Polyether ester modified organic silicon defoaming agent as well as preparation method and application thereof
Through the layered structure design of polyetherester modified silicone defoamer, the flocculation and layering problems of emulsion silicone defoamer in storage and application are solved, and the defoaming and foaming ability and color paste are improved. Dispersion efficiency.
Patent Information
- Application Number
- CN202411018168.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-05
AI Technical Summary
The existing emulsion silicone defoaming agents are prone to flocculation and layering after long-term storage, which affects the defoaming performance and interferes with the dispersion efficiency of the dispersant in the aqueous color paste, resulting in the fineness of the color paste not meeting the standard.
Using polyetherester modified silicone defoaming agent, the stable silicon paste is formed by condensing end-hydroxydimethyl silicone oil, hydrophobic white carbon black and MQ resin under alkali catalysis, and combined with sodium bentonite and emulsifier. Form a layered structure to improve storage stability and compatibility.
The storage stability of the defoaming agent and the compatibility of the water-based color paste are achieved, the defoaming and foaming ability is enhanced, the dispersion efficiency and wetting efficiency are improved, and flocculation and stratification are avoided.
Smart Images

Figure BDA0004966449690000111 
Figure BDA0004966449690000121
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of defoaming additives, and specifically relates to a polyether ester modified organosilicon defoaming agent and a preparation method and application thereof. Background Art
[0002] In the preparation process of water-based color paste, some surfactants are often used as dispersants, which easily generate a lot of foam during the production process, which not only wastes a lot of container volume, but also increases the activity space of the grinding medium during the grinding process, greatly reducing the grinding efficiency, resulting in the color paste fineness not meeting the requirements, affecting the quality of the color paste. In order to solve this problem, defoaming agents are generally added to reduce the surface tension of the liquid phase, inhibit the generation of foam or eliminate the generated foam.
[0003] Emulsion-type silicone defoamers are easy to disperse in water-based systems and are a common defoamer in the production process of water-based color pastes. They are generally composed of polyether-modified silicone, silicone paste, emulsifier, additives and water. Through the coordinated effect of various components, they have the characteristics of high temperature resistance, acid and alkali resistance, low dosage, high efficiency and long-lasting defoaming. However, common emulsion-type silicone defoamers will flocculate and stratify after long-term storage, which will reduce the defoaming performance of the product. After being added to the color paste slurry, it will also interfere with the dispersion system of the dispersant with a polyether solvated segment, resulting in reduced dispersion efficiency. Summary of the invention
[0004] The purpose of the present invention is to provide a polyether ester modified silicone defoamer and a preparation method and application thereof. The polyether ester modified silicone defoamer provided by the present invention has excellent defoaming and foam suppression capabilities, as well as excellent storage stability and compatibility with water-based color paste.
[0005] In order to achieve the above object, the present invention provides the following technical solutions:
[0006] The invention provides a polyether ester modified organic silicon defoamer, comprising the following raw materials in percentage by weight: 15-25% of polyether ester modified organic silicon, 10-20% of silicone paste, 0.5-1% of sodium bentonite, 5-10% of emulsifier and the balance of water;
[0007] The preparation method of the silicone paste comprises the following steps: mixing terminal hydroxy dimethyl silicone oil, hydrophobic white carbon black, MQ resin and alkali, and performing a first condensation reaction to obtain the silicone paste.
[0008] Preferably, the mass ratio of the terminal hydroxy dimethyl silicone oil to the hydrophobic white carbon black is 85-90:5-10;
[0009] The mass ratio of the terminal hydroxy dimethyl silicone oil to the MQ resin is 85-90:5-10;
[0010] The alkali is potassium hydroxide or sodium hydroxide; the mass ratio of the terminal hydroxy dimethyl silicone oil to the alkali is 85-90:0.5-1.
[0011] Preferably, the temperature of the first condensation reaction is 140-180° C., and the time is 3-5 hours.
[0012] Preferably, the preparation method of the polyether ester modified silicone comprises the following steps:
[0013] The allyl polyether, fatty acid and esterification catalyst are mixed to carry out esterification reaction to obtain polyether ester;
[0014] The polyether ester, silicone oil and condensation catalyst are mixed and subjected to a second condensation reaction to obtain the polyether ester modified silicone.
[0015] Preferably, the fatty acid is a single-chain fatty acid; the number of carbon atoms in the single-chain fatty acid is 10 to 18;
[0016] The esterification catalyst includes one or more of p-toluenesulfonic acid, benzenesulfonic acid and tetraisobutyl titanate;
[0017] The temperature of the esterification reaction is 150-200° C., and the time is 5-8 hours; the esterification reaction is carried out under a nitrogen environment.
[0018] Preferably, the silicone oil is low-hydrogen silicone oil; the mass percentage of hydrogen in the silicone oil is 0.1-0.2%; the molecular weight of the silicone oil is 1500-2500;
[0019] The condensation catalyst is chloroplatinic acid;
[0020] The temperature of the second condensation reaction is 140-160° C., and the time is 5-8 hours; the condensation reaction is carried out under a nitrogen environment.
[0021] Preferably, the emulsifier includes two or more of Span-20, Span-60, Span-80, Tween-60, Tween-80, EL-40, EL-80, SG-40, AEO-9 and Piperidin.
[0022] The present invention also provides a method for preparing the polyether modified silicone defoamer described in the above technical solution, comprising the following steps:
[0023] first mixing sodium bentonite and water to obtain a bentonite dispersion;
[0024] The polyether ester modified silicone, silicone paste and emulsifier are mixed for the second time to obtain a mixed material;
[0025] The bentonite dispersion is added into the mixed material for emulsification and diversion to obtain the polyether ester modified organosilicon defoamer.
[0026] Preferably, the first mixing is stirring; the stirring speed is 500-1000 r / min, and the time is more than 1 hour;
[0027] The second mixing is stirring; the stirring speed is 1000-2000 r / min, and the time is more than 1 hour;
[0028] The mass ratio of the amount of the bentonite dispersion added per minute to the polyether modified silicone defoamer is 1-2wt%:1; the bentonite dispersion is added under stirring; the stirring speed is 2500-20000r / min; and stirring is also performed for 10-20min after the bentonite dispersion is added.
[0029] The present invention also provides the use of the polyether ester modified silicone defoamer described in the above technical solution or the polyether ester modified silicone defoamer prepared by the preparation method described in the above technical solution in color paste.
[0030] The invention provides a polyether ester modified organic silicon defoamer, comprising the following raw materials in percentage by weight: 15-25% of polyether ester modified organic silicon, 10-20% of silicone paste, 0.5-1% of sodium bentonite, 5-10% of emulsifier and the balance of water; the preparation method of the silicone paste comprises the following steps: mixing terminal hydroxy dimethyl silicone oil, hydrophobic white carbon black, MQ resin and alkali, and performing a first condensation reaction to obtain the silicone paste. In the defoamer provided by the present invention, MQ silicone resin, hydrophobic white carbon black, and terminal hydroxyl dimethyl silicone oil all have hydroxyl groups or carboxyl groups. Under the catalysis of alkali, hydroxyl groups on the surfaces of MQ silicone resin and hydrophobic white carbon black are connected by dehydration condensation with terminal hydroxyl groups in terminal hydroxyl dimethyl silicone oil, and the silicone resin is stretched into a network branch structure, so that the silicone paste forms a structure mainly composed of dimethyl silicone oil and MQ silicone resin as a skeleton, which stably wraps the hydrophobic white carbon black and has strong stability. In an aqueous system, sodium bentonite expands into layered flakes as water molecules are inserted, and the flakes have a negative charge layer and can form a stable non-continuous layered flake suspension. Droplets of polyether ester modified organic silicone and silicone paste after self-emulsification and emulsification by an emulsifier are confined between limited layered flakes, so that it is not easy for the oil phase and the water phase of the emulsified system to have a droplet concentration gradient, thereby making the defoamer have excellent storage stability.
[0031] Moreover, in the defoamer provided by the present invention, the access of fatty acid anhydride makes the hydrophilicity of polyether ester modified silicone further decrease compared with traditional polyether modified silicone, weakens the hydrogen bond force between polyoxyethylene ether and water, is conducive to the decrease of surface tension, makes the defoamer more active, and has higher defoaming ability. Moreover, due to the decrease of this hydrophilicity, its hydrophilicity is weaker than that of dispersant, and the defoamer itself has no pigment affinity group, making the defoamer more easily dispersed at the interface of air (bubble) and water phase, and making the efficiency of defoaming and degassing higher, and even can help the dispersant to drain the air fixed by the pigment structure, improve the wetting efficiency, and then improve the dispersion efficiency. DETAILED DESCRIPTION
[0032] The invention provides a polyether ester modified organic silicon defoamer, comprising the following raw materials in percentage by weight: 10-20% of silicone paste, 15-25% of polyether ester modified organic silicon, 0.5-1% of sodium bentonite, 5-10% of emulsifier and the balance of water;
[0033] The preparation method of the silicone paste comprises the following steps: mixing terminal hydroxy dimethyl silicone oil, hydrophobic white carbon black, MQ resin and alkali, and performing a first condensation reaction to obtain the silicone paste.
[0034] In the present invention, unless otherwise specified, all raw material components are commercially available products well known to those skilled in the art.
[0035] In the present invention, the raw materials of the polyether ester modified organic silicon defoamer include 10-20% of silicone paste, preferably 10-15%.
[0036] In the present invention, the viscosity of the terminal hydroxy dimethyl silicone oil is preferably one or more of 500 mPa.s, 750 mPa.s, 1000 mPa.s, 1250 mPa.s and 1500 mPa.s.
[0037] In the present invention, the hydrophobic silica is preferably hydrophobic fumed silica, more preferably DM-20S silica produced by Tokuyama; the specific surface area of the hydrophobic silica is preferably 150 to 300 m 2 / g, more preferably 200 to 250 m 2 / g; the mass ratio of the terminal hydroxy dimethyl silicone oil to the hydrophobic white carbon black is preferably 85-90:5-10, and more preferably 87-90:5-8.
[0038] In the present invention, the mass ratio of the terminal hydroxy dimethyl silicone oil to the MQ resin is preferably 85-90:5-10, and more preferably 87-90:5-8.
[0039] In the present invention, the alkali is preferably potassium hydroxide or sodium hydroxide; the alkali is preferably an alkali solution; the mass percentage of the alkali in the alkali solution is preferably 10%; the solvent is preferably isopropanol; the addition amount of the alkali is preferably 50 to 500 ppm, more preferably 100 to 300 ppm.
[0040] In the present invention, the mixing is preferably stirring; the stirring speed is 150 to 500 r / min, more preferably 300 to 500 r / min.
[0041] In the present invention, the temperature of the first condensation reaction is preferably 140-180° C., more preferably 160-170° C.; the time is preferably 3-5 hours, more preferably 4-5 hours; the first condensation reaction is preferably carried out under stirring conditions.
[0042] In the present invention, the raw material of the polyether ester modified silicone defoamer includes 15-25% of polyether ester modified silicone, preferably 15-20%.
[0043] In the present invention, the preparation method of the polyether ester modified silicone preferably comprises the following steps:
[0044] The allyl polyether, fatty acid and esterification catalyst are mixed to carry out esterification reaction to obtain polyether ester;
[0045] The polyether ester, silicone oil and condensation catalyst are mixed and subjected to a second condensation reaction to obtain the polyether ester modified silicone.
[0046] The invention mixes allyl polyether, fatty acid and esterification catalyst to carry out esterification reaction to obtain polyether ester.
[0047] In the present invention, the allyl polyether is preferably a GPE type polyether; the source of the allyl polyether is preferably Shanghai Beko Chemical Allyl Polyether L-62.
[0048] In the present invention, the fatty acid is preferably a single-chain fatty acid; the number of carbon atoms in the single-chain fatty acid is preferably 10 to 18, more preferably 12 to 18; the fatty acid is preferably lauric acid or stearic acid; the molar ratio of the allyl polyether to the fatty acid is preferably 1:1.15 to 1.5, more preferably 1:1.2 to 1.4.
[0049] In the present invention, the esterification catalyst preferably includes p-toluenesulfonic acid, benzenesulfonic acid or tetraisobutyl titanate, more preferably p-toluenesulfonic acid or tetraisobutyl titanate; the mass of the esterification catalyst is preferably 0.3-1.5% of the total mass of allyl polyether and fatty acid, more preferably 0.5-1%.
[0050] In the present invention, the temperature of the esterification reaction is preferably 150-200°C, more preferably 180-190°C; the time is preferably 5-8h, more preferably 6-7h; the esterification reaction is preferably carried out under a nitrogen atmosphere; the process of heating to the esterification reaction temperature preferably includes stirring; the stirring speed is 150-500r / min, more preferably 300-500r / min; the water generated by the esterification reaction is preferably promptly pumped away under negative pressure.
[0051] After obtaining the polyether ester, the present invention mixes the polyether ester, silicone oil and a condensation catalyst to carry out a second condensation reaction to obtain the polyether ester modified silicone.
[0052] In the present invention, the mass percentage of hydrogen in the silicone oil is preferably 0.1-0.2%, more preferably 0.18%; the molecular weight of the silicone oil is preferably 1500-2500, more preferably 2000-2500; the molar ratio of active hydrogen in the polyether ester and low hydrogen silicone oil is preferably 1.1-1.3:1, more preferably 1.1-1.2:1.
[0053] In the present invention, the second catalyst is preferably chloroplatinic acid; the chloroplatinic acid is preferably a chloroplatinic acid solution; the mass percentage of chloroplatinic acid in the chloroplatinic acid solution is preferably 1%; the solvent is preferably isopropanol; the addition amount of the second catalyst is preferably 20 to 100 ppm, more preferably 50 ppm.
[0054] In the present invention, the temperature of the second condensation reaction is preferably 140-160°C, more preferably 150-160°C; the time is preferably 5-8h, more preferably 6-7h; the second condensation reaction is preferably carried out under a nitrogen atmosphere; the second condensation reaction is preferably carried out under vacuum dehydration conditions; the process of heating to the second condensation reaction temperature preferably includes stirring; the stirring speed is 150-300r / min, more preferably 300r / min; the water generated by the second condensation reaction is preferably promptly pumped away under negative pressure.
[0055] In the present invention, the raw materials of the polyether ester modified silicone defoamer include 0.5-1%, preferably 0.5-0.8% of sodium bentonite; the sodium bentonite is preferably white sodium bentonite.
[0056] In the present invention, the raw materials of the polyether modified silicone defoamer include 5-10% of emulsifier, preferably 5-8%; the emulsifier preferably includes two or more of Span-20, Span-60, Span-80, Tween-60, Tween-80, EL-40, EL-80, SG-40, AEO-9 and Pingpingjia, more preferably three or more of Span-80, Tween-60, Tween-80, EL-40, SG-40 and AEO-9; the HLB value of the emulsifier is preferably 10-11.5, more preferably 10.5-11; the present invention does not have any special limitation on the specific ratio of the emulsifier.
[0057] In the defoamer provided by the present invention, MQ silicone resin, hydrophobic white carbon black, and terminal hydroxyl dimethyl silicone oil all have hydroxyl groups or carboxyl groups. Under the catalysis of alkali, hydroxyl groups on the surfaces of MQ silicone resin and hydrophobic white carbon black are connected by dehydration condensation with terminal hydroxyl groups in terminal hydroxyl dimethyl silicone oil, and the silicone resin is stretched into a network branch structure, so that the silicone paste forms a structure mainly composed of dimethyl silicone oil and MQ silicone resin as a skeleton, which stably wraps the hydrophobic white carbon black and has strong stability. In an aqueous system, sodium bentonite expands into layered flakes as water molecules are inserted, and the flakes have a negative charge layer and can form a stable non-continuous layered flake suspension. Droplets of polyether ester modified organic silicone and silicone paste after self-emulsification and emulsification by an emulsifier are confined between limited layered flakes, so that it is not easy for the oil phase and the water phase of the emulsified system to have a droplet concentration gradient, thereby making the defoamer have excellent storage stability.
[0058] Moreover, in the defoamer provided by the present invention, the access of fatty acid anhydride makes the hydrophilicity of polyether ester modified silicone further decrease compared with traditional polyether modified silicone, weakens the hydrogen bond force between polyoxyethylene ether and water, is conducive to the decrease of surface tension, makes the defoamer more active, and has higher defoaming ability. Moreover, due to the decrease of this hydrophilicity, its hydrophilicity is weaker than that of dispersant, and the defoamer itself has no pigment affinity group, making the defoamer more easily dispersed at the interface of air (bubble) and water phase, and making the efficiency of defoaming and degassing higher, and even can help the dispersant to drain the air fixed by the pigment structure, improve the wetting efficiency, and then improve the dispersion efficiency.
[0059] The present invention also provides a method for preparing the polyether modified silicone defoamer described in the above technical solution, comprising the following steps:
[0060] first mixing sodium bentonite and water to obtain a bentonite dispersion;
[0061] The polyether ester modified organic silicon, silicone paste and emulsifier are mixed for the second time to obtain a mixed material;
[0062] The bentonite dispersion is added into the mixed material for emulsification and diversion to obtain the polyether ester modified organosilicon defoamer.
[0063] The present invention first mixes sodium bentonite and water to obtain a bentonite dispersion.
[0064] In the present invention, the first mixing is preferably stirring; the stirring speed is preferably 500-1000r / min, more preferably 800-1000r / min; the time is preferably more than 1h, more preferably 1-2h; the role of the first mixing is to make the organic bentonite form a stable non-continuous lamellar flake suspension under the action of high-speed shear force.
[0065] The present invention performs a second mixing of polyether ester modified organic silicon, silicone paste and emulsifier to obtain a mixed material.
[0066] In the present invention, the second mixing is preferably stirring; the stirring speed is preferably 1000-2000r / min, more preferably 1300-1500r / min; the time is more than 1h, more preferably 1-2h; the role of the second mixing is to make the emulsifier thoroughly disperse and wrap the silicone paste and polyether ester modified silicone oil.
[0067] After obtaining the bentonite dispersion and the mixed material, the present invention adds the bentonite dispersion into the mixed material for emulsification and diversion to obtain the polyether ester modified organosilicon defoamer.
[0068] In the present invention, the mass ratio of the amount of the bentonite dispersion added per minute to the polyether modified silicone defoamer is preferably 1-2wt%:1, more preferably 1.5-2wt%:1; the addition of the bentonite dispersion is carried out under stirring conditions; the stirring speed is 2500-20000r / min, more preferably 5000-15000r / min; after adding the bentonite dispersion, stirring is also included for 10-20min, more preferably 10-15min.
[0069] In the present invention, after the emulsification is turned, it is preferred to further include replenishing lost water and stirring; the present invention does not have any special limitation on the amount of the water replenished, which can be equal to the amount of material loss in the preparation process; the present invention does not have any special limitation on the stirring process, which can make the obtained polyether modified silicone defoamer uniform and stable.
[0070] Compared with adding bentonite after emulsification, the preparation method provided by the present invention not only reduces the dispersion difficulty of adding after emulsification, but also avoids the demulsification caused by the bentonite competing for water molecules. At the same time, the pre-formed negatively charged bentonite layered flakes can also help the droplets after emulsification to be dispersed more evenly.
[0071] The present invention also provides the use of the polyether ester modified silicone defoamer described in the above technical solution or the polyether ester modified silicone defoamer prepared by the preparation method described in the above technical solution in color paste.
[0072] In the present invention, the color paste is preferably a water-based color paste; the mass percentage of the polyether modified silicone defoamer in the color paste is preferably 0.1-0.3%, more preferably 0.1-0.12%. The present invention does not have any special restrictions on the application process of the polyether modified silicone defoamer in the color paste, and it can be carried out in a manner well known to those skilled in the art.
[0073] In order to further illustrate the present invention, the polyether ester modified silicone defoamer provided by the present invention and its preparation method and application are described in detail below in conjunction with embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0074] Example 1
[0075] Add 250 g of allyl polyether L-62, 28.5 g of lauric acid and 1.4 g of tetraisobutyl titanate into a pressure-resistant reaction vessel, fill the reaction vessel with nitrogen, stir at a speed of 300 r / min and heat to 190° C., keep stirring and react for 6 hours to obtain polyether ester.
[0076] 134.5 g of polyether ester and 32 g of hydrogen-containing silicone oil with a molecular weight of 2000 and a hydrogen content of 0.18% were added to a pressure-resistant reaction vessel, the temperature was raised to 140° C. with stirring at a speed of 300 r / min, 50 ppm of chloroplatinic acid catalyst was added, and the reaction was stirred for 5 hours under vacuum dehydration conditions to obtain polyether ester modified silicone.
[0077] Add 30 g each of terminal hydroxy dimethyl silicone oil with viscosities of 500 mPa.s, 1000 mPa.s and 1500 mPa.s into a reaction container, add 5 g of MQ silicone resin, 5 g of DM-20S white carbon black produced by Deshan, add 100 ppm of 10% isopropanol solution of sodium hydroxide, stir at a speed of 300 r / min and raise the temperature to 150°C, keep the reaction warm for 4 hours to obtain a silicone paste.
[0078] 59.2 g of water and 0.8 g of sodium bentonite were added to a stirring container and stirred at a speed of 1000 r / min for 1.5 h to obtain a bentonite dispersion.
[0079] Add 25 g of polyether ester modified silicone, 10 g of silicone paste, and 5 g of compound emulsifier (the ratio of Span-80: Tween-80: SG-40 is 2.4:0.9:1.8, and the HLB value is 10.5) into a stirring container, stir at a speed of 1500 r / min for 1.5 h to obtain a mixed material.
[0080] Add bentonite dispersion to the mixture at a speed of 10 g / min, stir at a speed of 5000 r / min until the addition is complete, continue stirring for 10 minutes to complete emulsification, then add the lost water to 100 g, stir evenly, and filter to obtain the polyether ester modified silicone defoamer.
[0081] Example 2
[0082] The polyether ester modified silicone defoamer was prepared according to the technical scheme provided in Example 1, except that the emulsification process was as follows:
[0083] 54.2 g of water and 0.8 g of sodium bentonite were added to a stirring container and stirred at a speed of 1000 r / min for 1.5 h to obtain a bentonite dispersion.
[0084] Add 20 g of polyether ester modified silicone, 15 g of silicone paste, and 10 g of compound emulsifier (the ratio of Span-80: Tween-80: SG-40 is 2.4:0.9:1.8, and the HLB value is 10.5) into a stirring container, stir at a speed of 1500 r / min for 1.5 h to obtain a mixed material.
[0085] Add bentonite dispersion to the mixture at a speed of 10 g / min, stir at a speed of 5000 r / min until the addition is complete, continue stirring for 10 minutes to complete emulsification, then add the lost water to 100 g, stir evenly, and filter to obtain the polyether ester modified silicone defoamer.
[0086] Example 3
[0087] The polyether ester modified silicone defoamer is prepared according to the technical scheme provided in Example 1, except that the preparation steps of the polyether ester modified silicone are as follows:
[0088] Add 250 g of allyl polyether L-62, 32.9 g of stearic acid and 2 g of p-toluenesulfonic acid into a pressure-resistant reaction vessel, fill the reaction vessel with nitrogen, stir at a speed of 300 r / min and heat to 190° C., keep stirring and react for 6 hours to obtain polyether ester.
[0089] 138.7 g of polyether ester and 39 g of low-hydrogen silicone oil with a molecular weight of 2500 were added to a pressure-resistant reaction vessel, the temperature was raised to 150° C. with stirring at a speed of 300 r / min, 50 ppm of chloroplatinic acid catalyst was added, and the reaction was continued with stirring for 5 hours under vacuum dehydration conditions to obtain polyether ester modified silicone.
[0090] Example 4
[0091] The polyether ester modified silicone defoamer was prepared according to the technical scheme provided in Example 1, except that the preparation steps of the silicone paste were as follows:
[0092] Add 90g of 500mPa.s terminal hydroxy dimethyl silicone oil, 5gMQ silicone resin, 5g of Deshan's DM-20S white carbon black, and 100ppm of 10% isopropanol solution of sodium hydroxide into the reaction container, stir at 300r / min and heat to 150°C, keep warm for 4h to obtain silicone paste.
[0093] Comparative Example 1
[0094] A polyether ester modified silicone defoamer was prepared according to the technical scheme provided in Example 1, except that the polyether ester modified silicone oil was replaced by a commercially available polyether modified silicone oil.
[0095] Comparative Example 2
[0096] A polyetherester modified silicone defoamer was prepared according to the technical scheme provided in Example 1, except that no sodium bentonite was added.
[0097] Comparative Example 3
[0098] The polyether ester modified silicone defoamer was prepared according to the technical scheme provided in Example 1, except that MQ silicone resin was not added in the preparation of the silicone paste. The specific preparation steps are as follows:
[0099] Add 30g of terminal hydroxy dimethyl silicone oil with a viscosity of 500mpa.s, 1000mpa.s, and 1500mpa.s, 10g of DM-20S white carbon black from Deshan, add 100ppm of 10% isopropanol solution of sodium hydroxide, stir at a speed of 300r / min and heat to 150℃, keep warm and react for 4h to obtain silicone paste.
[0100] Test Example 1
[0101] After fully stirring Examples 1 to 4, Comparative Examples 1 to 3 and a commercially available emulsion-type polyether-modified silicone (Sanyue high molecular weight SY-2152W), the mixture was allowed to stand at room temperature to observe the changes. The results are shown in Table 1.
[0102] Table 1 Defoamer stability observation test results
[0103] 3 days later 7 days later 1 month later 3 months later 6 months later Example 1 No change No change No change No change No change Example 2 No change No change No change No change No change Example 3 No change No change No change No change No change Example 4 No change No change No change No change No change Comparative Example 1 No change No change No change No change No change Comparative Example 2 No change No change Slight delamination Severe stratification Coagulation and demulsification Comparative Example 3 No change No change Slight flocculation Severe flocculation Coagulation and demulsification SY-2152W No change No change No change Slight delamination Severe stratification
[0104] As can be seen from Table 1, the defoamer prepared by the present invention has certain advantages over the commercially available emulsion-type organosilicon defoamer in terms of long-term storage stability, wherein the addition of silicone resin and organobentonite plays a key role in the storage stability of the defoamer.
[0105] Test Example 2
[0106] The water-based color paste was prepared according to the formula in Table 2, and the defoaming ability test, defoaming efficiency test and foam inhibition ability test were carried out respectively.
[0107] Table 2 Water-based color paste formula
[0108] Pigment PW6 50wt% Dispersant (Pingpingjia O-20) 5wt% water 44wt% Thickener (Sanyue molecular SY-1053) 1wt%
[0109] Defoaming ability test: Take 5 beakers respectively, take 200g of water-based color paste into each beaker, stir to a specific liquid level at a disperser speed of 1500r / min, add 1g of Examples 1-4, Comparative Example 1 and a commercially available emulsion polyether modified silicone (Sanyue high molecular SY-2152W) defoamer, continue stirring, observe and record the time required for complete defoaming.
[0110] Antifoaming ability test: Take 5 beakers respectively, take 200g of water-based color paste in each beaker, add 1g of Examples 1-4, Comparative Example 1 and commercially available emulsion polyether modified silicone (Sanyue high molecular SY-2152W) defoamer, continue stirring, increase the speed of the disperser to 2000r / min, observe and record the time when the liquid level reaches a specific height. The results of the defoaming ability test and the antifoaming ability test are shown in Table 3.
[0111] Table 3 Defoamer ability test results
[0112] Defoaming time Anti-foam time Example 1 11 102min Example 2 13 105min Example 3 11 101min Example 4 15 102min Comparative Example 1 20 94min Mitsukoshi SY-2152W 19 74min
[0113] As can be seen from Table 3, in Examples 1 to 4 prepared by the present invention, since the hydrophilicity of polyether ester modified silicone is weaker than that of polyether modified silicone oil, the hydrogen bonding force between polyoxyethylene ether and water is weakened, which is conducive to the decrease of surface tension, making the defoamer more active and having higher defoaming ability. In addition, due to the decrease of hydrophilicity, its hydrophilicity is weaker than that of the dispersant, and the defoamer itself has no pigment affinity group, making it easier for the defoamer to disperse at the interface between air (bubbles) and the water phase, making the defoaming efficiency higher, which is manifested as a shorter defoaming time. At the same time, due to the decrease of hydrophilicity of polyether ester modified silicone oil, and the stable three-dimensional structure constructed by MQ silicone resin, terminal hydroxy dimethyl silicone oil, and hydrophobic white carbon black, the defoamer is not easily solubilized by the aqueous system, and the anti-foaming ability is greatly improved.
[0114] Test Example 3
[0115] The water-based color paste was prepared according to the formula in Table 4, and the particle size test of the water-based color paste during stirring and dispersion was carried out. The defoamers were respectively Examples 1-4, Comparative Example 1, a commercially available emulsion type polyether modified silicone (Sanyue high molecular weight SY-2152W), and a blank.
[0116] Table 4 Water-based color paste formula
[0117]
[0118]
[0119] Particle size test of water-based color paste during stirring and dispersion: The water-based color paste was stirred and dispersed at a speed of 2500r / min. After 30min and 1h respectively, the particle size D97 (um) of the pigment was tested using a laser particle size tester. The test results are shown in Table 5.
[0120] Table 5 Particle size test results of water-based color paste stirring and dispersion process
[0121] Particle size D97 (30min) Particle size D97(1h) Example 1 10.35 7.89 Example 2 12.46 7.915 Example 3 11.578 7.93 Example 4 12.4 8.1 Comparative Example 1 16.88 11.55 Mitsukoshi SY-2152W 15.5 11.53 blank 15.37 8.75
[0122] As can be seen from Table 5, Comparative Example 1 and the commercially available product SY-2152W affect the dispersion efficiency of the water-based color paste, while Examples 1-4 of the present invention not only do not affect it, but even promote the dispersion process in the early stage of dispersion, thereby improving the dispersion efficiency.
[0123] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A polyether modified silicone defoamer, characterized in that: The preparation method comprises the following raw materials in percentage by weight: 15-25% of polyether ester modified silicone, 10-20% of silicone paste, 0.5-1% of sodium bentonite, 5-10% of emulsifier and the balance of water; The preparation method of the silicone paste comprises the following steps: mixing terminal hydroxy dimethyl silicone oil, hydrophobic white carbon black, MQ resin and alkali, and performing a first condensation reaction to obtain the silicone paste.
2. The polyether modified silicone defoamer according to claim 1, characterized in that: The mass ratio of the terminal hydroxy dimethyl silicone oil to the hydrophobic white carbon black is 85-90:5-10; The mass ratio of the terminal hydroxy dimethyl silicone oil to the MQ resin is 85-90:5-10; The base is potassium hydroxide or sodium hydroxide; the mass ratio of the terminal hydroxy dimethyl silicone oil to the base is 85 to 90: 0.5~1。 3. The polyether modified silicone defoamer according to claim 1 or 2, characterized in that: The temperature of the first condensation reaction is 140-180° C., and the time is 3-5 hours.
4. The polyether modified silicone defoamer according to claim 1, characterized in that: The preparation method of the polyether ester modified silicone comprises the following steps: Allyl polyether, fatty acid and esterification catalyst are mixed to carry out esterification reaction to obtain polyether ester; The polyether ester, silicone oil and condensation catalyst are mixed and subjected to a second condensation reaction to obtain the polyether ester modified silicone.
5. The polyether modified silicone defoamer according to claim 4, characterized in that: The fatty acid is a single-chain fatty acid; the number of carbon atoms in the single-chain fatty acid is 10 to 18; The esterification catalyst includes one or more of p-toluenesulfonic acid, benzenesulfonic acid and tetraisobutyl titanate; The temperature of the esterification reaction is 150-200° C., and the time is 5-8 hours; the esterification reaction is carried out under a nitrogen environment.
6. The polyether modified silicone defoamer according to claim 4, characterized in that: The silicone oil is low-hydrogen silicone oil; the mass percentage of hydrogen in the silicone oil is 0.1-0.2%; the molecular weight of the silicone oil is 1500-2500; The condensation catalyst is chloroplatinic acid; The temperature of the second condensation reaction is 140-160° C., and the time is 5-8 hours; the condensation reaction is carried out under a nitrogen environment.
7. The polyether modified silicone defoamer according to claim 1, characterized in that: The emulsifier includes two or more of Span-20, Span-60, Span-80, Tween-60, Tween-80, EL-40, EL-80, SG-40, AEO-9 and Pipinga.
8. The method for preparing the polyether modified silicone defoamer according to any one of claims 1 to 7, characterized in that: The following steps are involved: first mixing sodium bentonite and water to obtain a bentonite dispersion; The polyether ester modified silicone, silicone paste and emulsifier are mixed for the second time to obtain a mixed material; The bentonite dispersion is added to the mixed material and emulsified to obtain the polyether ester modified silicone defoamer.
9. The preparation method according to claim 8, characterized in that The first mixing is stirring; the stirring speed is 500 to 1000 r / min, and the time is more than 1 hour; The second mixing is stirring; the stirring speed is 1000-2000 r / min, and the time is more than 1 hour; The mass ratio of the bentonite dispersion added per minute to the polyether modified silicone defoamer is 1 to 2 wt%:1; the bentonite dispersion is added under stirring conditions; the stirring speed is 2500 to 20000 r / min; and stirring is further performed for 10 to 20 minutes after the bentonite dispersion is added.
10. Use of the polyether ester modified silicone defoamer according to any one of claims 1 to 7 or the polyether ester modified silicone defoamer prepared by the preparation method according to claim 8 or 9 in color paste.
Citation Information
Patent Citations
High-efficiency defoaming agent for biological fermentation system and preparation process of high-efficiency defoaming agent
CN102940982A
Organic silicon defoamer and preparation method thereof
CN103641195A
Organic silicon defoamer for paper making industry and preparation method thereof
CN103669108A
Polyether modified organic silicon defoamer, and preparation method and application thereof
CN103819630A
Preparation method of defoaming agent resistant to high temperature and strong alkali
CN105561634A