtain a mixed material;
[0077] (2) The mixed material is fed into a twin-screw extruder, fully melted and compounded under the conveying and shearing action of the screw, and then extruded through a die, drawn into strips, cooled, and pelletized.
[0078] Among them: the screw temperature of each section of the twin-screw extruder is: the temperature of zone 1 is controlled at 200℃, the temperature of each section from zone 2 to the die is controlled at 210℃ in zone 2, 230℃ in zone 3, 245℃ in zone 4, 245℃ in zone 5, 235℃ in zone 6, 235℃ in zone 7, 250 in die head, and the screw speed is 400r / min.
[0079] Performance Testing
[0080] The light shielding effect of the ultra-low viscosity light shielding acrylonitrile-butadiene-styrene composition material prepared in the above-mentioned embodiments and comparative examples is judged by the transmittance index of ISO 13468 (thickness 0.5 mm), wherein the larger the transmittance value, the worse the light shielding effect.
[0081] The viscosity of the ultra-low viscosity light-shielding acrylonitrile-butadiene-styrene composition material prepared in the above-mentioned embodiments and comparative examples is determined by injection molding the material into a 150mm×2mm×0.05mm rectangular sample piece and measuring the flow length of the injection-molded piece to judge its viscosity.
[0082] The performance test results of the materials prepared in various embodiments and comparative examples are shown in Table 1:
[0083] Table 1 Material performance test results
[0084]
[0085] It can be seen from Table 1 that the viscosity, light shielding and other indicators of the materials prepared by the examples are significantly improved. By comparing Example 1 with Comparative Example 1, it can be seen that the light shielding property of the material using rutile titanium dioxide of the present invention is significantly better than that of anatase titanium dioxide, and the transmittance of the prepared material is reduced by 81%. By comparing Example 2 with Comparative Example 2-1, after the present invention selects an ABS resin substrate with a melt viscosity index lower than the specified requirement, its injection viscosity is significantly reduced under the "neck" shear thinning effect, and a longer flow length can be more effectively formed in an ultra-thin thickness structure. By comparing Example 2 with Comparative Example 2-2, not adding metal powder will lead to a 28% increase in the material transmittance and a weakened light shielding effect. By comparing Example 3 with Comparative Example 3, it can be seen that the light shielding property of the material prepared by the present invention using a small-particle light diffusing agent has obvious advantages, and the transmittance is reduced by 92%.
[0086] The above description of the embodiments is to facilitate the understanding and application of the present invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the embodiments herein, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the protection scope of the present invention.
Claims
1. An ultra-low viscosity light-shielding acrylonitrile-butadiene-styrene composition, characterized in that: Made from the following components in parts by weight: Acrylonitrile-butadiene-styrene resin: 58-90 parts, Light diffuser: 3-15 parts, Light shielding agent: 5-20 parts, Light stabilizer: 0.5-2 parts, Processing aids: 0.5-2 parts, Metal powder: 0.5-3 parts; The melt viscosity index of the acrylonitrile-butadiene-styrene resin is ≤100 Pa.s under the test conditions of 220° C. and a shear rate of 1000 1 / s, and must be ≤2 Pa.s under a shear rate of 100000 1 / s.
2. The ultra-low viscosity light-shielding acrylonitrile-butadiene-styrene composition according to claim 1, characterized in that: The content of butadiene component in the acrylonitrile-butadiene-styrene resin is between 10% and 20%, and the relative density of the acrylonitrile-butadiene-styrene resin is between 1.02 and 1.05 g / cm 3 .
3. The ultra-low viscosity light-shielding acrylonitrile-butadiene-styrene composition according to claim 1, characterized in that: The light diffuser is at least one of barium sulfate, calcium carbonate and silicon dioxide, and the particle size of the light diffuser is less than 0.5 micrometers.
4. The ultra-low viscosity light-shielding acrylonitrile-butadiene-styrene composition according to claim 3, characterized in that: The light diffuser is a mixture of barium sulfate and calcium carbonate in a weight ratio of 2:
1.
5. The ultra-low viscosity light-shielding acrylonitrile-butadiene-styrene composition according to claim 1, characterized in that: The light shielding agent is rutile titanium dioxide, and the titanium dioxide content thereof is greater than 96%.
6. The ultra-low viscosity light-shielding acrylonitrile-butadiene-styrene composition according to claim 1, characterized in that: The light stabilizer is at least one of a benzophenone light stabilizer, a benzotriazole light stabilizer, a benzotriazole light stabilizer, and a hindered amine light stabilizer.
7. The ultra-low viscosity light-shielding acrylonitrile-butadiene-styrene composition according to claim 1, characterized in that: The processing aid comprises a heat stabilizer and a lubricant; the heat stabilizer is selected from at least one of hindered phenol heat stabilizers, thioester heat stabilizers and phosphite heat stabilizers; the lubricant is selected from at least one of solid paraffin, liquid paraffin, low molecular weight polyethylene, stearic acid amide, methylene bis stearic acid amide and ethylene bis stearic acid amide.
8. The ultra-low viscosity light-shielding acrylonitrile-butadiene-styrene composition according to claim 1, characterized in that: The metal powder is at least one of aluminum powder, silver powder, iron powder, nickel powder and zinc powder; the particle size of the metal powder is 5nm-100nm, belonging to the nanometer level, and the shape is spherical.
9. The method for preparing the ultra-low viscosity light-shielding acrylonitrile-butadiene-styrene composition according to any one of claims 1 to 8, characterized in that: The following steps are involved: (1) Weighing 58 to 90 parts of acrylonitrile-butadiene-styrene resin, 3 to 15 parts of light diffusing agent, 5 to 20 parts of light shielding agent, 0.5 to 2 parts of light stabilizer, 0.5 to 2 parts of processing aid, and 0.5 to 3 parts of metal powder, and mixing them uniformly to obtain a mixed material; (2) The mixed material is fed into a twin-screw extruder. Under the conveying and shearing action of the screw, the material is fully melted and compounded, and then extruded, drawn, cooled, and pelletized through a die head to obtain a final product. The screw temperature of the first zone of the twin-screw extruder is 190-210° C.; the screw temperature from the second zone to the die head is 210-250° C.; and the screw speed is 200-500 r / min.
10. The ultra-low viscosity light-shielding acrylonitrile-butadiene-styrene composition according to any one of claims 1 to 8 is used for preparing light-guiding ultra-thin structural parts.