Anti-ultraviolet light conversion yarn, fabric and preparation method
By using melt-spun yarns with light-converting agents such as rare earth chlorides and UV-reflecting agents such as kaolin in textiles, the problem that the anti-UV coating of existing anti-UV fabrics is easy to fall off is solved, and efficient anti-UV performance and durability are achieved. Washability meets the higher protection needs of modern clothing.
Patent Information
- Application Number
- CN202410816838.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-10-29
AI Technical Summary
The anti-UV coating of existing anti-UV fabrics is easily affected by washing and friction, resulting in reduced anti-UV performance and cannot meet the higher protection needs of modern clothing.
It uses anti-UV light conversion yarn made of chemical fiber-based light conversion masterbatch through melt spinning. The yarn contains rare earth chlorides, rare earth carboxylate complexes, rare earth ketone complexes and phycocyanin as light conversion agents. , combined with kaolin, calcium carbonate, talc, iron oxide, zinc oxide and titanium oxide as UV reflectors to form yarns with round and/or special-shaped cross sections, which are woven into fabrics to achieve UV resistance.
It realizes that the textiles have good washing resistance and breathability without reducing the anti-UV performance, enhances the anti-UV effect of the fabric, and avoids the complexity of constructing multi-layer fabrics.
Smart Images

Figure BDA0004907924540000091 
Figure HDA0004907924550000011 
Figure HDA0004907924550000021
Abstract
Description
Technical Field
[0001] The invention belongs to the field of textiles, and in particular relates to an anti-ultraviolet light-converting yarn and fabric, and a preparation method. Background Art
[0002] When people are outdoors, they are inevitably exposed to the sun. However, the ultraviolet rays in the sun are harmful to human skin. Therefore, avoiding the harm of ultraviolet rays to humans is a very worthy research topic. Among them, the use of textile products such as anti-ultraviolet clothing is one of the effective protection methods. However, few existing fabrics have excellent anti-ultraviolet function and can no longer meet the higher requirements of modern clothing. Therefore, it is very necessary to develop an effective anti-ultraviolet fabric.
[0003] In the prior art, a Chinese patent document with the announcement number CN 210062252 U discloses an anti-ultraviolet fabric, which includes a fabric body, an outer wear-resistant layer, a base layer and an inner layer, wherein the fabric body is composed of a base layer, an outer wear-resistant layer sewn on the upper surface of the base layer and an inner layer sewn on the lower surface of the base layer, an anti-ultraviolet coating is applied on the upper surface of the outer wear-resistant layer, the wear-resistant layer is made of a blend of polyester and nylon, and the base layer is composed of a heat insulation layer, an anti-static layer and a sweat-absorbing cotton layer. Among them, an anti-ultraviolet coating is applied on the outer wear-resistant layer to provide an anti-ultraviolet effect; the fabric body is composed of a base layer, an outer wear-resistant layer sewn on the upper surface of the base layer and an inner layer sewn on the lower surface of the base layer, the inner layer is a breathable mesh layer, breathable holes are provided on the base layer, and a sweat-absorbing cotton layer is provided in the base layer, and breathable holes are provided on the thicker base layer to cooperate with the inner layer of the breathable mesh layer, thereby improving the breathability and heat dissipation of the anti-ultraviolet fabric.
[0004] However, the anti-ultraviolet coating of the above anti-ultraviolet fabric will be greatly affected by washing and friction, and is easy to fall off, affecting its anti-ultraviolet performance. Summary of the invention
[0005] In order to solve the technical problems existing in the above-mentioned prior art, the present invention provides an anti-ultraviolet light-converting yarn and fabric, and a preparation method. The fabric made of the yarn of the present invention can effectively achieve anti-ultraviolet function and has good washing resistance, etc.
[0006] The present invention provides an anti-ultraviolet light-converting yarn, which is formed by melt spinning and weaving chemical fiber-based light-converting masterbatch; the chemical fiber-based light-converting masterbatch comprises a chemical fiber substrate, a light-converting agent and an ultraviolet reflector, the light-converting agent is one or more of rare earth chloride, rare earth carboxylate complex, rare earth ketone complex and phycocyanin; the ultraviolet reflector is one or more of kaolin, calcium carbonate, talc, iron oxide, zinc oxide and titanium oxide;
[0007] The single fiber of the anti-ultraviolet light-converting yarn has a round and / or a special-shaped cross section.
[0008] In an embodiment of the present invention, the mass percentage of the light conversion agent in the anti-ultraviolet light conversion yarn is 0.5% to 3%.
[0009] In an embodiment of the present invention, the chemical fiber substrate is polyester and / or nylon; the light conversion agent is CaS:Eu,Cl and / or Eu(TTA)3(TPPO)2.
[0010] In an embodiment of the present invention, the single fiber of the anti-ultraviolet light conversion yarn has a special-shaped cross-section, and the special-shaped cross-section is a flat cross-section, a polygonal cross-section or a gear-shaped cross-section.
[0011] The present invention provides a method for preparing an anti-ultraviolet light-converting yarn, comprising the following steps:
[0012] Provided is a chemical fiber-based light conversion masterbatch, wherein the chemical fiber-based light conversion masterbatch comprises a chemical fiber substrate, a light conversion agent and an ultraviolet reflector, wherein the light conversion agent is one or more of rare earth chlorides, rare earth carboxylate complexes, rare earth ketone complexes and phycocyanin; and the ultraviolet reflector is one or more of kaolin, calcium carbonate, talc, iron oxide, zinc oxide and titanium oxide;
[0013] The chemical fiber-based light-converting masterbatch is melt-spun through a spinning spinneret assembly to obtain a plurality of anti-ultraviolet light-converting fibers, which are then woven into anti-ultraviolet light-converting yarns.
[0014] In an embodiment of the present invention, the chemical fiber-based light conversion masterbatch is formed by mixing and granulating chemical fiber substrate slices, a light conversion agent, an ultraviolet reflector, a solvent and a dispersant, and the chemical fiber substrate slices are polyester slices and / or nylon slices.
[0015] In an embodiment of the present invention, the mass percentage of the light conversion agent in the anti-ultraviolet light conversion yarn is 0.5% to 3%; the light conversion agent is CaS:Eu,Cl and / or Eu(TTA)3(TPPO)2.
[0016] In an embodiment of the present invention, the temperature of the melt spinning is 240°C to 300°C.
[0017] The present invention provides a fabric, which is woven from the above-mentioned anti-ultraviolet light-converting yarn.
[0018] In an embodiment of the present invention, the single fiber of the anti-ultraviolet light-converting yarn has a special-shaped cross-section; and the fabric has a plain weave structure.
[0019] Compared with the prior art, the present invention provides a melt-spun chemical fiber yarn containing a light conversion agent and an ultraviolet reflector, wherein the light conversion agent is one or more of rare earth chloride, rare earth carboxylate complex, rare earth ketone complex and phycocyanin; the ultraviolet reflector is one or more of kaolin, calcium carbonate, talcum powder, iron oxide, zinc oxide and titanium oxide. At the same time, the present invention also provides a fabric containing the yarn. The present invention mainly utilizes the specific light conversion material contained in the yarn to convert ultraviolet rays in sunlight into visible light, and combines ultraviolet reflectors and the like to achieve excellent anti-ultraviolet performance of textiles. The fabric finally constructed by the embodiment of the present invention is integrated with the anti-ultraviolet component, so the anti-ultraviolet performance of the fabric will not be significantly reduced due to washing and friction.
[0020] Furthermore, the fabric provided by the present invention itself has anti-ultraviolet properties and does not require the construction of multi-layer fabrics, thereby ensuring air permeability and moisture permeability at the same time.
[0021] Furthermore, the single fiber of the anti-ultraviolet light-converting yarn of the present invention has a special-shaped cross-section, which can cause the ultraviolet light to be diffusely reflected on the surface of the fabric, reduce the fabric penetration, and further enhance the anti-ultraviolet effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0023] Figure 1 The ultraviolet absorption result of the fabric provided in Example 1 of the present invention;
[0024] Figure 2 The excitation spectrum of the fabric provided in Example 1 of the present invention;
[0025] Figure 3 This is the excitation-absorption spectrum of the fabric provided in Example 1 of the present invention. DETAILED DESCRIPTION
[0026] In order to make the purpose, technical solutions and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with embodiments. Unless otherwise defined, all professional terms used hereinafter have the same meaning as those skilled in the art generally understand. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0027] The present invention provides an anti-ultraviolet light-converting yarn, which is formed by melt spinning and weaving chemical fiber-based light-converting masterbatch; the chemical fiber-based light-converting masterbatch comprises a chemical fiber substrate, a light-converting agent and an ultraviolet reflector, the light-converting agent is one or more of rare earth chloride, rare earth carboxylate complex, rare earth ketone complex and phycocyanin; the ultraviolet reflector is one or more of kaolin, calcium carbonate, talc, iron oxide, zinc oxide and titanium oxide;
[0028] The single fiber of the anti-ultraviolet light-converting yarn has a round and / or a special-shaped cross section.
[0029] The fabric made of the yarn provided by the present invention can effectively achieve the anti-ultraviolet function and has good washing resistance and the like.
[0030] The embodiment of the present invention provides a chemical fiber-based light conversion masterbatch containing a light conversion agent and an ultraviolet reflector; wherein the light conversion agent is one or more of rare earth chlorides, rare earth carboxylates, rare earth ketones and phycocyanin, preferably CaS:Eu,Cl and / or Eu(TTA)3(TPPO)2. These light conversion materials can convert ultraviolet light into visible light in the yarn of the present invention. The light conversion system contains unstable ions or π electrons, which are excited to a high energy state after absorbing ultraviolet light. This energy can be transferred to the central ion, causing its electrons to transition from an unstable high energy state back to a stable ground state, that is, to generate transitions between different electron layers, while emitting visible light of a certain wavelength to achieve anti-ultraviolet function.
[0031] In an embodiment of the present invention, the mass percentage of the light-converting agent in the anti-ultraviolet light-converting yarn is preferably 0.5% to 3%, for example, 0.5%, 1%, 1.5%, 2%, or 3%. Some embodiments of the present invention mainly use rare earth materials containing europium elements, so that they can convert ultraviolet rays into harmless visible light that is beneficial to the human body and has a high intensity; among them, there are many methods for preparing rare earth inorganic luminescent materials such as CaS:Eu,Cl, such as a high-temperature solid-phase reaction method. Eu(TTA)3(TPPO)2 is a complex with europium (Eu) as the central ion. Eu(TTA)3 represents tris(2-phenylpyridine-4,6-dione) coordinated to the europium ion, and TPPO is (2,4,6-tris[2-(3-phenylpyrazolyl)]pyrimidine).
[0032] The ultraviolet reflector mainly achieves the anti-ultraviolet function by reflecting and refracting the incident ultraviolet rays, and is generally an inorganic substance such as ceramics and metal oxides. In the present invention, the ultraviolet reflector is one or more of kaolin, calcium carbonate, talcum powder, iron oxide, zinc oxide and titanium oxide, preferably calcium carbonate, zinc oxide and titanium dioxide; it plays a synergistic role with the above-mentioned light conversion agent, etc., to achieve excellent anti-ultraviolet performance of textiles. Specifically, the particle size of the ultraviolet reflector can be 200-500nm; its mass percentage content in the yarn is preferably 0.3%-1.0%.
[0033] The chemical fiber-based light-converting masterbatch described in the embodiment of the present invention is mainly composed of a chemical fiber base material, and the chemical fiber base material is preferably polyester and / or nylon, which has good comprehensive performance. For example, nylon includes nylon 6, nylon 66, and the like.
[0034] In an embodiment of the present invention, the single fiber of the anti-ultraviolet light-converting yarn can have a circular cross section or a special-shaped cross section, and the special-shaped cross section is preferably a flat cross section, a polygonal cross section or a gear-shaped cross section. The fineness of the anti-ultraviolet light-converting yarn in the embodiment of the present invention includes but is not limited to: 70d / 48f, 70d / 36f, 75d / 72f, 75d / 48f, 75d / 36f, 50d / 36f, 50d / 48f, etc.; yarn strength: 3.5-5cN / d; CV value is less than 1%.
[0035] Accordingly, an embodiment of the present invention provides a method for preparing an anti-ultraviolet light-converting yarn, comprising the following steps:
[0036] Provided is a chemical fiber-based light conversion masterbatch, wherein the chemical fiber-based light conversion masterbatch comprises a chemical fiber substrate, a light conversion agent and an ultraviolet reflector, wherein the light conversion agent is one or more of rare earth chlorides, rare earth carboxylate complexes, rare earth ketone complexes and phycocyanin; and the ultraviolet reflector is one or more of kaolin, calcium carbonate, talc, iron oxide, zinc oxide and titanium oxide;
[0037] The chemical fiber-based light-converting masterbatch is melt-spun through a spinning spinneret assembly to obtain a plurality of anti-ultraviolet light-converting fibers, which are then woven into anti-ultraviolet light-converting yarns.
[0038] In the embodiment of the present invention, a chemical fiber-based light conversion masterbatch is first prepared. Preferably, nylon slices or polyester slices, a light conversion agent, an ultraviolet reflector, a solvent and a dispersant are mixed, and the chemical fiber-based light conversion masterbatch is obtained by granulation. Among them, the contents of the light conversion agent and the ultraviolet reflector are as described above; all raw materials are commercially available products. The nylon slices are preferably nylon 6 and nylon 66 slices. The solvent is preferably a mixed solution of ethanol and water; the dispersant is preferably a silane coupling agent (typical silane coupling agents include A151 (vinyl triethoxysilane), A171 (vinyl trimethoxysilane), A172 (vinyl tri (β-methoxyethoxy) silane) and the like). In some embodiments, the specific raw material ratio is: 20 parts of raw materials and 80 parts of polyester / nylon carrier.
[0039] The granulation process described in the embodiment of the present invention specifically includes: fully mixing the dried polyester / nylon powder, the light-converting powder, and the dispersant, and then adding them to a mixture of anhydrous ethanol and deionized water (configuration volume ratio is 9:1), after fully dispersing, placing them in a vacuum oven to dry, and then blending and granulating.
[0040] In some preferred embodiments, the mass percentage of the light conversion agent in the anti-ultraviolet light conversion yarn is 0.5% to 3%; the light conversion agent is CaS:Eu,Cl and / or Eu(TTA)3(TPPO)2.
[0041] After obtaining the chemical fiber-based light-converting masterbatch, the embodiment of the present invention performs melt spinning through a spinning spinneret assembly to obtain a number of UV-resistant light-converting fibers. The spinning spinneret assembly includes a circular or shaped hole spinneret, and the shaped hole spinneret includes but is not limited to flat, flat groove, polygonal, and gear-shaped; the temperature of the melt spinning is preferably 240°C to 300°C, and further 240°C, 250°C, 260°C, 270°C, 280°C, 290°C, 300°C, etc.
[0042] Specifically, the number of spinneret holes involved in the embodiment of the present invention is, for example: 70d / 48f, 70d / 36f, 75d / 72f, 75d / 48f, 75d / 36f, 50d / 36f, 50d / 48f, etc. For polyester spinning, the temperature of each zone can be: 290°C in zones 1, 2 and 3, 280°C in zones 4 and 5, and 32°C in the cooling zone; the spinning speed is preferably 1000m / min. For nylon spinning, the temperature of each zone can be: 240°C in zone 1, 245°C in zone 2, 250°C in zone 3, 255°C in zone 4 and 5, and 30°C in the cooling zone; the spinning speed is 1000m / min. If fully drawn (FDY) yarn is produced, which includes a drawing process, the high-speed winding speed can be 3500m / min. The index parameters of the obtained anti-ultraviolet light conversion fiber are as described above, such as the fineness can be 50~75d / 36~72f.
[0043] In the embodiment of the present invention, the obtained anti-ultraviolet light conversion fiber is woven into yarn, and the yarn weaving method is not particularly limited. In some embodiments, the anti-ultraviolet light conversion yarn single fiber preferably has a special-shaped cross-section, which can make ultraviolet light diffusely reflected on the surface of the fabric, reduce the fabric penetration, and further enhance the anti-ultraviolet effect.
[0044] The embodiment of the present invention further provides a fabric, which is woven from the anti-ultraviolet light-converting yarn described above.
[0045] In an embodiment of the present invention, the fabric has a plain weave structure; the anti-ultraviolet light-converting yarn described above is used as the warp yarn and the weft yarn, and is woven according to the plain weave structure to obtain a single-layer plain weave fabric, which has anti-ultraviolet properties while also ensuring good air permeability and moisture permeability. Plain weave: a fabric formed by interweaving warp yarns and weft yarns one above and one below. In some embodiments, the fabric has a gram weight of 90-250gsm and a stitch count of 28-60. In addition, the fabric described in the embodiment of the present invention can also be a single-layer fabric such as dyed or yarn-dyed.
[0046] After the plain weave fabrics are woven in the embodiment of the present invention, the anti-ultraviolet performance and other performance tests are performed on them. The results show that the fabric textiles in the embodiment of the present invention have excellent anti-ultraviolet performance, washing resistance, friction resistance, and good air permeability and moisture permeability.
[0047] The technical solutions in the implementation cases of this application are described clearly and completely below. Obviously, the described embodiments are only some embodiments of this application, not all embodiments. Based on the embodiments in this application, other embodiments obtained by ordinary technicians in this field without creative work are all within the scope of invention protection. In the following embodiments, all raw materials are commercially available, and polyester and nylon are both conventional spinning grades.
[0048] Embodiment 1
[0049] Granulation process: fully mix the dried polyester powder, light-converting powder and dispersant, add them into a mixture of 50 parts of anhydrous ethanol and deionized water (configuration volume ratio is 9:1), and after fully dispersed, place them in a vacuum oven to dry, and then blend and granulate them.
[0050] Wherein, the solvent is an ethanol / water mixed solution; the dispersant is a silane coupling agent.
[0051] Raw material ratio: 20 parts of raw materials (17 parts of CaS:Eu,Cl, 3 parts of titanium oxide), 80 parts of polyester carrier.
[0052] The obtained chemical fiber-based light-converting masterbatch is melt-spun through a spinning spinneret assembly at a spinning temperature of about 300°C to obtain an anti-ultraviolet light-converting yarn. Among them, the light-converting masterbatch accounts for 25%. The temperature of each spinning zone: 290°C in zones 1, 2 and 3, 280°C in zones 4 and 5, and 32°C in the cooling zone; the spinning speed: 1000m / min.
[0053] FDY yarn stretching process: high-speed winding speed 3500m / min; yarn specification: 75d / 48f.
[0054] The anti-ultraviolet light-converting yarn is woven into a plain weave fabric according to a plain weave structure.
[0055] Embodiment 2
[0056] Granulation process: fully mix the dried polyester powder, light-converting powder and dispersant, add them into a mixture of 50 parts of anhydrous ethanol and deionized water (configuration volume ratio is 9:1), and after fully dispersed, place them in a vacuum oven to dry, and then blend and granulate them.
[0057] Wherein, the solvent is an ethanol / water mixed solution; the dispersant is a silane coupling agent.
[0058] Raw material ratio: 30 parts of raw material (25 parts of 2Eu(TTA)3(TPPO)2, 3 parts of titanium oxide, 2 parts of talcum powder), 70 parts of polyester carrier.
[0059] The obtained chemical fiber-based light-converting masterbatch is melt-spun through a spinning spinneret assembly at a spinning temperature of about 300°C to obtain an anti-ultraviolet light-converting yarn. Among them, the light-converting masterbatch accounts for 20%. The temperature of each spinning zone: 290°C in zones 1, 2 and 3, 280°C in zones 4 and 5, and 32°C in the cooling zone; the spinning speed: 1000m / min.
[0060] FDY yarn stretching process: high-speed winding speed 3500m / min; yarn specification: 50d / 48f.
[0061] The anti-ultraviolet light-converting yarn is woven into a plain weave fabric according to a plain weave structure.
[0062] Embodiment 3
[0063] Granulation process: fully mix the dried nylon 6 powder, light-converting powder and dispersant, add them into a mixture of 50 parts of anhydrous ethanol and deionized water (configuration volume ratio is 9:1), and after fully dispersed, place them in a vacuum oven to dry, and then blend and granulate them.
[0064] Wherein, the solvent is an ethanol / water mixed solution; the dispersant is a silane coupling agent.
[0065] Raw material ratio: 30 parts of raw material (25 parts of 2Eu(TTA)3(TPPO)2, 3 parts of titanium oxide, 2 parts of talcum powder), 70 parts of polyester carrier.
[0066] The obtained chemical fiber-based light-converting masterbatch is melt-spun through a spinning spinneret assembly, and the spinning temperature is about 250°C to obtain an anti-ultraviolet light-converting yarn. Among them, the light-converting masterbatch accounts for 20%. The temperatures of each spinning zone are: 240°C in zone 1, 245°C in zone 2, 250°C in zone 3, 255°C in zone 4 and 5, and 30°C in cooling zone; the spinning speed is 1000m / min.
[0067] FDY yarn stretching process: high-speed winding speed 3500m / min; yarn specification: 70d / 48f.
[0068] The anti-ultraviolet light-converting yarn is woven into a plain weave fabric according to a plain weave structure.
[0069] Comparative Example 1
[0070] Solvent: ethanol / water mixture;
[0071] Dispersant: silane coupling agent;
[0072] Raw material ratio: 17 parts CaS:Eu,Cl, 83 parts polyester carrier;
[0073] Granulation process: fully mix the dried polyester powder, light-converting powder and dispersant, add them into a mixture of 50 parts of anhydrous ethanol and deionized water (configuration volume ratio is 9:1), and after fully dispersed, place them in a vacuum oven to dry, and then blend and granulate them.
[0074] The temperature of each spinning zone: 290℃ in zones 1, 2 and 3, 280℃ in zones 4 and 5, and 32℃ in cooling zone;
[0075] Spinning speed: 1000m / min;
[0076] FDY yarn stretching process: high-speed winding speed 3500m / min;
[0077] Yarn specification: 70d / 48f.
[0078] Comparative Example 2
[0079] Solvent: ethanol / water mixture;
[0080] Dispersant: silane coupling agent;
[0081] Raw material ratio: 17 parts titanium oxide, 83 parts polyester carrier;
[0082] Granulation process: The dried polyester powder and dispersant are fully mixed, and then added into a mixture of 50 parts of anhydrous ethanol and deionized water (with a volume ratio of 9:1). After being fully dispersed, it is placed in a vacuum oven to dry, and then blended and granulated.
[0083] The temperature of each spinning zone: 290℃ in zones 1, 2 and 3, 280℃ in zones 4 and 5, and 32℃ in cooling zone;
[0084] Spinning speed: 1000m / min;
[0085] FDY yarn stretching process: high-speed winding speed 3500m / min;
[0086] Yarn specification: 70d / 48f.
[0087] The plain fabrics prepared in the above embodiments and comparative examples were tested, and the test contents were as follows:
[0088] 1) GB / T18830-2009 ultraviolet protection factor, results: UPF value>500, T(UVA)av<5%;
[0089] 2) GB / T35263-2017 cool feeling on contact;
[0090] 3) UV absorption curve; Figure 1 is the ultraviolet absorption curve of Example 1, and the absorption peak is located in the ultraviolet region; Figure 2 is the excitation spectrum, Figure 3 This is an excitation-absorption spectrum diagram, and the emission peak is in the blue light band.
[0091] 4) Verify the luminescence of the fabric after irradiation with ultraviolet light; using a standard multi-light source and multi-color light box, using an ultraviolet light source, it can be observed that the fabric emits bright visible blue light (or other colored light).
[0092] Table 1 Test data comparison
[0093]
[0094] It can be seen from the above embodiments that the embodiments of the present invention prepare a melt-spun chemical fiber yarn containing a light conversion agent and an ultraviolet reflector, wherein the light conversion agent is one or more of rare earth chlorides, rare earth carboxylate complexes, rare earth ketone complexes and phycocyanin; the ultraviolet reflector is one or more of kaolin, calcium carbonate, talcum powder, iron oxide, zinc oxide and titanium oxide. At the same time, the present invention also provides a fabric containing the yarn. The present invention mainly utilizes the specific light conversion material contained in the yarn, which can convert ultraviolet rays in sunlight into visible light, and combines ultraviolet reflectors, etc. to achieve excellent anti-ultraviolet performance of textiles. The fabric finally constructed by the embodiment of the present invention is integrated with the anti-ultraviolet component and has the characteristics of washing resistance.
[0095] Furthermore, the fabric provided by the present invention has anti-ultraviolet properties, and does not need to construct a multi-layer fabric, thereby ensuring air permeability and moisture permeability. The anti-ultraviolet light-converting yarn single fiber of the present invention can also have a special-shaped cross-section, which can make ultraviolet light diffusely reflected on the surface of the fabric, reduce the fabric penetration, and further enhance the anti-ultraviolet effect.
[0096] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. An anti-ultraviolet light-converting yarn, characterized in that: The chemical fiber-based light conversion masterbatch is formed by melt spinning and weaving; the chemical fiber-based light conversion masterbatch comprises a chemical fiber substrate, a light conversion agent and an ultraviolet reflector, the light conversion agent is one or more of rare earth chloride, rare earth carboxylate complex, rare earth ketone complex and phycocyanin; the ultraviolet reflector is one or more of kaolin, calcium carbonate, talc, iron oxide, zinc oxide and titanium oxide; The single fiber of the anti-ultraviolet light-converting yarn has a round and / or a special-shaped cross section.
2. The anti-ultraviolet light-converting yarn according to claim 1, characterized in that: The mass percentage of the light conversion agent in the anti-ultraviolet light conversion yarn is 0.5% to 3%.
3. The anti-ultraviolet light-converting yarn according to claim 1, characterized in that: The chemical fiber substrate is polyester and / or nylon; the light conversion agent is CaS:Eu,Cl and / or Eu(TTA)3(TPPO)2.
4. The anti-ultraviolet light-converting yarn according to any one of claims 1 to 3, characterized in that: The single fiber of the anti-ultraviolet light-converting yarn has a special-shaped cross section, which is a flat cross section, a polygonal cross section or a gear-shaped cross section.
5. A method for preparing an anti-ultraviolet light-converting yarn, characterized in that: The following steps are involved: Provided is a chemical fiber-based light conversion masterbatch, wherein the chemical fiber-based light conversion masterbatch comprises a chemical fiber substrate, a light conversion agent and an ultraviolet reflector, wherein the light conversion agent is one or more of rare earth chlorides, rare earth carboxylate complexes, rare earth ketone complexes and phycocyanin; and the ultraviolet reflector is one or more of kaolin, calcium carbonate, talc, iron oxide, zinc oxide and titanium oxide; The chemical fiber-based light-converting masterbatch is melt-spun through a spinning spinneret assembly to obtain a plurality of anti-ultraviolet light-converting fibers, which are then woven into anti-ultraviolet light-converting yarns.
6. The preparation method according to claim 5, characterized in that: The chemical fiber-based light-converting masterbatch is formed by mixing chemical fiber substrate slices, a light-converting agent, an ultraviolet reflector, a solvent and a dispersant and then granulating them. The chemical fiber substrate slices are polyester slices and / or nylon slices.
7. The preparation method according to claim 6, characterized in that: The mass percentage of the light conversion agent in the anti-ultraviolet light conversion yarn is 0.5% to 3%; the light conversion agent is CaS:Eu,Cl and / or Eu(TTA)3(TPPO)2.
8. The preparation method according to any one of claims 5 to 7, characterized in that: The temperature of the melt spinning is 240°C to 300°C.
9. A fabric, characterized in that: The invention is woven from the anti-ultraviolet light-converting yarn described in any one of claims 1 to 4.
10. The fabric according to claim 9, characterized in that: The single fiber of the anti-ultraviolet light-converting yarn has a special-shaped cross section; and the fabric has a plain weave structure.
Citation Information
Patent Citations
Ultraviolet resistant functional fabric
CN101451275A
Preparation method of rare earth efficient light-conversion polyester material
CN101845682A
Biodegradable light conversion film and preparation method thereof
CN109251488A
Preparation method of ultraviolet-proof modified special-shaped nylon filament
CN110257950A
Anti-ultraviolet master batch for polyester fiber, preparation method, anti-ultraviolet polyester fiber and fabric
CN114806096A
Cited By
Breathable sunscreen fabric with anti-perspective function and preparation method thereof
CN119265787A