Method for producing substance containing alkali metal element and sulfur element
By using inert gas stirring technology in a porous container, the problem of uneven composition caused by sulfur volatilization during the melting process of sulfide-based solid electrolytes is solved, and the manufacturing of sulfide-based solid electrolytes with high uniformity and miniaturization of equipment is achieved.
Patent Information
- Application Number
- CN202380019436.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-02-02
- Filing Date
- 2023-01-30
- Publication Date
- 2024-10-29
AI Technical Summary
When manufacturing sulfide-based solid electrolytes using the melting method, the volatility of sulfur results in uneven composition, and it is difficult to mechanically stir the melt in a closed or volatilization-suppressed system, limiting the miniaturization of equipment and mass production.
Raw materials containing alkali metal elements and sulfur elements are placed in a porous container, heated and melted, and stirred by inert gas flowing into the outside of the porous container to suppress the volatilization of sulfur and realize the production of materials with excellent uniformity.
It realizes the production of substances containing alkali metal elements and sulfur elements with excellent uniformity when using highly volatile sulfur element raw materials, avoiding the use of large machinery, and is suitable for mass synthesis and equipment miniaturization.
Smart Images

Figure CN118871384A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for producing a substance containing an alkali metal element and a sulfur element, and in particular to a method for producing a sulfide-based solid electrolyte containing a lithium element. Background Art
[0002] Lithium-ion secondary batteries are widely used in portable electronic devices such as mobile phones and laptop computers. In the past, liquid electrolytes have been used in lithium-ion secondary batteries, but there are concerns about leakage and fire, so for safety design, the housing needs to be enlarged. In addition, the problems of short battery life and narrow operating temperature range are also expected to be improved.
[0003] In this regard, all-solid-state lithium-ion secondary batteries using solid electrolytes as electrolytes for lithium-ion secondary batteries have attracted much attention from the perspectives of improved safety, high-speed charging and discharging, and miniaturization of the housing. As a method for manufacturing solid electrolytes, glass sealing, mechanical grinding, melting, etc. are known, among which melting is widely used as a method for mass production.
[0004] For example, Patent Document 1 discloses a method for producing a lithium ion conductive material, wherein a composite compound containing lithium, phosphorus, and sulfur as a composition is melted and vitrified, and the molten glass is quenched to obtain sulfide glass.
[0005] Patent Document 2 discloses a method for producing a sulfide-based lithium ion conductive solid electrolyte, in which each constituent compound of the sulfide-based lithium ion conductive solid electrolyte is mixed and heated and melted in a state in which sulfur is excessive.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Publication No. 2012-43654
[0009] Patent Document 2: Japanese Patent Application Laid-Open No. 6-115911 Summary of the invention
[0010] The raw materials used in the manufacture of sulfide-based solid electrolytes contain sulfur, but sulfur is easily volatilized. Therefore, if the sulfur volatilizes during the process of heating and melting the raw materials, the composition of the obtained sulfide-based solid electrolyte will be uneven. Therefore, in the case of manufacturing a sulfide-based solid electrolyte by a melting method, it is necessary to suppress the composition unevenness caused by the volatilization of sulfur in the raw materials by melting the raw materials in a closed or volatilization-suppressed system. However, in the above-mentioned closed or volatilization-suppressed system, it is difficult to mechanically stir the melt, and the method of stirring the melt is limited.
[0011] Furthermore, when synthesizing a large amount of sulfide-based solid electrolytes, it is necessary to enlarge the equipment, but it is difficult to stir the melt together with the equipment using a rocking furnace or the like, and it is difficult to stir and homogenize the melt of the raw materials.
[0012] Therefore, an object of the present invention is to provide a method for producing a substance containing an alkali metal element and a sulfur element with excellent uniformity even when a raw material containing a highly volatile sulfur element is used.
[0013] The present inventors have conducted intensive studies and have found a method in which a raw material containing an alkali metal element and a sulfur element is placed in a porous container, heated and melted to obtain a melt, and the melt is stirred by an inert gas flowing outside the porous container. The inventors have found that this method can suppress the uneven composition caused by the volatilization of sulfur in the raw material, and can produce a material containing an alkali metal element and a sulfur element with excellent uniformity, thereby completing the present invention.
[0014] That is, the present invention relates to the following [1] to
[10] .
[0015] [1] A method for producing a substance containing an alkali metal element and a sulfur element, comprising placing a raw material containing an alkali metal element and a sulfur element in a porous container, heating and melting the raw material to obtain a melt, and stirring the melt by flowing an inert gas outside the porous container.
[0016] [2] The production method according to [1] above, wherein the alkali metal element is lithium, and the substance containing the alkali metal element and sulfur is a sulfide-based solid electrolyte containing lithium.
[0017] [3] The production method according to [1] or [2] above, wherein the raw material further contains phosphorus.
[0018] [4] The production method according to any one of [1] to [3] above, wherein the contact angle between the porous container and the melt is 30° or more.
[0019] [5] The production method according to any one of [1] to [4] above, wherein the open porosity of the porous container is 5% or more.
[0020] [6] The production method according to any one of [1] to [5] above, wherein the porous container contains carbon.
[0021] [7] The method according to [6] above, wherein the bulk density of the carbon is 1.6 to 2.0 g / cm 3 .
[0022] [8] A manufacturing method according to any one of [1] to [7] above, wherein the ratio of the height of the porous container to the length of the long axis in a two-dimensional projection image when the porous container is projected from above, i.e., the aspect ratio, is less than 1.
[0023] [9] A manufacturing method according to any one of [1] to [8] above, wherein the porous container is connected to other containers to form a container connector, and the ratio of the height of the container connector to the length of the major axis in a two-dimensional projection image when the container connector is projected from above, i.e., the height-to-diameter ratio, is less than 1.
[0024]
[10] The manufacturing method according to any one of [1] to [9] above, wherein the porous container is surrounded on its outer side by a non-porous outer shell.
[0025] According to one embodiment of the present invention, a raw material containing an alkali metal element and a sulfur element is placed in a porous container, heated and melted to obtain a melt, and an inert gas flowing into the outside of the porous container flows into the container through the pores of the porous container, thereby stirring the melt. Therefore, even when a raw material containing a highly volatile sulfur element is used, it is possible to heat, melt, and stir in a closed or volatilization-suppressed system, and a material containing an alkali metal element and a sulfur element with excellent uniformity can be produced.
[0026] In addition, since an inert gas is used to stir the melt, there is no need to use large-scale machinery, and even in a closed or volatilization-suppressed system where mechanical stirring is difficult, a large amount of substances containing alkali metal elements and sulfur elements can be synthesized. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 It is a schematic diagram showing a production method according to one embodiment of the present invention.
[0028] Figure 2 (a) and (b) are schematic diagrams for explaining the high aspect ratio of the porous container (rectangular parallelepiped).
[0029] Figure 3 (a) and (b) are schematic diagrams for explaining the high aspect ratio of the porous container (cylindrical).
[0030] Figure 4 (a) and (b) are schematic diagrams for explaining the high aspect ratio of a container connection body formed by connecting a plurality of containers. DETAILED DESCRIPTION
[0031] Hereinafter, the present invention will be described in detail, but the present invention is not limited to the following embodiments, and can be arbitrarily deformed and implemented without departing from the scope of the present invention. In addition, the " to " indicating a numerical range is used to include the numerical values recorded before and after it as the meaning of the lower limit and the upper limit.
[0032] The method for producing a substance containing an alkali metal element and a sulfur element (hereinafter sometimes referred to as the present substance) according to an embodiment of the present invention (hereinafter sometimes referred to as the present production method) is characterized in that a raw material containing an alkali metal element and a sulfur element is placed in a porous container, heated and melted to obtain a melt, and the melt is stirred using an inert gas flowing into the outside of the porous container.
[0033] (raw material)
[0034] The raw material used in the present production method (hereinafter also referred to as the present raw material or simply referred to as the raw material) contains an alkali metal element (R) and a sulfur element (S).
[0035] Examples of the alkali metal element (R) include lithium element (Li), sodium element (Na), and potassium element (K). Among them, lithium element (Li) is preferred.
[0036] As the alkali metal element (R), a simple substance of an alkali metal element, a compound containing an alkali metal element, or a substance (component) containing an alkali metal element can be used in combination as appropriate. Among them, as the lithium element, a simple substance of Li, a compound containing Li, or a substance (component) containing Li can be used in combination as appropriate.
[0037] As the substance containing lithium element (Li), for example, lithium compounds such as lithium sulfide (Li2S), lithium iodide (LiI), lithium carbonate (Li2CO3), lithium sulfate (Li2SO4), lithium oxide (Li2O) and lithium hydroxide (LiOH), metallic lithium, etc. As the substance containing lithium element (Li), lithium sulfide is preferably used from the viewpoint of obtaining a sulfide material.
[0038] As the sulfur element (S), a simple substance of S, a compound containing S, or other substances (components) containing S may be used in combination as appropriate.
[0039] Examples of substances containing elemental sulfur (S) include phosphorus sulfides such as phosphorus trisulfide (P2S3) and phosphorus pentasulfide (P2S5), other sulfur compounds containing phosphorus, elemental sulfur, and compounds containing sulfur. Examples of compounds containing sulfur include H2S, CS2, iron sulfides (FeS, Fe2S3, FeS2, Fe 1-x S, etc.), bismuth sulfide (Bi2S3), copper sulfide (CuS, Cu2S, Cu 1-xS, etc.). From the viewpoint of obtaining a sulfide material, the substance containing sulfur element (S) is preferably phosphorus sulfide, and more preferably phosphorus pentasulfide (P2S5). These substances may be used alone or in combination of two or more. It should be noted that phosphorus sulfide is considered to be a compound that serves as both a substance containing S and a substance containing P described later.
[0040] The raw material preferably further contains phosphorus (P) from the viewpoint of improving the ion conductivity of the obtained material. As phosphorus (P), P simple substance, P-containing compound and other P-containing substances (components) can be used in appropriate combination.
[0041] As the substance containing phosphorus element (P), for example, phosphorus sulfides such as phosphorus trisulfide (P2S3) and phosphorus pentasulfide (P2S5), phosphorus compounds such as sodium phosphate (Na3PO4), and elemental phosphorus can be cited. As the substance containing phosphorus element (P), from the viewpoint of further exerting the effect of the present invention, phosphorus sulfide with high volatility is preferred, and phosphorus pentasulfide (P2S5) is more preferred. These substances can be used alone or in combination of two or more.
[0042] The raw material is obtained by appropriately mixing the above-mentioned substances according to the composition of the target substance. The mixing ratio is not particularly limited. For example, from the viewpoint of improving the ion conductivity of the obtained substance, the molar ratio S / R of sulfur element (S) to alkali metal element (R) in the raw material is preferably 0.25 / 0.75 or more, more preferably 0.3 / 0.7 or more.
[0043] As an example of a preferred combination of an alkali metal element and a sulfur element contained in the raw material, a combination of Li2S and P2S5 can be cited. In the case of combining Li2S and P2S5, the molar ratio of Li to P, Li / P, is preferably 40 / 60 to 88 / 12, and more preferably 50 / 50 to 88 / 12. By adjusting the mixing ratio so that P2S5 is less than Li2S, it is easy to suppress the volatilization of sulfur and phosphorus components during heat treatment due to the boiling point of P2S5 being lower than the melting point of Li2S.
[0044] On the other hand, since lithium sulfide is expensive, lithium compounds other than lithium sulfide, metallic lithium, etc. can be used from the viewpoint of suppressing the manufacturing cost of sulfide-based solid electrolytes. Specifically, in this case, the raw material preferably contains one or more selected from metallic lithium, lithium iodide (LiI), lithium carbonate (Li2CO3), lithium sulfate (Li2SO4), lithium oxide (Li2O) and lithium hydroxide (LiOH) as a substance containing Li. These substances can be used alone or in combination of two or more.
[0045] The raw material may contain other substances (compounds etc.) in addition to the above substances depending on the composition of the target substance or as additives.
[0046] For example, in the case of manufacturing the present material containing the halogen elements such as F, Cl, Br or I, the raw material preferably contains the halogen element (Ha). In this case, the raw material preferably comprises the compound containing the halogen element. As the compound containing the halogen element, lithium halides such as lithium fluoride (LiF), lithium chloride (LiCl), lithium bromide (LiBr), lithium iodide (LiI), phosphorus halides, phosphoryl halides, sulfur halides, sodium halides, boron halides, etc. can be enumerated. As the compound containing the halogen element, from the viewpoint of the reactivity of the raw material, preferably lithium halides, more preferably LiCl, LiBr, LiI. These compounds can be used alone, or two or more can be used in combination.
[0047] Alkali metal halides such as lithium halide are also compounds containing alkali metal elements such as Li. When the raw material contains an alkali metal halide, part or all of the alkali metal element such as Li in the raw material may be derived from the alkali metal halide such as lithium halide.
[0048] When the raw material contains a halogen element (Ha) and a phosphorus element (P), from the viewpoint of improving the ion conductivity of the obtained substance, the molar equivalent of Ha in the raw material relative to P is preferably 0.2 molar equivalent or more, and more preferably 0.5 molar equivalent or more. In addition, from the viewpoint of the stability of the obtained substance, the molar equivalent of Ha is preferably 4 molar equivalents or less, and more preferably 3 molar equivalents or less.
[0049] From the viewpoint of improving the glass formation state of the obtained substance, it is also preferred that the raw material contains sulfides such as SiS2, B2S3, GeS2, Al2S3, etc. By making glass formation easy, glass can be obtained even if the cooling rate is reduced when obtaining glass by rapid cooling, which can reduce the load on equipment.
[0050] In addition, from the viewpoint of imparting moisture resistance to the present material, it is also preferred to contain oxides such as SiO2, B2O3, GeO2, Al2O3, and P2O5. These compounds may be used alone or in combination of two or more.
[0051] It should be noted that these sulfides and oxides may be contained in the raw materials, or may be separately added when the raw materials are heated and melted. In addition, the amount of these sulfides and oxides added is preferably 0.1% by weight or more, more preferably 0.5% by weight or more, relative to the total amount of the raw materials. In addition, the amount added is preferably 50% by weight or less, more preferably 40% by weight or less.
[0052] Furthermore, the raw material may contain a compound that serves as a crystal nucleus as described later.
[0053] Even when the raw material containing the highly volatile compound is melted and stirred to produce the present material, the present manufacturing method can suppress the uneven composition caused by the volatilization of the compound. Therefore, the present manufacturing method is particularly suitable for the case where the raw material contains the highly volatile compound. Examples of the highly volatile compound include LiI, B2S3, S, Se, Sb2S3, and P2S5.
[0054] (Substances containing alkali metal elements and sulfur elements)
[0055] As the substance containing alkali metal elements and sulfur elements obtained by the present production method (the present substance), for example, solid electrolytes, infrared transparent materials, low melting point sealing materials, etc. can be cited. As the solid electrolyte, for example, sulfide solid electrolytes can be cited. The shape of the present substance is not particularly limited, and for example, powder, flakes, plates, etc. can be cited.
[0056] In addition, although the present production method is described below mainly using a sulfide-based solid electrolyte as the present substance, the present substance obtained by the present production method is not limited to the sulfide-based solid electrolyte.
[0057] <Sulfide-based solid electrolyte>
[0058] Examples of the sulfide-based solid electrolyte obtained by the present production method include sulfide-based solid electrolytes containing lithium elements, such as Li 10 GeP2S 12 Sulfide-based solid electrolytes with LGPS crystal structure, Li6PS5Cl, Li 5.4 PS 4.4 Cl 1.6 and Li 5.4 PS 4.4 Cl 0.8 Br 0.8 Sulfide-based solid electrolytes having an argyrodite-type crystal structure, Li-P-S-Ha-based (Ha represents at least one element selected from halogen elements) glass-ceramics, and Li7P3S 11 LPS glass-ceramics, etc.
[0059] The sulfide-based solid electrolyte may be an amorphous sulfide-based solid electrolyte, a sulfide-based solid electrolyte having a specific crystal structure, or a sulfide-based solid electrolyte containing a crystalline phase and an amorphous phase, depending on its purpose.
[0060] When the sulfide-based solid electrolyte contains a crystalline phase, the crystal contained in the sulfide-based solid electrolyte is preferably an ion-conductive crystal. Specifically, the ion-conductive crystal refers to a crystal having a lithium ion conductivity greater than 10 -4S / cm, more preferably greater than 10 -3 From the viewpoint of lithium ion conductivity, the crystalline phase is preferably an argyrodite type crystalline phase.
[0061] As a sulfide-based solid electrolyte with excellent lithium ion conductivity, a sulfide-based solid electrolyte having elements of Li-P-S-Ha is preferred, and a crystalline phase is more preferred. In addition, the halogen element is preferably a halogen element selected from one or more of lithium chloride, lithium bromide and lithium iodide.
[0062] The obtained sulfide-based solid electrolyte can be identified by analyzing the crystal structure using X-ray diffraction (XRD) measurement, and analyzing the elemental composition using various methods such as ICP emission spectrometry, atomic absorption spectrometry, and ion chromatography. For example, P and S can be measured by ICP emission spectrometry, Li can be measured by atomic absorption spectrometry, and Ha can be measured by ion chromatography.
[0063] In addition, by performing Raman spectroscopy, the uniformity of the composition of the sulfide-based solid electrolyte can be evaluated. Specifically, Raman spectroscopy is performed on a sample obtained from the obtained sulfide-based solid electrolyte at any two or more points. It should be noted that from the viewpoint of improving the accuracy of the evaluation, the number of measurement points is preferably 8 or more, and more preferably 10 or more.
[0064] Preferred Raman spectroscopic conditions for evaluating the uniformity of the composition of the sulfide-based solid electrolyte include, for example, a spot diameter of 3 μm and a number of measurement points of 10. By setting the spot diameter to 3 μm, the analysis region in the Raman spectroscopic measurement has a size suitable for evaluating the uniformity of the composition of the sulfide-based solid electrolyte at a microscopic level.
[0065] It is believed that PS4 in each measurement result 3- The smaller the deviation of the peak wave number (peak position) of the structure derived from the sulfide-based solid electrolyte, the more uniform the composition of the sulfide-based solid electrolyte. Alternatively, it is believed that the smaller the deviation of the full width at half maximum of the peak derived from the structure of the sulfide-based solid electrolyte, the more uniform the composition of the sulfide-based solid electrolyte.
[0066] Although it depends on the composition of the obtained sulfide-based solid electrolyte, it is preferable to confirm a peak derived from a P—S bond as a peak derived from the structure of the sulfide-based solid electrolyte.
[0067] The position of the peak derived from the P-S bond varies depending on the composition system, but is typically contained within 350 cm -1 ~500cm -1Hereinafter, in the present specification, the deviation of the peak position and the deviation of the full width at half maximum of the peak refer to the values confirmed for the peak with the strongest intensity among the peaks derived from the P—S bond.
[0068] The deviation of the peak position can be evaluated as follows. That is, the standard deviation of the peak position of each measurement point obtained by Raman spectroscopy is calculated and recorded as (peak position average value) ± (standard deviation). The value of the standard deviation is preferably 2 cm -1 Within, more preferably 1 cm -1 Within, more preferably 0.5cm -1 It should be noted that the peak position here refers to the position of the peak top.
[0069] For example, for the sulfide-based solid electrolyte obtained by the present production method, when Raman spectroscopy is performed with a spot diameter of 3 μm and 10 measurement points, the 350 cm -1 ~500cm -1 The standard deviation of the peak position derived from the P—S bond is preferably 2 cm -1 Within, more preferably 1 cm -1 Within, more preferably 0.5cm -1 Within.
[0070] The deviation of the half-maximum full width of the peak can be evaluated as follows. That is, the standard deviation of the half-maximum full width of the peak at each measurement point obtained by Raman spectroscopy is calculated by finding the half-maximum full width of each peak and finding the standard deviation of its value. When it is recorded as (peak half-maximum full width average) ± (standard deviation), the value of the standard deviation is preferably 2 cm -1 Within, more preferably 1.5cm -1 It should be noted that the full width at half maximum of the peak here refers to the width at which a value of half the peak intensity of the peak derived from the P—S bond intersects with the peak derived from the P—S bond when the Raman spectrum is plotted.
[0071] For example, for the sulfide-based solid electrolyte obtained by the present production method, when Raman spectroscopy is performed with a spot diameter of 3 μm and 10 measurement points, the 350 cm -1 ~500cm -1 The standard deviation of the half-maximum width of the peak derived from the P-S bond is preferably 2 cm -1 Within, more preferably 1.5cm -1 Within.
[0072] From the viewpoint of improving battery characteristics when used in lithium ion secondary batteries, the lithium ion conductivity of the obtained sulfide-based solid electrolyte is preferably 1.0×10 -4 S / cm or more, more preferably 5.0×10-4 S / cm or more, more preferably 1.0×10 -3 S / cm or more.
[0073] (porous container)
[0074] In the present production method, the raw material is placed in a porous container and heated to melt. In the present production method, by using a porous container, an inert gas is flowed into the outside of the porous container, so that the inert gas enters the porous container through the pores of the porous container to stir the melt. Therefore, even when a raw material containing sulfur element with high volatility is used, a material containing an alkali metal element and sulfur element with excellent uniformity can be produced in a closed or volatilization-suppressed system.
[0075] Here, the volatilization-suppressing system refers to a system that suppresses the highly volatile raw materials such as sulfur element put into the porous container from being discharged to the outside of the porous container due to volatilization.
[0076] For example, a system can be mentioned in which a lid is provided in a container provided with an opening for adding raw materials, etc. so as to minimize the area of the opening to suppress the discharge of highly volatile raw materials, etc., due to volatilization, to the outside of the container. In addition, a system can be mentioned in which a gas inlet and outlet having a minimum area for the inlet and outlet of an inert gas is provided in a part of the lid.
[0077] Another example is a system in which the porous container is surrounded by a non-porous shell described below to suppress volatilization. The shell may be provided with the minimum necessary openings such as gas inlet and outlet, raw material inlet, electrolyte outlet, etc.
[0078] The "porous" in the porous container used in the present manufacturing method refers to a state in which there are a plurality of pores on the surface and inside of the container to a degree that can be confirmed using an electron microscope. In addition, the pores penetrate the inside and outside of the container. The open porosity of the porous container is usually 1% or more, preferably 5% or more, more preferably 10% or more, and further preferably 15% or more. Here, the open porosity refers to the value measured according to JIS R1634:1998.
[0079] The material of the porous container is not particularly limited as long as it is a heat-resistant porous material. The porous container includes, for example, carbon, ceramics, and glass. Among them, the porous container preferably contains carbon from the viewpoint of low reactivity with the melt of the raw material.
[0080] The bulk density of carbon is preferably 1.6 to 2.0 g / cm 3 , more preferably 1.7 to 1.95 g / cm 3 , more preferably 1.75 to 1.8 g / cm 3When the bulk density of carbon is within the above range, the melt does not leak out of the container, and can be melted while stirring while introducing an inert gas through the hole.
[0081] The bulk density of carbon is measured in accordance with JIS R1634:1998.
[0082] The shape and size of the porous container are not particularly limited and can be appropriately selected according to the purpose. In addition, the porous container can constitute a container connector connected to other containers. That is, the container connector includes at least one porous container and is composed of a plurality of containers connected. The number of containers in the container connector is not particularly limited. The above-mentioned other containers can be porous containers or non-porous containers. Among them, as other containers, porous containers are preferably used. This is because if the other containers are porous containers, the container connector has a plurality of porous containers, so the effect of the above-mentioned present invention is more effectively exerted.
[0083] It should be noted that when a non-porous container is used as another container, there is no particular limitation on the function, but it is preferred to have a gas barrier function. Here, "non-porous" in the non-porous container means that no pores can be observed on the surface and inside of the container using an electron microscope. The open porosity of the non-porous container is usually 0.1% or less.
[0084] The means for connecting the containers in the container connection body is not particularly limited, and examples thereof include joining, screwing, bonding, etc. In addition, the number of connecting means (connecting parts) is also not particularly limited.
[0085] The high aspect ratio of the porous container is preferably 1 or less, more preferably 0.7 or less, and further preferably 0.5 or less. Here, the high aspect ratio of the porous container refers to the ratio of the height of the porous container to the length of the long axis in the two-dimensional projection image when the porous container is projected from above (the height of the porous container / the length of the long axis in the two-dimensional projection image when the porous container is projected from above). The high aspect ratio is obtained by dividing the height of the porous container by the length of the long axis in the two-dimensional projection image when the porous container is projected from above.
[0086] Here, the height of the porous container refers to the maximum height of the porous container in the height direction, and the length of the major axis refers to the maximum length in a two-dimensional projection image when the porous container is projected from above.
[0087] It should be noted that when the shape of the porous container is a rectangular parallelepiped (or substantially rectangular parallelepiped), the height and the length of the major axis are respectively as follows: Figure 2 As shown in (a) and (b), when the shape of the porous container is cylindrical (or substantially cylindrical), the height and the length of the major axis are respectively as follows Figure 3 as shown in (a) and (b).
[0088] In addition, as described above, when a porous container is connected to other containers to form a container connector, the ratio of the height of the container connector to the length of the major axis in a two-dimensional projection image when the container connector is projected from above, that is, the height aspect ratio, is preferably less than 1, more preferably less than 0.5, and further preferably less than 0.3.
[0089] For example, Figure 4 As shown in (a), when a plurality of containers (first container 22a, second container 22b) including a porous container are connected by a connecting portion 23 to form a container connection body 22, the high aspect ratio of the container connection body 22 is obtained by Figure 4 The height of the container connector 22 shown in (a) is divided by Figure 4 The length of the major axis of the container connection body 22 shown in (b) is obtained when the container connection body 22 is projected from above in a two-dimensional projection image.
[0090] Here, the height of the connected container body refers to the maximum height of the connected container body in the height direction, and the length of the major axis refers to the maximum length in a two-dimensional projection image when the connected container body is projected from above.
[0091] The contact angle of the porous container measured by the method described in Examples is preferably 30° or more. When the contact angle is 30° or more, the melt can be well suppressed from leaking out of the pores of the porous container, and the present material can be produced with excellent uniformity.
[0092] The contact angle is more preferably 45° or more, further preferably 60° or more, and particularly preferably 65° or more. For example, the contact angle is 150° or less.
[0093] In order to make the contact angle 30° or more, for example, a material with low wettability may be selected as the material of the porous container, or a material with low wettability such as a hydrophobic coating material may be applied to the porous container.
[0094] From the viewpoint of preventing oxygen and moisture in the atmosphere from entering the porous container, the porous container is preferably surrounded by a non-porous shell on its outside. The non-porous shell is not particularly limited as long as it is a material with gas barrier properties, and glass, ceramics, resins, metals, etc. can be cited. In particular, from the viewpoint of durability, metal is preferably used. The shell can also be provided with gas inlets and outlets, inlets for raw materials, etc., outlets for electrolytes, etc.
[0095] (Heating, melting, stirring)
[0096] In the present production method, the raw material is placed in a porous container and heated and melted to obtain a melt. The method of heating and melting is not particularly limited, and an example thereof is a method of heating the porous container containing the raw material in a melting furnace.
[0097] In the present production method, an inert gas is flowed into the porous container from the outside, and the inert gas enters the container through the pores of the porous container to stir the melt of the present raw material. Thus, by using the inert gas, the melt can be stirred in a non-contact manner, so even if the raw material contains sulfur, which is easily volatile, its volatilization can be suppressed during melting and stirring of the melt, and the present material with excellent uniformity can be obtained.
[0098] The type of the inert gas is not particularly limited as long as it does not react with the melt of the raw material, and examples thereof include nitrogen, argon, helium, etc. Among them, nitrogen is preferred from the viewpoint of procurement cost.
[0099] The oxygen concentration of the inert gas is preferably 1000 ppm by volume or less, more preferably 100 ppm by volume or less.
[0100] Below, use Figure 1 The method of heating, melting and stirring the raw materials is described in detail. Figure 1 In the figure, the following method is shown: a porous container 12 storing a raw material 11 containing an alkali metal element and a sulfur element is placed in a melting furnace 13, the porous container 12 is heated to obtain a melt of the raw material 11, and the melt in the porous container 12 is stirred by using an inert gas 15 flowing into a space 14 (outside the porous container 12) defined by the porous container 12 and the melting furnace 13.
[0101] First, the porous container 12 containing the raw material 11 is placed in the melting furnace 13. The melting furnace 13 is provided with, for example, a heater (not shown). The porous container 12 is heated in the melting furnace 13 to obtain a melt of the raw material 11.
[0102] The heating and melting can be carried out in a gas atmosphere containing sulfur. By heating and melting the raw material in a gas atmosphere containing sulfur, sulfur is introduced into the melt of the raw material. Thus, sulfur in an amount sufficient to obtain the material of the target composition can be introduced. The gas containing sulfur is, for example, sulfur gas, hydrogen sulfide gas, carbon disulfide gas, etc., which contains a compound containing sulfur or sulfur.
[0103] The sulfur-containing gas can be obtained by heating a sulfur source. In this case, the sulfur source is not particularly limited as long as it is elemental sulfur or a sulfur compound that can obtain a sulfur-containing gas by heating. Examples thereof include elemental sulfur, hydrogen sulfide, organic sulfur compounds such as carbon disulfide, iron sulfide (FeS, Fe2S3, FeS2, Fe1-xS, etc.), bismuth sulfide (Bi2S3), copper sulfide (CuS, Cu2S, Cu1-xS, etc.), lithium polysulfide, polysulfides such as sodium polysulfide, polysulfides, and rubber subjected to sulfur vulcanization treatment.
[0104] For example, these sulfur sources are heated in a separately provided sulfur source heating section to generate a gas containing sulfur element, and an inert gas such as N2 gas, argon gas, helium gas, etc. is transported to the furnace as a carrier gas, thereby obtaining a gas atmosphere containing sulfur element. By separating the sulfur source heating section and the section for heating and melting, even if the gas introduced into the furnace contains oxygen and water, it can be removed by reacting with the sulfur gas before introduction. In this way, a high-quality and high-purity sulfide-based solid electrolyte with few impurities can be obtained, so it is preferred.
[0105] In addition, in the present manufacturing method, an inert gas 15 is flowed into the outer side of the porous container 12, that is, into the space 14 defined by the melting furnace 13 and the porous container. By flowing the inert gas 15 into the outer side of the porous container 12, the inert gas 15 flows into the porous container 12 through the pores of the porous container. The inert gas 15 flowing into the porous container 12 promotes the flow of the melt in the porous container 12 and stirs the melt.
[0106] There is no particular restriction on the timing of flowing the inert gas 15 into the space 14. The inert gas 15 may be flowed into the space 14 before the heating and melting of the raw material is started, during the heating and melting of the raw material, or after the heating and melting of the raw material. There is no particular restriction on the timing of starting the flow of the inert gas 15. From the viewpoint of promoting stirring at the initial stage of melting of the raw material and shortening the melting time, it is preferred to start flowing the inert gas 15 into the space 14 before the heating and melting of the raw material is started.
[0107] The temperature for heating and melting is not particularly limited, but is preferably 600° C. or higher, more preferably 630° C. or higher, and further preferably 650° C. or higher from the viewpoint of homogenizing the melt in a short time. In addition, from the viewpoint of suppressing degradation and decomposition of the components in the melt caused by heating, the temperature for heating and melting is preferably 1000° C. or lower, more preferably 950° C. or lower, and further preferably 900° C. or lower.
[0108] The time of heating and melting is not particularly limited, and from the viewpoint of uniformity, is preferably more than 0.1 hour, more preferably more than 0.5 hour, more preferably more than 0.7 hour, and more preferably more than 1 hour. In addition, for the time of heating and melting, within the scope that the deterioration, decomposition caused by the heating of the composition in the melt can be allowed, the time of heating and melting can be very long. As the scope of reality, it is preferably less than 100 hours, more preferably less than 50 hours, and more preferably less than 24 hours.
[0109] The pressure during heating and melting is not particularly limited, and for example, normal pressure or slightly increased pressure is preferred, and normal pressure is more preferred.
[0110] The speed at which the inert gas 15 flows into the space 14 (outside the porous container 12 ) is not particularly limited, but is usually 20 to 2000 L / min, preferably 50 to 1000 L / min.
[0111] The dew point of the space 14 (outside the porous container 12 ) during stirring is preferably 0° C. to −75° C., and more preferably −25° C. to −70° C. When the dew point is within the above range, degradation of the electrolyte due to water can be prevented.
[0112] The temperature of the space 14 (outside the porous container 12 ) during stirring is preferably 300° C. to 1000° C., more preferably 500° C. to 950° C. When the temperature is within the above range, the melt can be melted in a short time.
[0113] The time for flowing the inert gas 15 into the space 14 (outside the porous container 12) is not particularly limited, and is usually 0.1 to 24 hours, preferably 0.3 to 10 hours, and more preferably 0.5 to 5 hours. When the time for flowing the inert gas 15 is within the above range, uniform stirring can be achieved.
[0114] The oxygen concentration in the space 14 (outside the porous container 12) is not particularly limited, but is preferably 1000 ppm by volume or less. When the oxygen concentration is within the above range, oxygen diffuses into the porous container, and oxidation of sulfides can be prevented.
[0115] The inert gas replacement rate in the space 14 (outside the porous container 12) is preferably 1 / 100 min -1 ~100min -1 , more preferably 1 / 50min -1 ~50min -1 . The inert gas replacement rate is 1 / 100min -1 As mentioned above, the flow rate of the inert gas flowing into the porous container is large, which is beneficial to the stirring of the melt. In addition, the inert gas replacement rate is 100min -1 Thereafter, the internal pressure increases, thereby preventing damage to the device.
[0116] The dew point of the space (space excluding the raw material) in the porous container 12 is not particularly limited, but is preferably -25° C. to -75° C., and more preferably -35° C. to -65° C. When the dew point is within the above range, degradation of the sulfide due to water can be prevented.
[0117] The oxygen concentration of the space (space excluding the raw material) in the porous container 12 is not particularly limited, but is preferably 1000 volume ppm or less. When the oxygen concentration is within the above range, oxidation of sulfides can be prevented.
[0118] The flow rate of the inert gas 15 flowing into the porous container 12 is not particularly limited, but is usually 0.1 to 100 L / min, preferably 0.1 to 50 L / min, and more preferably 0.5 to 30 L / min.
[0119] In addition to the above-mentioned holes, the porous container 12 may also be provided with an inlet and outlet for inert gas to flow in or out. The inlet and outlet are different from the holes in the porous container. By flowing in or out of the inert gas through the inlet and outlet, the space in the porous container 12 can be replaced with the inert gas.
[0120] When a cover is provided on the opening portion of the upper portion of the container, the inlet and outlet can be provided on the cover. In addition, the inlet and outlet can be provided on the side of the container.
[0121] When the porous container 12 is provided with the above-mentioned inlet and outlet, the dew point of the space in the porous container 12 (space excluding the raw material) is preferably -25°C to -75°C, more preferably -30°C to -70°C, and further preferably -35°C to -65°C.
[0122] When the porous container 12 is provided with the above-mentioned inlet and outlet, the oxygen concentration of the space in the porous container 12 (space excluding the raw material) is preferably 1000 volume ppm or less, more preferably 500 volume ppm or less, and further preferably 200 volume ppm or less.
[0123] When the porous container 12 is provided with the above-mentioned inlet and outlet, the flow rate of the inert gas 15 into the porous container 12 is preferably 0.1 to 100 L / min, more preferably 0.1 to 50 L / min, and further preferably 0.5 to 30 L / min.
[0124] Heating, melting and stirring can be performed as a continuous process. A continuous process refers to a process in which the melt of the raw material flows continuously from the porous container 12. As far as input is concerned, the input of the raw material can be continuous or intermittent. When heating and melting are performed as a continuous process, the melt can be kept in a molten state for a long time under appropriate conditions taking into account the degradation of the components in the melt. For example, a long time can be about 24 hours.
[0125] (cool down)
[0126] The present production method preferably further comprises a step of cooling the melt obtained by heating and melting to obtain a solid. The cooling can be performed by a known method, and the method is not particularly limited.
[0127] From the viewpoint of maintaining the composition obtained by heating and melting, the cooling rate is preferably 0.01°C / sec or more, more preferably 0.05°C / sec or more, and further preferably 0.1°C / sec or more. In addition, the upper limit of the cooling rate is not particularly limited, but it is generally believed that the cooling rate of the twin rolls with the fastest rapid cooling rate is 1,000,000°C / sec or less.
[0128] Here, for example, in the case where the obtained solid is an amorphous sulfide-based solid electrolyte, it is preferred to obtain a solid by quenching the melt obtained by heating and melting. Specifically, the cooling rate during quenching is preferably 10°C / sec or more, more preferably 100°C / sec or more, further preferably 500°C / sec or more, and particularly preferably 700°C / sec or more. In addition, the upper limit of the cooling rate is not particularly limited, and it is generally believed that the cooling rate of the twin rolls with the fastest quenching rate is 1,000,000°C / sec or less.
[0129] On the other hand, it is also possible to slowly cool during the cooling process to crystallize at least a portion of the solid, thereby obtaining a sulfide-based solid electrolyte having a specific crystal structure, or a sulfide-based solid electrolyte composed of a crystalline phase and an amorphous phase. The cooling rate during slow cooling is preferably 0.01°C / sec or more, and more preferably 0.05°C / sec or more. In addition, the cooling rate is preferably 500°C / sec or less, and more preferably 450°C / sec or less. The cooling rate may be 10°C / sec or less, or 5°C / sec or less. It should be noted that the cooling rate may be appropriately adjusted according to the conditions of crystallization.
[0130] Here, the crystal contained in the sulfide-based solid electrolyte is preferably an ion-conductive crystal. Specifically, the ion-conductive crystal has a lithium ion conductivity of more than 10 -4 S / cm, more preferably greater than 10 -3 S / cm crystals.
[0131] In the case where the solid obtained after cooling is desired to be a sulfide-based solid electrolyte containing a crystalline phase, it is preferred that the melt obtained in the heating and melting step contains a compound that becomes a crystal nucleus. Thus, crystals are easily precipitated in the cooling step. The method of making the melt contain a compound that becomes a crystal nucleus is not particularly limited, and examples thereof include methods such as adding a compound that becomes a crystal nucleus to a raw material or an intermediate, and adding a compound that becomes a crystal nucleus to a melt during heating and melting.
[0132] Examples of the compound that serves as a crystal nucleus include oxides, nitrogen oxides, nitrides, carbides, other chalcogen compounds, halides, etc. The compound that serves as a crystal nucleus is preferably a compound that has a certain degree of compatibility with the melt. It should be noted that a compound that is completely incompatible with the melt cannot serve as a crystal nucleus.
[0133] When the solid obtained after cooling is to be a sulfide-based solid electrolyte containing a crystalline phase, the content of the compound that becomes the crystal nucleus in the melt is preferably 0.01% by mass or more, more preferably 0.1% by mass or more, and further preferably 1% by mass or more. On the other hand, from the viewpoint of suppressing the decrease in lithium ion conductivity, the content of the compound that becomes the crystal nucleus in the melt is preferably 20% by mass or less, and more preferably 10% by mass or less.
[0134] In the case of a sulfide-based solid electrolyte that is intended to be amorphous in the solid obtained after cooling, it is preferred that the melt does not contain a compound that becomes a crystal nucleus, or its content is less than a specified amount. Specifically, the content of the compound that becomes a crystal nucleus in the melt is preferably 1% by mass or less, more preferably 0.1% by mass or less. The content of the compound that becomes a crystal nucleus in the melt may also be 0.01% by mass or less.
[0135] (Reheat)
[0136] Amorphous sulfide-based solid electrolytes or sulfide-based solid electrolytes containing an amorphous phase can be subjected to a heat treatment (post-annealing) to promote high-temperature crystallization. In the case where the solid obtained in the cooling step is an amorphous sulfide-based solid electrolyte or a sulfide-based solid electrolyte containing an amorphous phase, the present manufacturing method may further include reheating the solid. In addition, by reheating the sulfide-based solid electrolyte containing sulfide-based solid electrolyte crystals, the ions in the crystal structure can also be rearranged, thereby improving the lithium ion conductivity.
[0137] It should be noted that the reheating treatment refers to at least one of heating the cooled solid for crystallization and rearranging the ions in the crystal structure. Here, the heat treatment of these amorphous sulfide-based solid electrolytes or sulfide-based solid electrolytes containing an amorphous phase, including the crystallization treatment, is referred to as the reheating treatment.
[0138] Example
[0139] The present invention is described below by way of examples and comparative examples, but the present invention is not limited to the following examples. Examples 1 to 3 are examples of the present invention, and Examples 4 and 5 are comparative examples of the present invention.
[0140] [Example 1]
[0141] Li2S (made by Sigma, purity 99.98%) and P2S5 (made by Sigma, purity 99%) were prepared in a 50:50 (mol ratio). 100 g of the raw powder was placed in a porous container made of carbon (open porosity 16%, bulk density 1.78 g / cm 3), the porous container is placed in a furnace. The porous container made of carbon is covered with a lid, and 0.1 L / min of N2 gas is circulated for 0.25 hours through the inlet and outlet for introducing inert gas provided in the lid, and then discharged, thereby replacing the space in the porous container with N2 gas. The oxygen concentration in the space in the porous container is 1000 volume ppm or less.
[0142] Next, N2 gas was flowed into the outside of the porous container, i.e., the space defined by the melting furnace and the porous container, at a rate of 25 L / min to form an atmosphere with an oxygen concentration of less than 1000 volume ppm and a dew point of less than -70°C. The atmosphere was maintained under the conditions of pressure: 1 atmosphere, temperature: 750°C (heating rate: 10°C / min) for 0.5 hours to melt the raw materials in the porous container.
[0143] Then, the melt was withdrawn from the bottom of the porous container and cooled on a water cooling plate at a cooling rate of 50° C. / sec to obtain a sulfide compound in a glassy state.
[0144] [Example 2]
[0145] The glassy sulfide compound of Example 2 was produced in the same manner as in Example 1 except that the rate of N 2 gas flowing into the outside of the porous container, that is, the space defined by the melting furnace and the porous container, was set to 70 L / min.
[0146] [Example 3]
[0147] As materials, the glassy sulfide compound of Example 3 was manufactured in the same manner as in Example 2, except that the raw material powders of Li2S (manufactured by Sigma, with a purity of 99.98%), P2S5 (manufactured by Sigma, with a purity of 99%) and Lil (manufactured by Sigma, with a purity of 99.9%) were mixed in a ratio of 40:30:30 (mol ratio), and the temperature of the outside of the porous container, i.e., the space defined by the melting furnace and the porous container, was set to 650°C (heating rate of 10°C / min).
[0148] [Example 4]
[0149] The porous container is made of glassy carbon (open porosity <1%) and a non-porous container (bulk density 1.54 g / cm 3 ), N 2 gas was flowed into the space defined by the melting furnace and the container at 25 L / min to form an atmosphere with a dew point of less than -70°C. The glassy sulfide compound of Example 4 was produced in the same manner as in Example 1, except that
[0150] [Example 5]
[0151] Without flowing N2 gas into the outside of the porous container, i.e., the space defined by the melting furnace and the porous container, 25 L / min of N2 gas is circulated through the lid of the above-mentioned carbon porous container to make the dew point of the atmosphere -70°C. Except for this, the glassy sulfide compound of Example 5 is manufactured in the same manner as in Example 1.
[0152] (Wettability Evaluation)
[0153] 30 mg of the obtained sulfide compound was placed on a plate made of the material of each porous container, melted, and the contact angle was measured. Specifically, a droplet obtained by melting at 750°C for 5 minutes and cooling was photographed from the side using a camera to obtain the contact angle with the above plate. The results are shown in Table 1.
[0154] (Uniformity Evaluation)
[0155] As samples for composition analysis, 30 g (sample 1) that first flowed out from the bottom side of the porous container onto the water-cooled plate, the next 30 g (sample 2), and the last 30 g (sample 3) that flowed out were collected, and composition analysis of these samples 1 to 3 was performed to evaluate uniformity.
[0156] In the composition analysis, the obtained electrolyte was pulverized, and the powder was dissolved in an alkaline aqueous solution. P and S were measured by ICP emission spectrometry, Li was measured by atomic absorption spectrometry, and I was measured by ion chromatography.
[0157] The results are shown in Table 1. The difference (= deviation) between the maximum value and the minimum value of the S component (wt %) in the average values of Samples 1 to 3 was evaluated as follows.
[0158] ◎: Deviation is 0.5 wt% or less
[0159] ○: Deviation is more than 0.5 wt% and less than 3 wt%
[0160] ×: Deviation exceeds 3% by weight
[0161] [Table 1]
[0162] In Examples 1 to 3 as working examples, an inert gas was flowed outside the porous container to stir the melt, thereby obtaining a sulfide compound with high uniformity.
[0163] On the other hand, in Example 4 as a comparative example, a non-porous and dense container was used, so stirring of the melt due to the inflow of the inert gas from the outside did not occur, resulting in a sulfide compound having a non-uniform composition.
[0164] In Example 5 as a comparative example, no inert gas was flowed into the outside of the porous container, so the melt was not stirred, resulting in a sulfide compound with uneven composition. In addition, the flow rate of N2 gas flowing into the container was increased to maintain the dew point, resulting in uneven composition.
[0165] Various embodiments have been described above with reference to the accompanying drawings, but it goes without saying that the present invention is not limited to these examples. Those skilled in the art can obviously think of various variations or modifications within the scope of the scope of the patent claim, and understand that they certainly also belong to the technical scope of the present invention. In addition, the various components in the above-mentioned embodiments can be used in combination without departing from the scope of the invention.
[0166] It should be noted that the present application is based on the Japanese patent application (Japanese Patent Application No. 2022-015190) filed on February 2, 2022, and the contents thereof are incorporated herein by reference.
[0167] Explanation of symbols
[0168] 11 Raw Materials
[0169] 12 porous containers
[0170] 13 Melting furnace
[0171] 14 Space
[0172] 15 Inert Gas
[0173] 22 container connector
[0174] 22a First container
[0175] 22b Second container
[0176] 23Connection
Claims
1. A method for producing a substance containing an alkali metal element and a sulfur element, comprising placing a raw material containing an alkali metal element and a sulfur element in a porous container, heating and melting the raw material to obtain a melt, and stirring the melt by using an inert gas flowing into the outside of the porous container.
2. The manufacturing method according to claim 1, wherein: The alkali metal element is lithium, and the substance containing the alkali metal element and the sulfur element is a sulfide-based solid electrolyte containing lithium.
3. The manufacturing method according to claim 1 or 2, wherein: The raw material further contains phosphorus.
4. The production method according to any one of claims 1 to 3, wherein The contact angle between the porous container and the melt is greater than 30°.
5. The production method according to any one of claims 1 to 4, wherein The open porosity of the porous container is greater than 5%.
6. The production method according to any one of claims 1 to 5, wherein The porous container contains carbon.
7. The manufacturing method according to claim 6, wherein: The bulk density of the carbon is 1.6 to 2.0 g / cm 3 .
8. The production method according to any one of claims 1 to 7, wherein The aspect ratio, which is a ratio of the height of the porous container to the length of the major axis in a two-dimensional projection image when the porous container is projected from above, is 1 or less.
9. The production method according to any one of claims 1 to 8, wherein The porous container is connected to other containers to form a container connection body, and the ratio of the height of the container connection body to the length of the major axis in a two-dimensional projection image when the container connection body is projected from above, that is, the aspect ratio is 1 or less.
10. The production method according to any one of claims 1 to 9, wherein: The porous container is surrounded on its outer side by a non-porous outer shell.
Citation Information
Patent Citations
Manufacturing method of lithium ion conductive material
JP2012043654A
Lithium battery high-conductivity glassy-ceramic-state solid electrolyte and preparation method thereof
CN110620261A
Sulfide-based lithium ion-conductive solid electrolyte and synthesis thereof
JP1994279049A
Manufacture of porous electrode for thin film solid electrolyte element
JP2000182628A
Lithium ion conducting sulfide glass fabrication
US20210320328A1