High-temperature-resistant powder coating with gloss retention performance and production method of high-temperature-resistant powder coating
By using acrylic resin, silicone resin and other constituent materials in powder coatings, and forming a structure of zirconium dioxide core and nano-cerium oxide shell through a specific preparation method, the lack of gloss retention and high temperature resistance of existing powder coatings is solved. problem, significantly improving the high temperature resistance and gloss retention properties of the coating, and is suitable for the automotive coating field.
Patent Information
- Application Number
- CN202411354761.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-27
- Publication Date
- 2024-10-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing high-viscosity powder coatings have poor gloss retention and high temperature resistance, which affects their service life and quality.
A powder coating composed of acrylic resin, silicone resin, isophorone diisocyanate, functional additives, inorganic fillers, leveling agents, defoaming agents, pigments and antioxidants is used to prepare a powder coating with two properties through a specific preparation method. The inorganic base material of zirconium oxide core and nano-cerium oxide shell forms a dense antioxidant film layer to improve the high temperature resistance and gloss retention performance of the coating.
It significantly improves the high temperature resistance and gloss retention performance of powder coatings, extends its service life and ensures quality, and is suitable for automotive painting fields.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of coatings, and in particular to a high temperature resistant powder coating with gloss retention performance and a production method thereof. Background Art
[0002] Powder coating is a solid powdered synthetic resin coating composed of solid resin, pigment, filler and additives. Unlike ordinary solvent-based coatings and water-based coatings, its dispersion medium is not solvent and water, but air. It has the characteristics of no solvent pollution, 100% film formation and low energy consumption. Powder coatings are divided into two categories: thermoplastic and thermosetting. Thermoplastic powder coatings have poor coating film appearance (gloss and leveling) and poor adhesion to metal, so they are rarely used in the field of automotive coating. Automotive coating generally uses thermosetting powder coatings. Thermosetting powder coatings use thermosetting synthetic resin as the film-forming material. During the drying process, the resin first melts and then solidifies into a smooth and hard coating film after chemical cross-linking. The coating film appearance, various mechanical properties and corrosion resistance formed by this kind of coating can meet the requirements of automotive finishing.
[0003] A high-viscosity powder coating, a preparation method and an application thereof are disclosed in the patent document with application number "CN202211584395.5", which relates to the technical field of powder coatings. The high-viscosity powder coating comprises the following components by weight: 50-60 parts of modified acrylic resin; 2-3 parts of polar curing agent; 0.1-0.5 parts of catalyst; 0.5-1 parts of brightener; 0.2-0.5 parts of benzoin; 0.5-1 parts of pigment; 20-50 parts of filler. Although the powder coating prepared according to this patent document has the advantages of strong adhesion and corrosion resistance, its own light retention and high temperature resistance are relatively poor, which not only shortens its service life to a certain extent, but also affects its quality. Therefore, the present invention provides a high-temperature resistant powder coating with light retention performance and a production method thereof to solve the above-mentioned technical problems. Summary of the invention
[0004] The purpose of the present invention is to provide a high temperature resistant powder coating with gloss retention performance and a production method thereof. The produced powder coating not only has excellent high temperature resistance, but also has good gloss retention performance, which prolongs its service life to a certain extent and also effectively guarantees its quality.
[0005] To achieve the above object, the present invention provides the following technical solutions: A high temperature resistant powder coating with gloss retention performance, comprising the following raw materials in parts by weight: 20 to 60 parts of acrylic resin, 15 to 40 parts of silicone resin, 7 to 15 parts of isophorone diisocyanate, 0.5 to 1.2 parts of benzoic acid ketone, 8 to 15 parts of functional additives, 20 to 45 parts of inorganic fillers, 0.5 to 2.5 parts of leveling agents, 0.8 to 3.5 parts of defoaming agents, 2 to 6 parts of pigments and 0.8 to 1.5 parts of antioxidants; The acid value of the acrylic resin is 7-10 mgKOH / g; the silicone resin is SH-1068 solid silicone resin or German Wacker silicone resin SILRES-610.
[0006] Furthermore, the preparation method of the functional additive comprises the following steps: The first step is to put the inorganic substrate into xylene at a solid-liquid ratio of 5 to 8 g / L, and ultrasonically disperse it for 50 to 70 minutes, then add 3-aminopropyltrimethoxysilane with a mass of 1.5 to 2.0 times that of the inorganic substrate, mix and stir evenly, and reflux for 8 to 12 hours under the protection of nitrogen; after the reaction is completed, filter the product components, wash with alcohol, and vacuum dry them in turn, and the obtained pretreated inorganic substrate is stored and used; The second step is to put the pretreated inorganic substrate into anhydrous ethanol at a solid-liquid ratio of 0.02 to 0.05 g / mL, and add pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] in an amount 2 to 3 times the mass of the pretreated inorganic substrate, mix and stir evenly, and then keep the mixture at a temperature of 50 to 60°C for 40 to 50 hours; after the reaction is completed, filter the resulting components, wash the filter cake with anhydrous ethanol for 3 to 5 times, and then vacuum dry it at a temperature of 60 to 70°C, and the final product is the functional additive.
[0007] Furthermore, the method for preparing the inorganic substrate comprises the following steps: Step 1, adjusting the pH of 0.3-0.6wt% sodium polyacrylate aqueous solution to 4.3-4.8, then adding zirconium dioxide with a mass of 40-60% of the sodium polyacrylate aqueous solution and a particle size of 2-5 μm, mixing and stirring evenly, and then ball milling and dispersing for 25-35 hours, and the obtained zirconium dioxide dispersion is stored and used for standby; Step 2: Add 8-15% of the mass of inorganic sol to the zirconium dioxide dispersion while stirring. After the addition is completed, continue stirring for 6-10 hours and then raise the temperature to 80-85°C. After stirring and drying, dry the obtained solid material at 220-240°C for 5-8h; after drying, heat treat it at 700-900°C for 7-10h; the solid material after heat treatment is naturally cooled to room temperature, and then ground and sieved through a 250-mesh sieve to obtain an inorganic substrate.
[0008] Furthermore, the preparation method of the inorganic sol includes the following steps: dropping 0.01-0.02 g / mL of cerium nitrate aqueous solution into 3-5 M sodium hydroxide aqueous solution, and after precipitation is complete, adjusting the pH to 10.5-11.5, mixing and stirring for 3-5 hours, and filtering. When the filter cake is washed until there is no nitrate ion, the pH is adjusted to 0.8-1.5, and the mixture is stirred at 30-40° C. for 4-6 hours, and then stirred at 50-70° C. for 20-25 hours. The obtained colloid is immediately cooled and then the impurity ions therein are removed by dialysis, and the final product is the inorganic sol.
[0009] Furthermore, the inorganic filler is selected from any one of barium sulfate, titanium dioxide and talc.
[0010] Furthermore, the leveling agent is selected from any one of leveling agent GLP388, leveling agent GLP588, and leveling agent GLP788.
[0011] Furthermore, the defoaming agent is selected from any one of TP-39 defoaming agent, polyoxyethylene polyoxypropanolamine ether defoaming agent, and polydimethylsiloxane.
[0012] Furthermore, the pigment is selected from any one of cobalt blue and cobalt green.
[0013] Furthermore, the antioxidant is selected from any one of triphenyl phosphite, 2,6-di-tert-butyl-p-cresol, antioxidant 1076, and antioxidant 1010.
[0014] A method for producing a high-temperature resistant powder coating with gloss-retaining properties comprises the following steps: accurately weighing each raw material according to the formula amount and pouring each raw material into a high-speed mixer, fully mixing for 10 to 15 minutes, transferring the obtained mixture into an extruder, and after melt extrusion, passing through a tabletting roller to cool the tablet, and then successively crushing, pulverizing and sieving to obtain the high-temperature resistant powder coating with gloss-retaining properties.
[0015] Compared with the prior art, the present invention has the following beneficial effects: In the present invention, an inorganic sol is prepared by using cerium nitrate and sodium hydroxide as raw materials, and then the inorganic sol is added to a zirconium dioxide dispersion while stirring, and the inorganic sol is dried and sintered at high temperature in sequence after heat preservation reaction, so as to obtain an inorganic substrate with zirconium dioxide as a core and nano-cerium oxide as a shell layer. Since a dense nano-cerium oxide film layer is deposited on the surface of zirconium dioxide as a shell layer, the zirconium dioxide is put into xylene, ultrasonically dispersed uniformly, and then 3-aminopropyltrimethoxysilane is added and refluxed under the protection of nitrogen, so that the 3-aminopropyltrimethoxysilane reacts chemically with the active groups on the surface of the nano-cerium oxide in the shell layer to bond, and finally a pre-treated inorganic substrate is prepared.
[0016] The pretreated inorganic substrate is put into anhydrous ethanol and tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] pentaerythritol ester is added, mixed and stirred evenly, and then the mixture is kept warm for reaction. Finally, tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] pentaerythritol ester is grafted on the cerium dioxide shell layer under the bridge action of 3-aminopropyltrimethoxysilane, and a dense three-dimensional network structure of the antioxidant film layer is formed on its surface. After the reaction is completed, the resulting components are filtered, washed and vacuum dried in turn to obtain the functional additive. Since the core of the functional additive is zirconium dioxide, it has good high temperature resistance; furthermore, the nano cerium oxide shell layer itself has good high temperature performance and UV resistance, and the core-shell structure formed by the synergistic cooperation between the nano cerium oxide shell layer and the zirconium dioxide in the core further improves the high temperature resistance of the functional additive. In addition, the synergy between the nano-cerium dioxide shell and [β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] pentaerythritol ester significantly improved the anti-ultraviolet and aging resistance of the functional additive. Using it as a raw material makes the prepared coating not only have excellent high temperature resistance, but also has good light retention performance, which extends its service life to a certain extent while effectively ensuring its quality. DETAILED DESCRIPTION
[0017] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0018] Example 1 A high-temperature resistant powder coating with gloss-retaining properties is composed of the following raw materials in parts by weight: 20 parts of acrylic resin, 15 parts of silicone resin, 7 parts of isophorone diisocyanate, 0.5 parts of benzoic acid ketone, 8 parts of functional additives, 20 parts of barium sulfate, 0.5 parts of leveling agent GLP388, 0.8 parts of TP-39 defoaming agent, 2 parts of cobalt blue and 0.8 parts of triphenyl phosphite; wherein the acid value of the acrylic resin is 7 mgKOH / g; the silicone resin is SH-1068 solid silicone resin.
[0019] The preparation method of the functional additive comprises the following steps: The first step is to put the inorganic substrate into xylene at a solid-liquid ratio of 5g / L, and after ultrasonic dispersion for 50 minutes, add 3-aminopropyltrimethoxysilane with a mass 1.5 times that of the inorganic substrate, mix and stir evenly, and reflux for 8 hours under the protection of nitrogen; after the reaction is completed, filter the product components in turn, wash with alcohol and vacuum dry, and the obtained pretreated inorganic substrate is stored and used; In the second step, the pretreated inorganic substrate is put into anhydrous ethanol at a solid-liquid ratio of 0.02 g / mL, and pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] in an amount twice the mass of the pretreated inorganic substrate is added thereto, the mixture is stirred evenly, and the mixture is kept warm at 50°C for 40 hours; after the reaction is completed, the resulting components are filtered, the filter cake is washed three times with anhydrous ethanol, and then vacuum dried at 60°C, and the final product is the functional additive.
[0020] The method for preparing the inorganic substrate comprises the following steps: Step 1, adjusting the pH of 0.3wt% sodium polyacrylate aqueous solution to 4.3, then adding zirconium dioxide with a mass of 40% of the sodium polyacrylate aqueous solution and a particle size of 2 μm, mixing and stirring evenly, and then ball milling and dispersing for 25 hours, and the obtained zirconium dioxide dispersion is stored for standby use; Step 2: Add 8% of the mass of inorganic sol to the zirconium dioxide dispersion while stirring. After the addition is completed, continue stirring for 6 hours and then raise the temperature to 80°C. After stirring and drying, dry the obtained solid material at 220°C for 5 hours; after drying, heat treat it at 700°C for 7 hours; the solid material after heat treatment is naturally cooled to room temperature, and then ground and sieved through a 250-mesh sieve to obtain an inorganic substrate.
[0021] The preparation method of the inorganic sol comprises the following steps: dropping a 0.01 g / mL cerium nitrate aqueous solution into a 3M sodium hydroxide aqueous solution, adjusting the pH to 10.5 after precipitation is complete, mixing and stirring for 3 hours and filtering, washing the obtained filter cake until there is no nitrate ion, adjusting the pH to 0.8, stirring at 30°C for 4 hours, and then stirring at 50°C for 20 hours, cooling the obtained colloid immediately, and then removing the impurity ions therein by dialysis, and finally obtaining the inorganic sol.
[0022] A method for producing a high-temperature resistant powder coating with gloss-retaining properties comprises the following steps: accurately weighing each raw material according to the formula amount and pouring each raw material into a high-speed mixing agitator, fully mixing for 10 minutes, transferring the obtained mixture into an extruder, and after melt extrusion, passing through a tabletting roller to cool the tablet, and then successively crushing, pulverizing and sieving to obtain a high-temperature resistant powder coating with gloss-retaining properties.
[0023] Example 2 The production method of a high temperature resistant powder coating with gloss retention performance provided in this embodiment is basically the same as that in Example 1, except that the specific composition of the raw materials used and the preparation method of the functional additives are not completely the same, and the specific composition of the raw materials used in this embodiment and the preparation method of the functional additives are as follows: A high-temperature resistant powder coating with gloss-retaining properties is composed of the following raw materials in parts by weight: 40 parts of acrylic resin, 25 parts of silicone resin, 10 parts of isophorone diisocyanate, 0.8 parts of benzoic acid ketone, 12 parts of functional additives, 35 parts of titanium dioxide, 1.5 parts of leveling agent GLP588, 2.0 parts of polyoxyethylene polyoxypropanolamine ether defoaming agent, 4 parts of cobalt green and 1.2 parts of 2,6-di-tert-butyl-p-cresol; wherein the acid value of the acrylic resin is 8 mgKOH / g; the silicone resin is German Wacker silicone resin SILRES-610.
[0024] The preparation method of the functional additive comprises the following steps: The first step is to put the inorganic substrate into xylene at a solid-liquid ratio of 6g / L, and after ultrasonic dispersion for 60 minutes, add 3-aminopropyltrimethoxysilane with a mass 1.5 times that of the inorganic substrate, mix and stir evenly, and reflux for 10 hours under the protection of nitrogen; after the reaction is completed, filter, wash with alcohol and vacuum dry the resultant components in turn, and store the obtained pretreated inorganic substrate for standby use; In the second step, the pretreated inorganic substrate is put into anhydrous ethanol at a solid-liquid ratio of 0.03 g / mL, and pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] in an amount 2.5 times the mass of the pretreated inorganic substrate is added thereto. After mixing and stirring evenly, the mixture is kept warm at 55°C for 45 hours. After the reaction is completed, the resulting components are filtered, the filter cake is washed 4 times with anhydrous ethanol and then vacuum dried at 65°C. The final product is the functional additive.
[0025] The method for preparing the inorganic substrate comprises the following steps: Step 1, adjusting the pH of a 0.5wt% sodium polyacrylate aqueous solution to 4.5, then adding zirconium dioxide having a particle size of 3 μm and a mass of 50% of the sodium polyacrylate aqueous solution, mixing and stirring evenly, and then ball milling and dispersing for 30 hours, and the obtained zirconium dioxide dispersion is stored for standby use; Step 2: Add 12% of the mass of inorganic sol to the zirconium dioxide dispersion while stirring. After the addition is completed, continue stirring for 8 hours and then raise the temperature to 80°C. After stirring and drying, dry the obtained solid material at 230°C for 6 hours; after drying, heat treat it at 800°C for 8 hours; the solid material after heat treatment is naturally cooled to room temperature, and then ground and sieved through a 250-mesh sieve to obtain an inorganic substrate.
[0026] The preparation method of the inorganic sol comprises the following steps: dropping a 0.015 g / mL cerium nitrate aqueous solution into a 4M sodium hydroxide aqueous solution, adjusting the pH to 11 after precipitation is complete, mixing and stirring for 4 hours and filtering, washing the obtained filter cake until there is no nitrate ion, adjusting the pH to 1.0, stirring at 35°C for 5 hours, and then stirring at 60°C for 20 hours, cooling the obtained colloid immediately, and then removing the impurity ions therein by dialysis, and finally obtaining the inorganic sol.
[0027] Example 3 The production method of a high temperature resistant powder coating with gloss retention performance provided in this embodiment is basically the same as that in Example 1, except that the specific composition of the raw materials used and the preparation method of the functional additives are not completely the same, and the specific composition of the raw materials used in this embodiment and the preparation method of the functional additives are as follows: A high temperature resistant powder coating with gloss retention performance is composed of the following raw materials in parts by weight: 60 parts of acrylic resin, 40 parts of silicone resin, 15 parts of isophorone diisocyanate, 1.2 parts of benzoic acid ketone, 15 parts of functional additives, 45 parts of talc, 2.5 parts of leveling agent GLP788, 3.5 parts of polydimethylsiloxane, 6 parts of cobalt blue and 1.5 parts of antioxidant 1076; wherein the acid value of the acrylic resin is 10 mgKOH / g; the silicone resin is SH-1068 solid silicone resin.
[0028] The preparation method of the functional additive comprises the following steps: The first step is to put the inorganic substrate into xylene at a solid-liquid ratio of 8g / L, and after ultrasonic dispersion for 70 minutes, add 3-aminopropyltrimethoxysilane with a mass 2.0 times that of the inorganic substrate, mix and stir evenly, and reflux for 12 hours under the protection of nitrogen; after the reaction is completed, filter, wash with alcohol and vacuum dry the resulting components in turn, and store the obtained pretreated inorganic substrate for standby use; In the second step, the pretreated inorganic substrate is put into anhydrous ethanol at a solid-liquid ratio of 0.05 g / mL, and pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] in an amount 3 times the mass of the pretreated inorganic substrate is added thereto. After mixing and stirring evenly, the mixture is kept warm at 60°C for 50 hours. After the reaction is completed, the resulting components are filtered, the filter cake is washed 5 times with anhydrous ethanol and then vacuum dried at 70°C. The final product is the functional additive.
[0029] The method for preparing the inorganic substrate comprises the following steps: Step 1, adjusting the pH of a 0.6wt% sodium polyacrylate aqueous solution to 4.8, then adding zirconium dioxide having a mass of 60% of the sodium polyacrylate aqueous solution and a particle size of 5 μm, mixing and stirring evenly, and then ball milling and dispersing for 35 hours, and the obtained zirconium dioxide dispersion is stored for standby use; Step 2: Add 15% of the mass of inorganic sol to the zirconium dioxide dispersion while stirring. After the addition is completed, continue stirring for 10 hours and then raise the temperature to 85°C. After stirring and drying, dry the obtained solid material at 240°C for 8 hours; after drying, heat treat it at 900°C for 10 hours; the solid material after heat treatment is naturally cooled to room temperature, and then ground and sieved through a 250-mesh sieve to obtain an inorganic substrate.
[0030] The preparation method of the inorganic sol comprises the following steps: dropping a 0.02 g / mL cerium nitrate aqueous solution into a 5M sodium hydroxide aqueous solution, adjusting the pH to 11.5 after precipitation is complete, mixing and stirring for 5 hours and filtering, washing the obtained filter cake until there is no nitrate ion, adjusting the pH to 1.5, stirring at 40°C for 6 hours, and then stirring at 70°C for 25 hours, cooling the obtained colloid immediately, and then removing the impurity ions therein by dialysis, and finally obtaining the inorganic sol.
[0031] Comparative Example 1: The main difference between this example and Example 1 is that an equal amount of inorganic base material is used to replace the functional additive in this example.
[0032] Comparative Example 2: The main difference between this example and Example 1 is that in this example, zirconium dioxide with an equal particle size of 2 μm is used to replace the functional additive.
[0033] Performance Testing The high temperature resistant powder coating samples produced in Examples 1 to 3 and Comparative Examples 1 to 2 were sprayed on aluminum sheets and placed in an oven and cured at 165° C. for 3 h. The coating thickness after curing was 68±0.5 μm. The coatings on each group of aluminum sheets were then subjected to the following performance tests: 1. Test method of water contact angle: The water contact angle of each group of test sample coatings was tested using the method described in GB / T 30693-2014.
[0034] 2. Gloss retention test: The initial gloss (60°) test was performed on the coating of each group of test samples, and the test result was recorded as A0; then the coating of each group of test samples was heat-treated at 320°C for 4 hours. After the treatment, the gloss (60°) test was performed on them respectively, and the test result was recorded as A1. Finally, the gloss retention of the coating of each group of test samples was calculated by the following formula: Gloss retention = (A1 / A0) × 100%; among which, the gloss test steps refer to the test method recorded in ASTM D 523.
[0035] The test data obtained are recorded in the following table:
[0036] By comparing and analyzing the relevant data in the table, it can be seen that the powder coating produced by the present invention not only has excellent high temperature resistance, but also has good gloss retention performance, which prolongs its service life to a certain extent and also effectively guarantees its quality. This shows that the high temperature resistant powder coating with gloss retention performance and the production method thereof provided by the present invention have a broader market prospect and are more suitable for promotion.
[0037] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0038] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A high temperature resistant powder coating with gloss retention performance, characterized in that: The invention is composed of the following raw materials in parts by weight: 20 to 60 parts of acrylic resin, 15 to 40 parts of silicone resin, 7 to 15 parts of isophorone diisocyanate, 0.5 to 1.2 parts of benzoic acid ketone, 8 to 15 parts of functional additives, 20 to 45 parts of inorganic fillers, 0.5 to 2.5 parts of leveling agents, 0.8 to 3.5 parts of defoaming agents, 2 to 6 parts of pigments and 0.8 to 1.5 parts of antioxidants; The acid value of the acrylic resin is 7-10 mgKOH / g; the silicone resin is SH-1068 solid silicone resin or German Wacker silicone resin SILRES-610.
2. The high temperature resistant powder coating with gloss retention performance according to claim 1, characterized in that: The preparation method of the functional additive comprises the following steps: The first step is to put the inorganic substrate into xylene at a solid-liquid ratio of 5 to 8 g / L, and ultrasonically disperse it for 50 to 70 minutes, then add 3-aminopropyltrimethoxysilane with a mass of 1.5 to 2.0 times that of the inorganic substrate, mix and stir evenly, and reflux for 8 to 12 hours under the protection of nitrogen; after the reaction is completed, filter the product components, wash with alcohol, and vacuum dry them in turn, and the obtained pretreated inorganic substrate is stored and used; The second step is to put the pretreated inorganic substrate into anhydrous ethanol at a solid-liquid ratio of 0.02 to 0.05 g / mL, and add pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] in an amount 2 to 3 times the mass of the pretreated inorganic substrate, mix and stir evenly, and then keep the mixture at a temperature of 50 to 60°C for 40 to 50 hours; after the reaction is completed, filter the resulting components, wash the filter cake with anhydrous ethanol for 3 to 5 times, and then vacuum dry it at a temperature of 60 to 70°C, and the final product is the functional additive.
3. The high temperature resistant powder coating with gloss retention performance according to claim 2, characterized in that: The method for preparing the inorganic substrate comprises the following steps: Step 1, adjusting the pH of 0.3-0.6wt% sodium polyacrylate aqueous solution to 4.3-4.8, then adding zirconium dioxide with a mass of 40-60% of the sodium polyacrylate aqueous solution and a particle size of 2-5 μm, mixing and stirring evenly, and then ball milling and dispersing for 25-35 hours, and the obtained zirconium dioxide dispersion is stored and used for standby; Step 2: Add 8-15% of the mass of inorganic sol to the zirconium dioxide dispersion while stirring. After the addition is completed, continue stirring for 6-10 hours and then raise the temperature to 80-85°C. After stirring and drying, dry the obtained solid material at 220-240°C for 5-8h; after drying, heat treat it at 700-900°C for 7-10h; the solid material after heat treatment is naturally cooled to room temperature, and then ground and sieved through a 250-mesh sieve to obtain an inorganic substrate.
4. The high temperature resistant powder coating with gloss retention performance according to claim 3, characterized in that: The preparation method of the inorganic sol comprises the following steps: dropping 0.01-0.02 g / mL of cerium nitrate aqueous solution into 3-5 M sodium hydroxide aqueous solution, adjusting the pH to 10.5-11.5 after precipitation is complete, mixing and stirring for 3-5 hours and filtering, washing the obtained filter cake until there is no nitrate ion, adjusting the pH to 0.8-1.5, stirring at 30-40° C. for 4-6 hours, and then stirring at 50-70° C. for 20-25 hours, cooling the obtained colloid immediately, and then removing the impurity ions therein by dialysis, and finally obtaining the inorganic sol.
5. The high temperature resistant powder coating with gloss retention performance according to claim 1, characterized in that: The inorganic filler is selected from any one of barium sulfate, titanium dioxide and talcum powder.
6. The high temperature resistant powder coating with gloss retention performance according to claim 1, characterized in that: The leveling agent is selected from any one of leveling agent GLP388, leveling agent GLP588, and leveling agent GLP788.
7. The high temperature resistant powder coating with gloss retention performance according to claim 1, characterized in that: The defoamer is selected from any one of TP-39 defoamer, polyoxyethylene polyoxypropanolamine ether defoamer and polydimethylsiloxane.
8. The high temperature resistant powder coating with gloss retention performance according to claim 1, characterized in that: The pigment is selected from any one of cobalt blue and cobalt green.
9. The high temperature resistant powder coating with gloss retention performance according to claim 1, characterized in that: The antioxidant is selected from any one of triphenyl phosphite, 2,6-di-tert-butyl-p-cresol, antioxidant 1076, and antioxidant 1010.
10. A method for producing a high temperature resistant powder coating with gloss retention performance according to any one of claims 1 to 9, characterized in that: The method comprises the following steps: accurately weighing each raw material according to the formula amount and pouring each raw material into a high-speed mixing stirrer, fully mixing for 10 to 15 minutes, transferring the obtained mixture into an extruder, and after melt extrusion, passing through a sheeting roller to cool the sheet, and then successively crushing, pulverizing and sieving to obtain a high-temperature resistant powder coating with gloss-retaining performance.
Citation Information
Patent Citations
High-viscosity powder coating as well as preparation method and application thereof
CN116004121A
Heat-insulation anti-ultraviolet automobile membrane and preparation method thereof
CN105348750A
Weather resistant high-temperature powder coating and production process thereof
CN108977061A
High-temperature-resistant powder coating composition and product
CN113088184A
Silicane modified polyurethane cementing sealing glue and method for making same
CN1594480A