Temperature control process for homogeneous heat treatment of large forgings

By finely controlling the heating, insulation and cooling processes of large forgings and using step heating and multi-stage cooling processes, the cooling rate and temperature difference problems in the heat treatment of forgings are solved, residual stress is significantly reduced, and the overall performance and service life of forgings are improved.

CN118854014APending Publication Date: 2024-10-29WUXI YITONG PRECISION MACHINERY
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410922744.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

During the heat treatment process of large forgings, the cooling rate is difficult to meet the requirements, resulting in a large temperature difference between the surface and the core, which easily causes thermal stress and cracking problems.

Method used

Using step heating and multi-stage cooling processes, residual stress is reduced by finely controlling the temperature and time in the heating, insulation and cooling processes, including step heating, sufficient insulation, rapid quenching and multi-stage air-cooling and water-cooling alternating treatment, and through optimized return The fire process avoids temper brittleness.

Benefits of technology

It effectively improves the uniformity of the internal structure of the forging, reduces residual stress, and improves the overall quality and service life of the forging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118854014A_ABST
    Figure CN118854014A_ABST
Patent Text Reader

Abstract

The invention discloses a temperature control process for homogeneous heat treatment of a large forge piece, which comprises the following steps: step temperature rise: starting from room temperature, firstly raising the temperature of the forge piece to 430-450 DEG C at a speed of 30-70 DEG C / h, and preserving heat to reduce the temperature difference of the forge piece in a blue brittle temperature range and prevent the forge piece from cracking caused by overlarge thermal stress; the temperature is increased to 620-670 DEG C at the speed of 100-150 DEG C / h, heat preservation is conducted, and the temperature difference between the surface and the core of the forge piece is further reduced; high-temperature heating is conducted, specifically, the forge piece is heated to 830-870 DEG C and subjected to heat preservation; the method has the beneficial effects that the uniformity of the internal structure of the large forge piece is effectively improved through the measures of stepped heating, sufficient heat preservation and multi-stage cooling; through reasonable heating and cooling speed control, the residual stress generated in the heat treatment process of the forge piece is obviously reduced; an optimized tempering process is adopted, so that the occurrence of tempering brittleness is effectively avoided, and the toughness of the forge piece is improved; the overall heat treatment process is optimized, so that the comprehensive mechanical property and the service life of the large forge piece are remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of heat treatment of forgings, and in particular relates to a temperature control process for homogenous heat treatment of large forgings. Background Art

[0002] In actual production, most large forgings are forged and then hot-charged in a furnace for normalizing and tempering. Forgings that are air-cooled after forging can only be cold-charged in a furnace for normalizing and tempering. The purpose of supercooling after normalizing is to reduce the center temperature of the forging, and to make the temperature uniform through proper insulation, which can also play a role in removing hydrogen. The supercooling temperature varies with different steel types. Generally, the hot-charged furnace is 350-400℃ or 400-450℃, and the cold-charged furnace is 300-450℃.

[0003] In order to avoid the production of coarse products in high-temperature forgings, attention should also be paid to the coarse grains of high-temperature forgings during forging processing. The raw materials and each link in the forging process are related. Therefore, in order to ensure the stable quality of forgings, the process preparation should be detailed and correct, and the execution of the process should be strict and accurate; important forgings of high-temperature alloys should be die forged even if they are produced in small quantities.

[0004] For high-temperature forgings of the same grade but with different smelting methods and furnace numbers, the actual recrystallization temperature and the aggregate recrystallization temperature are often different due to the difference in the actual content of chemical composition.

[0005] The patent discloses a homogenization heat treatment process for disc energy storage forgings with publication number CN115323127A, which includes: heating the forgings to 640-660°C and keeping them warm for 1 hour; heating the forgings to 870-910°C, keeping them warm for 3 hours, then taking them out of the furnace, and air cooling them to below 300°C; putting the forgings into the furnace, heating them to 570-610°C, tempering them for 12 hours, then taking them out of the furnace, and air cooling them to below 350°C; putting the forgings into the furnace, heating them to 830-870°C, and keeping them warm for 4 hours; taking them out of the furnace, performing the first air cooling treatment for 1 minute, the first water cooling treatment for 5 minutes, the second air cooling treatment for 1.5 minutes, the second water cooling treatment for 3 minutes, the third air cooling treatment for 1.5 minutes, the third water cooling treatment for 3 minutes, and then air cooling them to below 200-350°C; putting the forgings into the furnace for tempering, heating them to 590-610°C, keeping them warm for 12 hours, then taking them out of the furnace, and air cooling them to room temperature.

[0006] In the prior art, although the homogeneity of forgings has been improved to a certain extent, when processing large forgings, there are still problems such as difficulty in meeting the cooling speed requirements, large temperature difference between the surface and the core, and easy generation of thermal stress leading to cracking. Summary of the invention

[0007] The purpose of the present invention is to provide a temperature control process for homogenous heat treatment of large forgings, which can achieve homogenization of the internal structure of the forgings by finely controlling the temperature and time during heating, insulation, cooling and tempering, while effectively reducing residual stress and tempering brittleness, and improving the overall quality and service life of the forgings.

[0008] To achieve the above object, the present invention provides the following technical solution: a temperature control process for homogenous heat treatment of large forgings, the process method is as follows:

[0009] Heating phase:

[0010] Step heating: Starting from room temperature, the forging is first heated to 430-450℃ at a rate of 30-70℃ / h and kept warm to reduce the temperature difference of the forging within the blue brittle temperature range and prevent cracking caused by excessive thermal stress;

[0011] Continue heating: heat up to 620-670℃ at a rate of 100-150℃ / h and keep warm to further reduce the temperature difference between the surface and the core of the forging;

[0012] High temperature heating: raise the temperature of the forging to 830-870℃ and keep it warm to ensure that the forging is fully austenitized;

[0013] Quenching and cooling stage:

[0014] Quenching treatment: After keeping at 830-870℃, cooling is carried out by rapid quenching to obtain the required martensitic structure;

[0015] Multi-stage cooling: Multi-stage air cooling and water cooling are carried out alternately until the forging temperature drops to 180-320℃ to refine the structure and reduce residual stress;

[0016] Tempering stage:

[0017] Low temperature tempering: The forgings are put back into the furnace for the first tempering to eliminate quenching stress and avoid temper brittleness;

[0018] Temperature uniformity treatment: Extend the holding time to ensure uniform temperature inside and outside the forging;

[0019] Cooling after furnace removal: After tempering, the forgings are removed from the furnace and naturally cooled to room temperature.

[0020] As a preferred technical solution of the present invention, step heating: starting from room temperature, the forging is first heated to 430-450°C at a rate of 30-70°C / h, and kept warm for 1-2h.

[0021] As a preferred technical solution of the present invention, the temperature is continued to be raised: the temperature is raised to 620-670°C at a rate of 100-150°C / h, and kept at this temperature for 2-3h.

[0022] As a preferred technical solution of the present invention, high temperature heating: the forging is heated to 830-870°C and kept warm for 3-5 hours.

[0023] As a preferred technical solution of the present invention, the rapid quenching method is one of oil quenching and water quenching.

[0024] As a preferred technical solution of the present invention, multi-stage air cooling and water cooling are performed alternately, including first air cooling for 1-2 minutes, first water cooling for 2-4 minutes, second air cooling for 1-2 minutes, and second water cooling for 3-5 minutes.

[0025] As a preferred technical solution of the present invention, low temperature tempering: the forging is put back into the furnace, the temperature is raised to 570-580°C at a rate of 40-90°C / h, and the temperature is kept for 10-16h.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] Through step-by-step heating, sufficient heat preservation and multi-stage cooling measures, the uniformity of the internal structure of large forgings is effectively improved;

[0028] Reasonable heating and cooling rate control significantly reduces the residual stress generated in the forging during heat treatment;

[0029] The optimized tempering process is adopted to effectively avoid the occurrence of temper brittleness and improve the toughness of forgings;

[0030] The optimization of the overall heat treatment process has significantly improved the comprehensive mechanical properties and service life of large forgings. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION

[0032] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0033] Example 1

[0034] See also Figure 1 , which is the first embodiment of the present invention, provides a temperature control process for homogenous heat treatment of large forgings, comprising the following steps:

[0035] Heating phase:

[0036] Step heating: Starting from room temperature, the forging is first heated to 430℃ at a rate of 30℃ / h and kept at this temperature for 1h to reduce the temperature difference of the forging within the blue brittle temperature range and prevent cracking caused by excessive thermal stress;

[0037] Continue heating: heat up to 620℃ at a rate of 100℃ / h and keep warm for 2h to further reduce the temperature difference between the surface and the core of the forging;

[0038] High temperature heating: raise the temperature of the forging to 830℃ and keep it at this temperature for 3 hours to ensure that the forging is fully austenitized;

[0039] Quenching and cooling stage:

[0040] Quenching treatment: After keeping at 830℃, cooling is carried out by rapid quenching, and the rapid quenching method is oil quenching to obtain the required martensitic structure;

[0041] Multi-stage cooling: Perform multi-stage air cooling and water cooling alternately, including the first air cooling for 1 minute, the first water cooling for 2 minutes, the second air cooling for 1 minute, and the second water cooling for 3 minutes, until the forging temperature drops to 180°C, so as to refine the structure and reduce the residual stress;

[0042] Tempering stage:

[0043] Low temperature tempering: The forgings are put back into the furnace and heated to 570℃ at a rate of 40℃ / h, kept at this temperature for 10h for the first tempering to eliminate quenching stress and avoid temper brittleness;

[0044] Temperature uniformity treatment: Extend the holding time to ensure uniform temperature inside and outside the forging;

[0045] Cooling after furnace removal: After tempering, the forgings are removed from the furnace and naturally cooled to room temperature.

[0046] Through step-by-step heating, sufficient heat preservation and multi-stage cooling measures, the uniformity of the internal structure of large forgings is effectively improved;

[0047] Reasonable heating and cooling rate control significantly reduces the residual stress generated in the forging during heat treatment;

[0048] The optimized tempering process is adopted to effectively avoid the occurrence of temper brittleness and improve the toughness of forgings.

[0049] Example 2

[0050] See also Figure 1 , which is the second embodiment of the present invention, provides a temperature control process for homogenous heat treatment of large forgings, comprising the following steps:

[0051] Heating phase:

[0052] Step heating: Starting from room temperature, the forging is first heated to 440°C at a rate of 50°C / h and kept at this temperature for 1.5 hours to reduce the temperature difference of the forging within the blue brittle temperature range and prevent cracking caused by excessive thermal stress;

[0053] Continue heating: heat up to 645℃ at a rate of 125℃ / h and keep warm for 2.5h to further reduce the temperature difference between the surface and the core of the forging;

[0054] High temperature heating: raise the temperature of the forging to 850℃ and keep it at this temperature for 4 hours to ensure that the forging is fully austenitized;

[0055] Quenching and cooling stage:

[0056] Quenching treatment: After keeping at 850℃, cooling is carried out by rapid quenching, which is one of oil quenching and water quenching, to obtain the required martensitic structure;

[0057] Multi-stage cooling: Multi-stage air cooling and water cooling are carried out alternately, including the first air cooling for 1.5 minutes, the first water cooling for 3 minutes, the second air cooling for 1.5 minutes, and the second water cooling for 4 minutes, until the forging temperature drops to 250°C, so as to refine the structure and reduce the residual stress;

[0058] Tempering stage:

[0059] Low temperature tempering: The forgings are put back into the furnace and heated to 575℃ at a rate of 65℃ / h, kept at this temperature for 13h for the first tempering to eliminate quenching stress and avoid temper brittleness;

[0060] Temperature uniformity treatment: Extend the holding time to ensure uniform temperature inside and outside the forging;

[0061] Cooling after furnace removal: After tempering, the forgings are removed from the furnace and naturally cooled to room temperature.

[0062] Through step-by-step heating, sufficient heat preservation and multi-stage cooling measures, the uniformity of the internal structure of large forgings is effectively improved;

[0063] Reasonable heating and cooling rate control significantly reduces the residual stress generated in the forging during heat treatment;

[0064] The optimized tempering process is adopted to effectively avoid the occurrence of temper brittleness and improve the toughness of forgings.

[0065] Example 3

[0066] See also Figure 1 , which is the third embodiment of the present invention, provides a temperature control process for homogenous heat treatment of large forgings, comprising the following steps:

[0067] Heating phase:

[0068] Step heating: Starting from room temperature, the forging is first heated to 450℃ at a rate of 70℃ / h and kept at this temperature for 2h to reduce the temperature difference of the forging within the blue brittle temperature range and prevent cracking caused by excessive thermal stress;

[0069] Continue heating: heat up to 670℃ at a rate of 150℃ / h and keep warm for 3h to further reduce the temperature difference between the forging surface and the core;

[0070] High temperature heating: raise the temperature of the forging to 870℃ and keep it at this temperature for 5 hours to ensure that the forging is fully austenitized;

[0071] Quenching and cooling stage:

[0072] Quenching treatment: After keeping at 870℃, cooling is carried out by rapid quenching, which is one of oil quenching and water quenching, to obtain the required martensitic structure;

[0073] Multi-stage cooling: Multi-stage air cooling and water cooling are carried out alternately, including the first air cooling for 2 minutes, the first water cooling for 4 minutes, the second air cooling for 2 minutes, and the second water cooling for 5 minutes, until the forging temperature drops to 320°C, so as to refine the structure and reduce the residual stress;

[0074] Tempering stage:

[0075] Low temperature tempering: The forgings are put back into the furnace and heated to 580℃ at a rate of 90℃ / h, kept at this temperature for 16h for the first tempering to eliminate quenching stress and avoid temper brittleness;

[0076] Temperature uniformity treatment: Extend the holding time to ensure uniform temperature inside and outside the forging;

[0077] Cooling after furnace removal: After tempering, the forgings are removed from the furnace and naturally cooled to room temperature.

[0078] Through step-by-step heating, sufficient heat preservation and multi-stage cooling measures, the uniformity of the internal structure of large forgings is effectively improved;

[0079] Reasonable heating and cooling rate control significantly reduces the residual stress generated in the forging during heat treatment;

[0080] The optimized tempering process is adopted to effectively avoid the occurrence of temper brittleness and improve the toughness of forgings.

[0081] Although the embodiments of the present invention have been shown and described, as detailed above, it will be understood by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A temperature control process for homogeneous heat treatment of large forgings. Features: The process is as follows: Heating phase: Step heating: Starting from room temperature, the forging is first heated to 430-450℃ at a rate of 30-70℃ / h and kept warm to reduce the temperature difference of the forging within the blue brittle temperature range and prevent cracking caused by excessive thermal stress; Continue heating: heat up to 620-670℃ at a rate of 100-150℃ / h and keep warm to further reduce the temperature difference between the surface and the core of the forging; High temperature heating: raise the temperature of the forging to 830-870℃ and keep it warm to ensure that the forging is fully austenitized; Quenching and cooling stage: Quenching treatment: After keeping at 830-870℃, cooling is carried out by rapid quenching to obtain the required martensitic structure; Multi-stage cooling: Multi-stage air cooling and water cooling are carried out alternately until the forging temperature drops to 180-320℃ to refine the structure and reduce residual stress; Tempering stage: Low temperature tempering: The forgings are put back into the furnace for the first tempering to eliminate quenching stress and avoid temper brittleness; Temperature uniformity treatment: Extend the holding time to ensure uniform temperature inside and outside the forging; Cooling after furnace removal: After tempering, the forgings are removed from the furnace and naturally cooled to room temperature.

2. The temperature control process for homogenous heat treatment of large forgings according to claim 1, Features: Step heating: Starting from room temperature, the forging is first heated to 430-450℃ at a rate of 30-70℃ / h and kept at this temperature for 1-2h.

3. The temperature control process for homogenous heat treatment of large forgings according to claim 1, Features: Continue heating: increase the temperature to 620-670℃ at a rate of 100-150℃ / h and keep warm for 2-3h.

4. The temperature control process for homogenous heat treatment of large forgings according to claim 1, Features: High temperature heating: raise the temperature of the forging to 830-870℃ and keep it warm for 3-5h.

5. The temperature control process for homogenous heat treatment of large forgings according to claim 1, Features: The rapid quenching method is one of oil quenching and water quenching.

6. The temperature control process for homogenous heat treatment of large forgings according to claim 1, Features: Multi-stage air cooling and water cooling are performed alternately, including the first air cooling for 1-2 minutes, the first water cooling for 2-4 minutes, the second air cooling for 1-2 minutes, and the second water cooling for 3-5 minutes.

7. The temperature control process for homogenous heat treatment of large forgings according to claim 1, Features: Low temperature tempering: The forgings are put back into the furnace and heated to 570-580℃ at a rate of 40-90℃ / h and kept at this temperature for 10-16h.

Citation Information

Cited By

  • Irregular metal forge piece heat treatment method and system

    CN120758729A

  • A method and system for heat treating irregular metal forgings

    CN120758729B