Stretchable wiring material and stretchable device

By using a combination of resin and flake-shaped metal powder in stretchable devices, adjusting the ratio of resin and metal powder solves the problem of composition deviation caused by uneven hardening reaction, and realizes a stretchable wiring material with high conductivity and high stretchability. , improving the durability and reliability of the device.

CN118872004APending Publication Date: 2024-10-29TDK CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202280093357.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2022-08-30
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

When the curing reaction of the existing resin composition is uneven, the composition hardening degree of the stretchable device varies, affecting its stretchability and durability, and it is difficult to realize a wiring material with high conductivity and high stretchability.

Method used

Use a stretchable wiring material containing resin and scale-shaped metal powder. By adjusting the ratio and structure of resin and metal powder, we ensure that the elongation at break reaches more than 130% and maintains low resistivity changes during the expansion and contraction process. The resin is dried by Formed by solidification to avoid compositional inhomogeneities in the hardening reaction.

Benefits of technology

A stretchable wiring material with high conductivity and high stretchability is achieved to ensure small changes in conductivity during repeated expansion and contraction, improve the durability and reliability of the device, and avoid composition unevenness and time-based deterioration caused by hardening reactions. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005033561920000111
    Figure BDA0005033561920000111
  • Figure BDA0005033561920000151
    Figure BDA0005033561920000151
  • Figure BDA0005033561920000161
    Figure BDA0005033561920000161
Patent Text Reader

Abstract

The stretchable wiring material contains a resin and a metal powder, the elongation at break is 130% or more, the resistivity ([rho] 0) before stretching is 2 * 10 <-2 > [[omega] mm] or less, the metal powder includes a scale-shaped powder, and the proportion of the resin is 8 wt% to 20 wt% (inclusive).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a stretchable wiring material and a stretchable device. This application claims priority based on Japanese Patent Application No. 2022-060116 filed in Japan on March 31, 2022, and uses the contents thereof herein. Background Art

[0002] In recent years, with the development of flexible sensors, wearable devices that can manage physical conditions have attracted attention. In the fields of sports science and health care, wearable devices are envisioned to be built into suits, directly attached to the skin, etc. to measure and monitor specific parts of the body, and are expected to be used in a wide range of applications. Human skin normally expands and contracts repeatedly, so when wearable devices are required to be wearable without pressure, the wearable devices are preferably stretchable in accordance with the worn object. In addition, the wearable device is envisioned to be subjected to human activities, and preferably has a certain strength or more for the stress generated when it is bent or rolled. Devices with such characteristics are not limited to wearable devices in this specification and are referred to as stretchable devices.

[0003] As a stretchable device, it is assumed that electrodes, wiring, devices, electronic components, thin film sensors, etc. are included in the stretchable element, and they need to maintain their quality even in a repeated stretching environment. However, it is difficult to realize such a stretchable device with a polyimide sheet used in the conventional thin film resin substrate. For this reason, it is assumed that the element and electrodes in the stretchable device use a resin that can cope with stretchability, such as polyurethane resin, silicone resin, acrylic resin, epoxy resin, polycarbonate, polystyrene or polyolefin, as the main constituent material. Among them, a (meth)acrylate compound having a siloxane bond, a (meth)acrylate compound other than the (meth)acrylate compound having a urethane bond, and a (meth)acrylate compound having a siloxane bond as a cured product of a composition containing an organic solvent having a boiling point in the range of 115 to 200°C at atmospheric pressure. The stretchable film has excellent stretchability and strength to the same degree as polyurethane (polyurethane), and the film surface has excellent water repellency to the same degree as silicone (see Patent Document 1). Prior art literature Patent Literature

[0004] Patent Document 1: Japanese Patent Application Publication No. 2017-206626 Summary of the invention The technical problem that the invention is intended to solve

[0005] However, in the case of a resin sheet (resin film) whose main constituent material is a cured product of a resin composition as described in Patent Document 1, if the curing reaction proceeds unevenly, deviations (unevenness) in composition and degree of curing will occur in the resin sheet, resulting in a problem of forming a product that does not have the intended stretchability, strength, and resistance to deterioration over time. Furthermore, in order to realize a stretchable device, it is desirable to use wiring that has high conductivity and high stretchability and that has a small change in conductivity when stretched or stretched.

[0006] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a stretchable wiring material and a stretchable device which have high conductivity and high stretchability and which have a small change in conductivity when stretched. Technical means for solving technical problems

[0007] In order to solve the above-mentioned technical problems, the present invention provides the following technical means.

[0008] A first aspect of the present invention is a stretchable wiring material comprising a resin and a metal powder, having a breaking elongation of 130% or more, and a resistivity (ρ0) before stretching of 2×10 -2 [Ωmm] or less, the metal powder includes flake-shaped powder, and the ratio of the resin is 8wt% to 20wt%.

[0009] A second aspect of the present invention is a stretchable wiring material comprising a resin and a metal powder, wherein the elongation at break is 130% or more, and the resistivity (ρ 50 ) to the resistivity before expansion (ρ0) (ρ 50 / ρ0) is less than 7, the metal powder includes flake-shaped powder, and the proportion of the resin is more than 8wt% and less than 20wt%.

[0010] A third aspect of the present invention is that in the stretchable wiring material of the second aspect, the resistivity (ρ 100 ) and the resistivity (ρ 50 ) ratio (ρ 100 / ρ 50 ) is less than 8.

[0011] A fourth aspect of the present invention is a stretchable wiring material comprising a resin and a metal powder, wherein the elongation at break is 130% or more, and the resistivity (ρ 100 ) and the resistivity (ρ 50 ) ratio (ρ 100 / ρ 50 ), relative to the resistivity (ρ) when the expansion ratio is 50% 50 ) to the resistivity before expansion (ρ0) (ρ50 / ρ0) is less than 140%, the metal powder includes flake-shaped powder, and the proportion of the resin is more than 8wt% and less than 20wt%.

[0012] According to a fifth aspect of the present invention, in the stretchable wiring material according to any one of the first to fourth aspects, the resin is cured by drying.

[0013] According to a sixth aspect of the present invention, in the stretchable wiring material of any one of the first to fifth aspects, the ratio of the flaky powder in the metal powder is 2.5 wt % or more and 50 wt % or less.

[0014] According to a seventh aspect of the present invention, in the stretchable wiring material according to any one of the first to sixth aspects, the flaky powder has an average maximum particle size of 3 μm or more and 10 μm or less.

[0015] According to an eighth aspect of the present invention, in the stretchable wiring material according to any one of the first to seventh aspects, the resin includes a polyurethane-based resin.

[0016] A ninth aspect of the present invention is a stretchable device using the stretchable wiring material of any one of the first to eighth aspects. Effects of the Invention

[0017] According to the present invention, it is possible to provide a stretchable wiring material which has high conductivity and high stretchability and in which the change in conductivity when stretched or contracted is small. DETAILED DESCRIPTION

[0018] The materials, dimensions, etc. described in the following description are merely examples, and the present invention is not limited thereto, and can be appropriately changed within the scope of the gist thereof.

[0019] (Stretchable wiring material (first embodiment)) The stretchable wiring material of the first embodiment includes resin and metal powder, has a breaking elongation of 130% or more, and a resistivity of 2×10 -3 [Ωmm] or less, the metal powder includes flaky powder, and the proportion of the resin is 4wt% to 20wt%.

[0020] (resin) The resin contained in the stretchable wiring material of the first embodiment is not particularly limited, and a known resin can be used as a stretchable resin. For example, polyurethane resins, acrylic resins, epoxy resins, urea-formaldehyde resins, polyurethane-urea resins, methacrylic resins, polyacrylic resins, silicone resins, diene resins, polyester resins, polyether resins, polyamide resins, polystyrene resins, and polyimide resins can be exemplified. These resins can be used alone or in combination of two or more.

[0021] The resin is preferably soluble in at least one selected from the group consisting of diethylene glycol monobutyl ether acetate (BCA), butyl carbitol (BC), ethyl cyanoacrylate (ECA), α-terpineol, diethylene glycol monobutyl ether, and diethylene glycol monoethyl ether acetate as a solvent.

[0022] The stretchable wiring material of the first embodiment can be formed by applying a resin composition containing a resin, metal powder, and a solvent to be used and curing the resin composition. Among the above resins, a dry curing type resin that can be formed and cured by simply applying and drying the resin composition without undergoing a curing reaction is preferred. As a dry curing type resin, a polyurethane resin can be exemplified. In this case, the stretchable wiring material of the present invention can be referred to as a dry curing type stretchable wiring material. This is because, if the curing reaction of the resin that needs to undergo a curing reaction does not proceed uniformly, the composition and degree of curing may vary in the wiring sheet, resulting in a wiring material that does not have the desired elasticity, strength, and resistance to deterioration over time. When a polyurethane resin is used, it is preferred that the resin component contain a siloxane bond because in this case, the resin composition has appropriate water repellency and can suppress the hydrolysis of the urethane bond.

[0023] The ratio of the resin in the stretchable wiring material of the first embodiment is 8 wt % or more and 20 wt % or less. The stretchable wiring material of the first embodiment is a wiring material with a small change in conductivity during stretching, and as a premise, in order to ensure high stretchability (high elongation at break), the proportion of resin is set to 8wt% or more. On the other hand, the stretchable wiring material of the first embodiment is a wiring material with high conductivity before and during stretching, and in order to ensure high conductivity (low resistivity), the proportion of resin is set to 20wt% or less. The ratio of the resin in the stretchable wiring material is preferably 10 wt % or more, and the ratio of the resin in the stretchable wiring material is preferably 18 wt % or less.

[0024] When the resin in the stretchable wiring material of the first embodiment includes a polyurethane-based resin, the ratio of urethane bonds in the resin is preferably 15 wt % or more, and more preferably 17 wt % or more. For example, by calculating in C 13 The ratio of urethane bonds in the resin can be calculated from the peak area corresponding to the urethane bonds in the NMR (Nuclear Magnetic Resonance) spectrum. In addition, in the examples described later in which the ratio of urethane bonds in the resin is high, there are cases where the elongation at break is low. The current situation is that, although the reason is not clear, based on the examples, the ratio of urethane bonds in the resin is preferably 30 wt% or less, more preferably 25 wt% or less, and further preferably 22 mol% or less.

[0025] (Metal powder) The metal powder is not particularly limited, and known metal powders can be used as the metal powder. For example, silver (Ag) powder, carbon (C), copper (Cu) powder, palladium (Pd) powder, gold (Au) powder, and platinum (Pt) powder can be exemplified. Among them, silver powder or alloy powder with silver as the main component is preferred due to its low resistance. Here, alloy powder with silver as the main component means that more than 50wt% is silver, preferably silver is 70wt% or more, more preferably silver is 80wt% or more, and further preferably silver is 90wt% or more.

[0026] As the metal powder, a suitably produced metal powder may be used, or a commercially available item may be used. For example, as a method for producing silver powder, there can be cited a method of reducing and precipitating silver particles by adding an aqueous solution containing a reducing agent to an aqueous reaction system containing silver ions, etc. In addition, silver powder can also be used, such as silver-coated copper powder, which has a silver surface and a metal other than silver inside.

[0027] Metal powder includes flake-shaped powder. Here, in this specification, "flake-shaped powder" refers to a powder (metal powder) whose thickness is less than 1 / 10 relative to the maximum particle size. Here, the maximum particle size of the flake-shaped powder is determined as follows. The length of each powder from one end to the other end is different depending on the direction when viewed from above, but the longest length among these lengths is the maximum particle size. The maximum particle size can be determined by optical microscope observation, scanning electron microscope (SEM) observation (for example, 5000 times the field of view), etc. When the metal powder is in a scale shape, since it has upper and lower surfaces extending in the plane direction, the proportion of surface contact between the metal powders increases, resulting in high conductivity (low resistivity).

[0028] As the scale-shaped (flake-shaped) metal powder, a suitably produced metal powder may be used, or a commercially available one may be used. Flake-shaped metal powder can be produced, for example, by making a desired metal film and pulverizing the film. With this production method, since the film is pulverized, each broken metal flake is also flat. The thickness relative to the particle size (i.e., the degree of flatness) can be adjusted by adjusting the thickness of the film and the degree of pulverization.

[0029] The proportion of the flaky powder contained in the metal powder is preferably 2.5 wt% or more, more preferably 5 wt% or more, and further preferably 7.5 wt% or more. In addition, the proportion of the flaky powder contained in the metal powder is preferably 50 wt% or less, more preferably 40 wt% or less, further preferably 30 wt% or less, and further preferably 25 wt% or less. From the viewpoint of high conductivity (low resistivity), it is preferred that the proportion of the flaky powder contained in the metal powder is high, but when it is too high, the stretchability decreases and the elongation at break becomes low. In order to smoothly stretch and contract the stretchable wiring material, the freedom of movement of the metal powder is required, but when the proportion of the flaky powder exceeds 50wt%, it is believed that the flaky shape itself causes a large impedance to the movement.

[0030] The average maximum particle size of the flaky powder is preferably 3 μm or more and 10 μm or less. This is because if it is 3 μm or more, sufficiently high conductivity (low resistivity) can be obtained due to the surface contact effect of the metal powders, and if it is 10 μm or less, sufficient elasticity can be suppressed from decreasing and the elongation at break can be reduced.

[0031] (Elongation at break) The elongation at break of the stretchable wiring material is 130% or more, preferably 150% or more, more preferably 200% or more, further preferably 250% or more, and further preferably 300% or more. The elongation at break of the stretchable wiring material can be increased by increasing the proportion of the resin contained in the stretchable wiring material, but the increase in the proportion of the resin leads to an increase in the resistivity. Therefore, the elongation at break can be appropriately adjusted by adjusting the proportion of the resin according to the elongation at break and resistivity required for the stretchable device using the stretchable wiring material.

[0032] In this specification, "elongation at break" is defined by {(length at break - length before stretching) / length before stretching} × 100. The elongation at break can be measured in each specified direction. In this specification, the so-called "elongation at break of 150% or more" is defined as the elongation at break in the direction with the maximum specified elongation at break. In addition, if there is no anisotropy in the elongation at break, the elongation at break is the same in any direction. In addition, if the anisotropy of the elongation at break is small, the elongation at break becomes a similar value in any direction.

[0033] (Method for measuring elongation at break) First, an example of a method for preparing a sample is described below. Prepare a glass plate with a clean surface. Next, place a PET film on the glass plate and fix the upper side with tape. Next, prepare and set an applicator (for example, YA type, 75 mm, 152 μm, manufactured by YOSHIMITSU). Next, stir the stretchable wiring paste in the container in a state where air does not enter. Next, apply the stretchable wiring paste on the PET film. Next, slide the applicator to spread the stretchable wiring paste. Next, after spreading the stretchable wiring paste, fix the PET film and the glass plate with tape. Next, after leaving it for more than 3 minutes but less than 5 minutes, put it into a dryer that has been pre-heated to more than 90°C but less than 100°C, and dry it for 1 hour. Through the above steps, a sheet sample of a stretchable wiring material with a thickness of about 30 μm to 70 μm is obtained. In addition, the thickness of the sheet sample of the PET film and the stretchable wiring material added together is about 150 μm.

[0034] The elongation at break can be measured as described below. Six strip-shaped measurement samples with a width of 10 mm and a length of 30 mm are cut one by one from the sheet-like sample of the stretchable wiring material. For each measurement sample, the elongation at break is calculated using the method described below, and the average value is used as the elongation at break. The metal substrate is clamped at the upper and lower gripping parts of the measuring device, and the measurement sample is fixed to the metal substrate with double-sided tape so that the measurement part becomes 10 mm in width and 10 mm in length. Afterwards, a tensile testing machine (for example, trade name: Autograph AGS-5kNX, manufactured by Shimadzu Corporation) is used to stretch the measurement sample at a stretching speed of 10 mm / min. Then, the length of the measurement sample at break is measured, and the length before stretching 10 mm is subtracted from the length to calculate the elongation at break of each measurement sample. The average value is used as the elongation at break, and the elongation at break is calculated according to the above definition.

[0035] (Resistivity before expansion) The resistivity of the stretchable wiring material before stretching (normal resistivity) is 2×10 -2[Ωmm] or less. Preferably 7×10 -3 [Ωmm] or less, more preferably 6×10 -3 [Ωmm] or less, more preferably 4×10 -3 [Ωmm] or less. The resistivity before stretching of the stretchable wiring material can be reduced by increasing the ratio of metal powder contained in the stretchable wiring material, but the reduction in the resin ratio caused by the increase in the metal powder ratio leads to a reduction in the elongation at break. Therefore, the resistivity before stretching can be appropriately adjusted by adjusting the ratio of metal powder according to the elongation at break and resistivity required for the stretchable device using the stretchable wiring material.

[0036] (Methods for measuring resistance value and resistivity) First, a sheet-like sample of a stretchable wiring material is prepared by the above-mentioned method. The resistivity before expansion and contraction can be measured as described below. As with the measurement of the elongation at break, 6 strip-shaped measurement samples with a width of 10 mm and a length of 30 mm are cut one by one from the sheet-like sample of the stretchable wiring material. The metal substrate is clamped at the upper and lower gripping parts of the measuring device so that the measurement part becomes 10 mm in width and 10 mm in length, and the measurement sample is fixed to the metal substrate with double-sided tape. The resistance value of each measurement sample is measured in this state. The average value is taken as the resistance value R0 before expansion and contraction. In addition, for the resistance value of each elongation, the metal substrate is moved 1 mm each time, and the sample is stretched while measuring the resistance value during the stretch each time, and the average value of the 6 samples is taken as the resistance value R during the stretch. Next, the thickness of the sheet sample of the stretchable wiring material is measured as described below. The sheet sample of the stretchable wiring material is punched into a circle. Next, the sample is placed on a platform, and a rectangular PET film having one side larger than the diameter of the circular sample is placed on the sample. The thickness of the four corners of the rectangular PET film is measured, for example, using DIGIMICRO ZC-101 (manufactured by Nikon Corporation), and the average is taken as the thickness of the PET film. Next, the thickness of the sample and the PET film added together is measured at 5 points in the top, bottom, left, right and center, and the thickness t of the sample is calculated by subtracting the thickness of the PET film from the average thickness. Next, the resistivity ρ0 (= R0×(cross-sectional area / length)) is calculated from the above-mentioned resistance value R0 before stretching and the thickness t, width, and length of the sheet-like sample of the stretchable wiring material. In addition, similarly to the resistivity at each elongation, the resistivity ρ (=R×(cross-sectional area / length)) was calculated from the resistance value at each elongation and the thickness t, width, and length of the sheet sample of the stretchable wiring material.

[0037] In the stretchable wiring material of the first embodiment, it is preferable that the resistivity (ρ 50 ) to the resistivity before expansion (ρ0) (ρ 50 / ρ0) is 7 or less, more preferably 6 or less, and even more preferably 5 or less. In addition, it is preferred that the resistivity (ρ 100 ) and the resistivity (ρ 50 ) ratio (ρ 100 / ρ 50 ) is 8 or less, more preferably 7 or less, further preferably 6 or less, and further preferably 5 or less. In addition, the resistivity (ρ) when the expansion ratio is 50% is preferably 50 ) to the resistivity before expansion (ρ0) (ρ 50 / ρ0), and the resistivity when the expansion ratio is 100% (ρ 100 ) and the resistivity (ρ 50 ) ratio (ρ 100 / ρ 50 ) are all 7 or less, more preferably 6 or less, and further preferably 5 or less.

[0038] In the stretchable wiring material of the first embodiment, the resistivity (ρ 100 ) and the resistivity (ρ 50 ) ratio (ρ 100 / ρ 50 ), relative to the resistivity (ρ) when the expansion ratio is 50% 50 ) to the resistivity before expansion (ρ0) (ρ 50 The rate of change of (ρ / ρ0) is preferably 140% or less, more preferably 80% or less, further preferably 70% or less, further preferably 60% or less, and further preferably 50% or less.

[0039] In the stretchable wiring material of the first embodiment, it is more preferable that the resistivity (ρ 50 ) to the resistivity before expansion (ρ0) (ρ 50 / ρ0), and the resistivity when the expansion ratio is 100% (ρ 100 ) and the resistivity (ρ 50 ) ratio (ρ 100 / ρ 50 ) are all below 7, and the resistivity (ρ 100 ) and the resistivity (ρ 50 ) ratio (ρ 100 / ρ 50), relative to the resistivity when the expansion ratio is 50% (ρ 50 ) to the resistivity before expansion (ρ0) (ρ 50 / ρ0) is less than 140%.

[0040] (Stretchable wiring material (Second embodiment)) The stretchable wiring material of the second embodiment includes a resin and metal powder, has a breaking elongation of 130% or more, and a resistivity (ρ 50 ) to the resistivity before expansion (ρ0) (ρ 50 / ρ0) is 7 or less, the metal powder includes flaky powder, and the ratio of the resin is 8wt% or more and 20wt% or less. The description of the common structure with the stretchable wiring material of the first embodiment is omitted. Furthermore, the resistivity (ρ 100 ) and the resistivity (ρ 50 ) ratio (ρ 100 / ρ 50 ) is preferably 8 or less. Furthermore, the ratio of the resin in the stretchable wiring material is preferably 10 wt % or more, and the ratio of the resin in the stretchable wiring material is preferably 18 wt % or less.

[0041] The smaller the change in resistivity of the stretchable wiring material when it is stretched, the better. The resistivity ratio (ρ) when the expansion ratio is 50% to that before expansion 50 / ρ0) is preferably 6 or less, and more preferably 5 or less. In addition, the resistivity (ρ 100 ) and the resistivity (ρ 50 ) ratio (ρ 100 / ρ 50 ) is more preferably less than 7, further preferably less than 6, and further preferably less than 5.

[0042] In the stretchable wiring material of the second embodiment, the resistivity (ρ 100 ) and the resistivity (ρ 50 ) ratio (ρ 100 / ρ 50 ), relative to the resistivity when the expansion ratio is 50% (ρ 50 ) to the resistivity before expansion (ρ0) (ρ 50 The change rate of / ρ0) is preferably 140% or less.

[0043] (Stretchable wiring material (third embodiment)) The stretchable wiring material of the third embodiment includes a resin and metal powder, has a breaking elongation of 130% or more, and has an s resistivity (ρ 100 ) and the resistivity (ρ 50 ) ratio (ρ 100 / ρ 50 ), relative to the resistivity (ρ) when the expansion ratio is 50% 50 ) to the resistivity before expansion (ρ0) (ρ 50 The change rate of / ρ0) is 140% or less, the metal powder includes flaky powder, and the ratio of the resin is 8wt% or more and 20wt% or less. The description of the common structure with the stretchable wiring material of the first embodiment is omitted. Furthermore, the ratio of the resin in the stretchable wiring material is preferably 10 wt % or more, and the ratio of the resin in the stretchable wiring material is preferably 18 wt % or less.

[0044] The resistivity of the stretchable wiring material decreases as it is stretched, and the smaller the rate of decrease, the better. 100 / ρ 50 ) / ratio(ρ 50 / ρ0)) is preferably 80% or less, more preferably 70% or less, further preferably 60% or less, and further preferably 50% or less.

[0045] (Method for producing stretchable wiring material) The stretchable wiring materials of the first to third embodiments can be produced through the following main steps: (1) a stretchable wiring paste preparation step, (2) a stretchable wiring paste application step, and (3) a drying and curing step. That is, in the (1) stretchable wiring paste preparation step, the metal powder is added to the resin composition containing the above-mentioned resin and solvent to prepare the stretchable wiring paste. Then, in the (2) stretchable wiring paste coating step, the stretchable wiring paste is coated on a substrate (e.g., a PET film). Thereafter, in the (3) drying and curing step, the solvent is removed and the paste is dried and cured, thereby preparing the stretchable wiring material.

[0046] Hereinafter, specific examples of the resin composition (resin and solvent) for producing the stretchable wiring material will be given to explain the characteristics of the stretchable wiring material. Specific examples include resin compositions containing a resin component (sometimes referred to as "resin component (II)" in this specification) having a group represented by the following general formula (11), (21) or (31) and a urethane bond.

[0047] [Chemistry 1] (In the formula, Z1 is an alkyl group, one or more hydrogen atoms in the alkyl group may be substituted with a cyano group, a carboxyl group or a methoxycarbonyl group, and the two or more substituents may be the same or different from each other. Z2 is an alkyl group. Z3 is an aryl group. R4 is a hydrogen atom or a halogen atom. The bond given the symbol * is formed between the bonding target of the group represented by the above general formula (11), (21) or (31).)

[0048] The resin component (II) contained in the resin composition has a urethane bond and therefore has high flexibility. In addition, the resin component (II) is obtained by carrying out a polymerization reaction using a resin having a urethane bond and a polymerizable unsaturated bond and a RAFT agent for reversible addition fragmentation chain transfer polymerization (sometimes referred to as "RAFT polymerization" in this specification) which is a source of the group represented by the general formula (11), (21) or (31). By carrying out the polymerization reaction in this way, gelation can be avoided during the process of the resin forming a crosslinking structure during polymerization, and a resin component with a target degree of polymerization and crosslinking state can be obtained. That is, the resin component (II) having the group represented by the general formula (11), (21) or (31) has a small deviation in the degree of polymerization and the crosslinking state. In addition, the resin component (II) may also have a siloxane bond. In this case, the resin composition has moderate water repellency and can inhibit the hydrolysis of the urethane bond of the resin component (II). Such a resin component (II) can also be obtained by polymerization reaction using a resin having a siloxane bond and a polymerizable unsaturated bond. In addition, the method for producing the resin component (II) by RAFT polymerization will be described in detail separately.

[0049] The resin having the urethane bond and the polymerizable unsaturated bond used for the production of the resin component (II) is an oligomer and is sometimes referred to as "resin (a)". The resin having the siloxane bond and the polymerizable unsaturated bond used for producing the resin component (II) is an oligomer and may be referred to as "resin (b)" in the present embodiment. The resin component (II) is a polymer produced by polymerizing the resins (a) at their polymerizable unsaturated bonds. When the resin (b) is used, the resin component (II) is a polymer produced by polymerizing the resins (a) and (b) at their polymerizable unsaturated bonds.

[0050] When the resin (b) is used, the resin component (II) preferably has both a urethane bond and a siloxane bond in one molecule.

[0051] The resin (a) is not particularly limited as long as it has a urethane bond and a polymerizable unsaturated bond. Examples of the resin (a) include resins having a urethane bond and a (meth)acryloyl group as a group having a polymerizable unsaturated bond, and more specifically, urethane (meth)acrylate. In this specification, "(meth)acrylate" is a concept including both "acrylate" and "methacrylate". The same applies to terms similar to (meth)acrylate, for example, "(meth)acryloyl" is a concept including both "acryloyl" and "methacryloyl".

[0052] The resin (b) is not particularly limited as long as it has a siloxane bond and a polymerizable unsaturated bond. Examples of the resin (b) include various known silicone resins having a (meth)acryloyl group as a group having a polymerizable unsaturated bond. More specifically, examples include modified polydialkylsiloxanes such as polydimethylsiloxanes having a (meth)acryloyl group bonded to one or both ends thereof.

[0053] The resin component (II) has high solubility in a solvent due to its composition. Therefore, the resin composition containing the resin component (II) also has high solubility in a solvent. Such a resin composition with high solubility can be printed on an application object by various printing methods, so that a resin composition layer can be easily formed. In addition, by making the resin composition layer not hardened by drying and solidifying, a layer (resin layer, wiring material sheet) the same as the wiring material sheet can be manufactured. Such a method is suitable for forming an electrode or wiring using the resin composition containing a conductive component.

[0054] A stretchable wiring material sheet formed by using such a highly soluble resin composition and a stretchable device formed by using the wiring material sheet have a great advantage that damage can be suppressed during stretching. The main reasons for the damage of conventional stretchable devices during stretching and contraction can be considered from the perspective of materials: (i) structural defects such as voids and interface peeling caused by shrinkage due to heat or accompanying hardening reactions; (ii) uneven hardness due to uneven composition; and (iii) time-dependent degradation of the material due to light irradiation, oxidation, etc. Therefore, by suppressing structural defects such as voids, interface peeling, compositional nonuniformity, and time-dependent degradation of the material, damage during stretching of the stretchable device can be suppressed. As processing of stretchable substrates, molding by hot melting and cross-linking by heat or light curing reaction are common, but due to the reasons (i) to (iii) above, there is a concern that the reliability of stretchable devices may be reduced if fine processing is considered. In this regard, for example, if a resin is molded only by coating and drying a resin composition corresponding to a lamination method, good results can be expected.

[0055] Regarding the stretchable wiring material, the resin composition of the above specific example contains metal powder to prepare a stretchable wiring paste, which is then applied to a substrate and then cured by drying to obtain a stretchable wiring material in the form of a wiring material sheet (hereinafter sometimes referred to as a "wiring material sheet"). The stretchable wiring material can also be prepared by stacking a plurality of wiring material sheets. The wiring material sheet has good elasticity because it contains the resin component (II) as a main component. When the resin (b) is used, the wiring material sheet also has moderate water repellency, thereby being able to suppress the time-dependent degradation caused by hydrolysis. The wiring material sheet having such characteristics is particularly suitable for constituting various stretchable devices, such as wearable devices.

[0056] The wiring material sheet can be formed by simply drying and curing the resin composition as described above without causing the resin composition to undergo a curing reaction, and therefore does not have the disadvantages that would otherwise occur due to the progress of the curing reaction.

[0057] For example, regarding the photocuring reaction, it is very difficult to uniformly cure a material that does not transmit ultraviolet light. For example, when ultraviolet light is irradiated to the periphery of a device or electronic component mounted in a photocurable wiring material sheet, the uneven transmittance of ultraviolet light produces areas with different degrees of curing, and the wiring material sheet is easily damaged in areas with low crosslinking density. In addition, non-crosslinked areas are easily degraded by oxidation. On the other hand, the heat curing reaction is prone to shrinkage differences in the wiring material sheet due to the heat distribution during curing. When such shrinkage differences occur, parts with different constituent materials such as between the device and the sealant are prone to peeling off at their interfaces. In addition, when parts with different curing degrees are generated in the wiring material sheet due to heat distribution, they are prone to deterioration due to repeated expansion and contraction. Furthermore, in either case of the photohardening reaction or the heat hardening reaction, it is difficult to carry out the reaction uniformly in the wiring material sheet, which results in uneven composition or hardening degree in the wiring material sheet, and the hardened wiring material sheet does not have the desired elasticity and strength. Moreover, since the hardener is contained, it is easy to deteriorate over time due to heat and light. On the other hand, the wiring material sheet obtained by drying and curing the stretchable wiring paste containing the resin composition of the above specific example does not have such a problem.

[0058] The wiring material sheet can be produced, for example, by applying the stretchable wiring paste to a target location and drying and solidifying the paste without causing a curing reaction.

[0059] The stretchable wiring paste can be applied by, for example, a known method using various coaters or a wire bar coater, or various printing methods including an inkjet printing method.

[0060] When manufacturing the wiring material sheet, the drying temperature of the stretchable wiring paste is preferably 25 to 150° C., and more preferably 25 to 120° C. When the drying temperature is 25° C. or higher, the wiring material sheet can be manufactured more efficiently. When the drying temperature is 150° C. or lower, the drying temperature can be prevented from becoming excessively high, and deformation of the peeling sheet and damage to the wiring material sheet are unlikely to occur, and modification of the wiring material sheet can be suppressed.

[0061] When manufacturing the wiring material sheet, the drying time of the stretchable wiring paste can be appropriately set according to the drying temperature, preferably from 10 minutes to 120 minutes, more preferably from 30 minutes to 90 minutes. When the drying time is within this range, a wiring material sheet with good characteristics can be efficiently manufactured.

[0062] The completion of curing (formation of a wiring material sheet) of the stretchable wiring paste by drying can be confirmed, for example, by the fact that no clear change is observed in the mass of the resin composition subjected to drying.

[0063] The thickness of the stretchable wiring material is not particularly limited, and for example, a stretchable wiring material having a thickness of 10 μm to 5000 μm can be used.

[0064] (use) The stretchable wiring material of the present invention can be used as wiring in, for example, a stretchable device. Regardless of whether or not a stretchable device is put to practical use, a so-called stretchable device is included. Example

[0065] Hereinafter, the present invention will be described in more detail by way of specific examples, but the present invention is not limited to the following examples.

[0066] The raw materials used in the preparation of the stretchable wiring paste are as follows. Resin (a) (a)-1: Urethane acrylate oligomer (product name: UN-5500, manufactured by Negami Industries, Ltd.) Resin (b) (b)-1: Methacrylate-modified polydimethylsiloxane modified with a methacryloyl group at one end (product name: SILAPLANE (registered trademark) FM-0721, manufactured by JNC Corporation) Polymerization initiator (c) (c)-1: dimethyl-2,2'-azobis(2-methylpropionate), azo polymerization initiator (product name: V601, manufactured by FUJIFILM Wako Pure Chemical Corporation) RAFT agent (1)-1: RAFT agent represented by the following formula (1)-1 (manufactured by FUJIFILM Wako Pure Chemical Corporation) (3)-1: RAFT agent represented by the following formula (3)-1 (manufactured by FUJIFILM Wako Pure Chemical Corporation) Other polymeric ingredients MMA: Methyl Methacrylate Solvent BCA: Butyl Carbitol Acetate Metal powder Silver powder (ratio of flake-shaped powder: 12.5 [wt%], average maximum particle size: 3 μm)

[0067]

[0068] [Example 1] Resin (a)-1, polymerization initiator (c)-1, RAFT agent (1)-1, silver powder and BCA were weighed in a flask and mixed using a stirrer at room temperature to obtain a stretchable wiring paste. Resin (a): The amounts of resin (b), polymerization initiator (c) and RAFT agent were determined so that the ratio of urethane bonds in the resin of the obtained stretchable wiring material was 20 wt % based on 100 parts by mass. In addition, the amount of silver powder was determined so that the ratio of the resin of the obtained stretchable wiring material was 5 wt %. That is, the amount of silver powder was determined so that the ratio of the resin to the silver powder was 8 wt %:92 wt %.

[0069] Next, a sheet sample of the stretchable wiring material was prepared by the above method, and the elongation at break, the resistivity before stretching (ρ0), and the resistivity when the stretching ratio was 50% (ρ 50 ), the resistivity (ρ 100 Table 1 shows the obtained results.

[0070] [Table 1]

[0071] (Examples 2 to 5, Comparative Examples 1 and 2) Examples 2 to 5 and Comparative Examples 1 and 2 were used to prepare sheet samples of stretchable wiring materials in the same manner as in Example 1, except that the amount of silver powder was adjusted so that the resin ratio of the stretchable wiring materials obtained was 10 wt%, 15 wt%, 18 wt%, 20 wt%, 6 wt%, and 22 wt%, respectively. The same properties were measured for the obtained samples. The results are shown in Table 1.

[0072] (Examples 6 to 9, Comparative Examples 3 to 5) In Examples 6 to 9 and Comparative Examples 3 to 5, the proportion of the resin in the obtained stretchable wiring material was 15 wt %, and the proportion of the urethane bond in the resin in the obtained stretchable wiring material was adjusted to 17.5 wt %, 20 wt %, 22 wt %, 25 wt %, 30 wt %, 0 wt %, 10 w %, and 15 wt %, respectively. Sheet-shaped samples of the stretchable wiring material were prepared in the same manner as in Example 1. The same characteristics were measured for the obtained samples. The results are shown in Table 1.

[0073] (Comparative Examples 6 and 7) Comparative Examples 6 and 7 were obtained by applying the stretchable wiring paste and then allowing it to harden without drying and curing. Comparative Example 6 was prepared in the same manner as Comparative Example 5 except that the silver powder did not contain scale-shaped silver powder. Comparative Example 7 used the same stretchable wiring paste as Example 9. The same properties were measured for the obtained samples. The results are shown in Table 1.

[0074] (Examples 10 to 16) In Examples 10 to 16, the proportion of the resin of the obtained stretchable wiring material was 15 wt%, the proportion of urethane bonds in the resin of the obtained stretchable wiring material was 20 mol%, and the proportion of flake-shaped powder in the silver powder was 2.5 wt%, 7.5 wt%, 12.5 wt%, 30 wt%, 40 wt%, and 50 wt%, respectively. Except for this, sheet samples of the stretchable wiring material were prepared in the same manner as in Example 1. The same characteristics were measured for the obtained samples. The results are shown in Table 1.

[0075] The findings obtained from the results in Table 1 are shown. Results without numerical values ​​in Table 1 are the results that could not be measured or were not measured.

[0076] First, Examples 1 to 6 were compared with Comparative Examples 1 and 2. When the ratio of the urethane bond in the resin and the ratio of the flaky powder were fixed to the ratios shown in Table 1, the following findings were obtained. When the proportion of the resin in the wiring material is 8wt% or more (resin: silver powder = 8:92), the elongation at break becomes 130% or more. The higher the proportion of the resin, the higher the elongation at break. On the other hand, when the proportion of the resin is 20wt% or more, the resistivity before expansion becomes 1×10 -2 [Ωcm] or more. By taking into account both higher elongation at break (more than 150%) and lower resistivity before stretching (5×10 -3 [Ωcm] or less), the ratio of the resin in the wiring material is preferably 10 wt % or more and 18 wt % or less. In addition, when the resin ratio is 20 wt% (resin: silver powder = 20:80) (Example 5), the resistivity before expansion is 1.53×10 -2 [Ωcm] is slightly higher, reflecting the high elongation at break, and the resistivity (ρ 50 ) to the resistivity before expansion (ρ0) (ρ 50 / ρ0) is a low change rate of 1.7. In addition, the resistivity (ρ 100 ) and the resistivity (ρ 50 ) ratio (ρ 100 / ρ 50 ) is a sufficiently low rate of change of 4.0. From achieving both high elongation at break (more than 150%) and low ratio (ρ 50 / ρ0) and ratio (ρ 100 / ρ 50 ), the ratio of the resin in the wiring material is preferably 10 wt % or more and 20 wt % or less. In addition, from the simultaneous realization of high elongation at break (more than 150%) and low specific 100 / ρ 50 ) relative to the ratio (ρ 50 From the viewpoint of the change rate of ρ / ρ0), the ratio of the resin in the wiring material is preferably 10 wt % or more and 15 wt % or less. Furthermore, from all the requirements of high elongation at break (more than 150%), low resistivity before expansion, low ratio (ρ 50 / ρ0) and ratio (ρ 100 / ρ 50 ), and low ratio (ρ 100 / ρ 50 ) relative to the ratio (ρ 50 From the viewpoint of the change rate of ρ / ρ0), the ratio of the resin in the wiring material is preferably 10 wt% to 15 wt%.

[0077] Next, Examples 3, 6 to 9 are compared with Comparative Examples 3 and 4. When the ratio of the resin in the wiring material and the ratio of the flaky powder were fixed to the ratios shown in Table 1, the following findings were obtained. When the proportion of urethane bonds in the resin is 15wt% or less, the elongation at break is 40% or less. On the other hand, when the proportion of urethane bonds is 25wt% (Example 8), the elongation at break is 245.5%, but when the proportion of urethane bonds is 30wt% (Example 9), the elongation at break is 130.4%. From the viewpoint of achieving a high elongation at break (above 150%), it is preferred that the proportion of urethane bonds in the resin is 17.5wt% or more and 25wt% or less. In addition, from the viewpoint of achieving both a higher elongation at break (above 150%) and a lower resistivity before expansion (7×10 -3 [Ωcm] or less), it is preferred that the ratio of urethane bonds in the resin is 20 wt% or more and 25 wt% or less. In addition, from the simultaneous realization of high elongation at break (more than 150%) and low specific 50 / ρ0) and ratio (ρ 100 / ρ 50 ), the ratio of urethane bonds in the resin is preferably 17.5 wt % or more and 25 wt % or less. In addition, from the simultaneous realization of high elongation at break (more than 150%) and low specific 100 / ρ 50 ) relative to the ratio (ρ 50 From the viewpoint of the rate of change of ρ / ρ0), the ratio of urethane bonds in the resin is preferably 17.5 wt % or more and 22 wt % or less. Furthermore, from all the requirements of high elongation at break (more than 150%), low resistivity before expansion, low ratio (ρ 50 / ρ0) and ratio (ρ 100 / ρ 50 ), and low ratio (ρ 100 / ρ 50 ) relative to the ratio (ρ 50 From the viewpoint of the rate of change of ρ / ρ0), the ratio of urethane bonds in the resin is preferably 17.5 wt % or more and 22 wt % or less.

[0078] Comparative Examples 6 and 7 are obtained by applying the stretchable wiring paste and then allowing it to undergo a hardening reaction without drying and curing. It can be seen that in Comparative Example 6 where the silver powder does not include scale-shaped silver powder, the resistivity before stretching is 5×10 -1 [Ωcm] is quite high. In addition, in Comparative Example 7 in which the composition of the stretchable wiring paste itself is the same as that of Example 9, the elongation at break is less than 10%, which is not suitable for application in stretchable devices.

[0079] Next, a comparison is made between Examples 3 and 10 to 14. When the ratio of the resin in the wiring material and the ratio of the urethane bond in the resin were fixed to the ratios shown in Table 1, the following findings were obtained. When the proportion of the flaky powder in the silver powder is 40wt% and 50wt%, a negative effect is observed on the elongation at break, and the elongation at break gradually decreases. 100 / ρ 50 ) relative to the ratio (ρ 50 / ρ0) becomes larger than 130%. In addition, when it is 50wt% (Example 14), the ratio (ρ 50 / ρ0) is 51 times. One viewpoint is that when the proportion of the flaky powder in the silver powder is in the range of 2.5wt% to 50wt%, a higher elongation at break (150% or more) and a lower resistivity before stretching (7×10 -3 [Ωcm] or less). From achieving high elongation at break (more than 150%) and low specific tensile strength (ρ 50 / ρ0) and ratio (ρ 100 / ρ 50 ), the ratio of the scaly powder in the silver powder is preferably 2.5 wt % or more and 40 wt % or less. In addition, from the simultaneous realization of high elongation at break (more than 150%) and low specific 100 / ρ 50 ) relative to the ratio (ρ 50From the viewpoint of the change rate of ρ / ρ0), the ratio of the scaly powder in the silver powder is preferably 2.5 wt% or more and 12.5 wt% or less. Furthermore, from all the requirements of high elongation at break (more than 150%), low resistivity before expansion, low ratio (ρ 50 / ρ0) and ratio (ρ 100 / ρ 50 ), and low ratio (ρ 100 / ρ 50 ) relative to the ratio (ρ 50 From the viewpoint of the change rate of ρ / ρ0), the ratio of the scaly powder in the silver powder is preferably 2.5 wt% or more and 12.5 wt% or less.

[0080] By including urethane bonds in the resin, high flexibility can be obtained. In addition, when the resin includes either urethane bonds or siloxane bonds, high elasticity and low resistance can be simultaneously achieved through the improvement effect of dispersion and aggregation of silver powder. Further, when both urethane bonds and siloxane bonds are included, a higher improvement effect can be obtained.

Claims

1. A stretchable wiring material, wherein: Contains resin and metal powder, The elongation at break is more than 130%, The resistivity ρ0 before expansion is 2×10 -2 Ωmm or less, The metal powder includes flake-shaped powder, The ratio of the resin is 8 wt % or more and 20 wt % or less.

2. A stretchable wiring material, wherein: Contains resin and metal powder, The elongation at break is more than 130%, Resistivity ρ when the expansion ratio is 50% 50 The ratio of the resistivity ρ0 before expansion to ρ 50 / ρ0 is less than 7, The metal powder includes flake-shaped powder, The ratio of the resin is 8 wt % or more and 20 wt % or less.

3. The stretchable wiring material according to claim 2, wherein Resistivity ρ when the expansion ratio is 100% 100 The resistivity ρ when the expansion ratio is 50% 50 Ratio 100 / ρ 50 Is below 8.

4. A stretchable wiring material, wherein: Contains resin and metal powder, The elongation at break is more than 130%, Resistivity ρ when the expansion ratio is 100% 100 The resistivity ρ when the expansion ratio is 50% 50 Ratio 100 / ρ 50 , relative to the resistivity ρ when the expansion ratio is 50% 50 The ratio of the resistivity ρ0 before expansion to ρ 50 The change rate of / ρ0 is less than 140%, The metal powder includes flake-shaped powder, The ratio of the resin is 8 wt % or more and 20 wt % or less.

5. The stretchable wiring material according to any one of claims 1 to 4, wherein The resin is cured by drying.

6. The stretchable wiring material according to any one of claims 1 to 5, wherein The ratio of the flaky powder in the metal powder is 2.5 wt % or more and 50 wt % or less.

7. The stretchable wiring material according to any one of claims 1 to 6, wherein The flaky powder has an average maximum particle size of 3 μm or more and 10 μm or less.

8. The stretchable wiring material according to any one of claims 1 to 7, wherein The resin includes a polyurethane resin.

9. A stretchable device, wherein: The stretchable wiring material according to any one of claims 1 to 8 is used.

Citation Information

Patent Citations

  • Stretchable film, method for forming the same, method for manufacturing wiring coated substrate, stretchable wiring film, and method for manufacturing the same

    JP2017206626A