Modified lithium ion battery negative electrode carbon adsorbent and preparation method and application thereof
The fluorine-depleted adsorbent is prepared by low-temperature baking of modified lithium-ion battery negative electrode carbon slag and aluminum and cerium salts, which solves the problems of lithium-ion battery recycling and fluorine pollution, and achieves high-efficiency fluorine ion adsorption and removal effects with low energy consumption and low cost. Promote the resource utilization of carbon slag for negative electrodes of lithium-ion batteries and the control of fluorine pollution.
Patent Information
- Application Number
- CN202411164709.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-05
AI Technical Summary
In the recycling of existing lithium-ion batteries, waste negative electrode carbon materials cannot be effectively utilized, resulting in environmental pollution and waste of resources. At the same time, the preparation process of existing fluorine ion adsorbents consumes energy, is complex and has limited applicability, so it is impossible to effectively remove fluorine-containing wastewater. fluoride ions in it.
The preparation method of modified lithium-ion battery negative electrode carbon adsorbent is prepared by calculating the lithium-ion battery negative electrode carbon slag with aluminum salt and cerium salt at low temperature, and the fluorine-depleted adsorbent is prepared using its high specific surface area and loaded aluminum and cerium. Oxides achieve efficient adsorption and removal of fluoride ions.
It realizes a low energy consumption, simple preparation process, low production cost, and the adsorbent surface is rich in active groups and metal ion sites. It can quickly and effectively remove fluoride ions in water, reduce it to industrial emission standards, and solve the negative electrode of lithium-ion battery Carbon slag resource treatment and fluorine pollution problems.
Smart Images

Figure BDA0005007513660000161 
Figure BDA0005007513660000171 
Figure BDA0005007513660000172
Abstract
Description
Technical Field
[0001] This invention relates to the field of fluorine adsorbents, and more particularly to a modified carbon adsorbent for lithium-ion battery anodes, its preparation method, and its application. Background Technology
[0002] With the rapid development of the new energy industry, lithium-ion batteries have been widely used in various fields due to their excellent performance. However, the average lifespan of lithium-ion batteries is only 3-5 years, resulting in a huge number of retired lithium-ion batteries. Typically, discarded lithium-ion batteries are disposed of as regular solid waste, causing environmental pollution and even other safety hazards. Therefore, there is an urgent need for effective recycling methods and a well-developed recycling market.
[0003] Graphite, a non-renewable resource, accounts for approximately 12-21 wt.% of waste lithium-ion batteries. With the increasing number of discarded lithium-ion batteries, the stock of waste negative electrode carbon materials has become enormous and inexpensive. China is the world's second-largest graphite mining country, but also the world's largest graphite supplier. With the continuous growth in graphite demand, my country's graphite supply will face certain pressures. Currently, the focus of lithium-ion battery recycling is mainly on the positive electrode, because the positive electrode contains a large amount of valuable metals, including iron, cobalt, and nickel. Compared to the metals in the battery, waste graphite has lower utilization value. In industrial processes, graphite is often burned in combustion chambers or directly discarded as waste residue, which is detrimental to sustainable environmental development.
[0004] my country is one of the countries most severely and extensively affected by fluoride pollution, with approximately 2.2 million square kilometers of water bodies suffering from varying levels of fluoride contamination, and about 50 million people drinking high-fluoride water. Fluoride-containing wastewater mainly originates from industries such as metallurgy, fluorochemical production, semiconductors, electroplating, metal processing, phosphate fertilizers, and pesticide production. Due to the properties of fluoride and technological limitations, these industries generate large volumes of wastewater with high fluoride content. Direct discharge without treatment can cause irreparable damage to surrounding soil and water resources, leading to regional fluorosis and even poisoning of humans and livestock. Therefore, strict control of fluoride levels in water bodies is crucial. The environmental hazards of fluoride have now become a focus of attention in environmental science and hygiene.
[0005] Patent application number WO2024119629 discloses a method for preparing a fluoride ion adsorbent. The method involves wet acid leaching and calcination of a first mixture containing negative electrode graphite material obtained from a lithium-ion battery to obtain calcined residue. This residue is then nitrogen-doped and calcined, and then mixed with manganese salts, aluminum salts, aluminates, and auxiliary agents to form a slurry. Metal precipitation is then performed under alkaline conditions. The slurry is aged, filtered, washed to neutral, and dried to obtain a metal hydroxide-carbon composite. The metal hydroxide-carbon composite is then calcined to obtain the fluoride ion adsorbent. This method requires acid leaching and alkaline calcination to remove impurities from the negative electrode graphite material, resulting in high energy consumption. Subsequent modification processes involve nitrogen doping, calcination, slurry preparation, pH adjustment, aging, filtration, washing, and calcination, making the preparation process lengthy and complex, involving numerous chemical reagents. Furthermore, its applicability is not very wide. Summary of the Invention
[0006] Against the above background, the present invention provides a modified lithium-ion battery negative electrode carbon adsorbent with low production cost and good defluorination adsorption effect.
[0007] This invention also provides a method for preparing modified lithium-ion battery negative electrode carbon adsorbent, which has low energy consumption and a simple preparation process.
[0008] This invention also provides the application of modified lithium-ion battery negative electrode carbon adsorbent in fluoride-containing wastewater.
[0009] To achieve the above objectives, the technical solution adopted by the present invention is as follows:
[0010] A method for preparing a modified carbon adsorbent for the negative electrode of a lithium-ion battery includes the following steps:
[0011] S1. Fine carbon slag is obtained by drying, crushing and screening the negative electrode carbon slag of lithium-ion batteries.
[0012] S2. Dissolve the fine carbon slag, aluminum salt, and cerium salt in water or alcohol solution at a ratio of 2g:(0.001-0.009)mol:(0.001-0.009)mol. Stir and heat the resulting mixed solution to completely evaporate the solvent.
[0013] S3. Grind the mixture obtained in S2 until homogeneous, and then calcine it to obtain the final product.
[0014] Patent application CN106824058A discloses a cerium / aluminum modified montmorillonite defluorination adsorbent and its preparation method. The adsorbent is prepared through processes including montmorillonite sodium conversion, columnar liquid preparation, columnar modification, calcination, pulverization, and sieving. It exhibits an adsorption capacity of 1.55 mg / g for 50 ml of a solution containing 4 mg / L of fluoride ions. While this method uses cerium / aluminum modified montmorillonite to prepare the defluorination adsorbent, its preparation is time-consuming, requires large amounts of aluminum and cerium salts, necessitates the addition of alkali to adjust the pH of the cerium-aluminum mixture, involves high calcination temperatures, results in high adsorbent costs, and requires further improvement in adsorption capacity.
[0015] This application uses cerium / aluminum modified lithium-ion battery negative electrode carbon slag, which has a short preparation time, requires less aluminum and cerium salts, has a low calcination temperature, low adsorbent cost, and further improves adsorption capacity.
[0016] Preferably, the molar ratio of aluminum salt to cerium salt is 1-3:1. This molar ratio can further improve the fluorine adsorption capacity of the prepared adsorbent.
[0017] In one preferred embodiment, the fine carbon slag in S1 is ball-milled. The ball-milled carbon slag has a relatively smaller particle size and a relatively larger specific surface area, which is beneficial to improving the fluorine adsorption capacity of the prepared adsorbent.
[0018] In one preferred embodiment, the fine carbon slag in S1 undergoes acid leaching and water leaching treatment, including:
[0019] Acid leaching: Fine carbon residue is mixed evenly with concentrated sulfuric acid, and the resulting slurry is calcined at 150-280℃ for 1-4 hours;
[0020] Water immersion: After complete cooling, the sintered carbon slag obtained from roasting is immersed in water, separated from solids and liquids, washed, and dried to obtain impurity-free carbon slag.
[0021] Preferably, the slurry obtained from the acid leaching step is calcined at a temperature of 210-280°C, and more preferably, the calcination temperature is 250-280°C. This temperature range can further increase the carbon content of the impurity-removing carbon residue, which is beneficial for the subsequent treatment of fluoride-containing wastewater by the prepared adsorbent.
[0022] In one preferred embodiment, the ratio of fine carbon residue to concentrated sulfuric acid in the acid leaching step is 1 g:(0.1-1.5) ml.
[0023] In one preferred embodiment, the water immersion step involves immersing, separating the solid from the liquid, washing, and drying the sintered carbon slag obtained from roasting, including:
[0024] The sintered carbon slag obtained by roasting is soaked in water at 40-80℃ for 1-3 hours to separate the solid and liquid. It is then washed with deionized water until neutral. The washed filter residue is placed in an oven at 60-80℃ to dry, thus obtaining impurity-free carbon slag.
[0025] Preferably, the water immersion temperature is 60-80℃. This temperature range can further increase the carbon content of the impurity-removing carbon residue, which is beneficial for the subsequent treatment of fluoride-containing wastewater by the prepared adsorbent.
[0026] In one preferred embodiment, the calcination temperature in S3 is 150-250°C, and the calcination time is 1-4 hours.
[0027] When the temperature is raised to around 200℃, aluminum and cerium salts decompose into amorphous structures, which is conducive to fluoride ion adsorption. As the temperature continues to rise, aluminum and cerium salts completely decompose, their structures are destroyed, and their adsorption capacity decreases. The calcination temperature in S3 is below 150℃, and the resulting adsorbent is not conducive to fluoride ion adsorption.
[0028] In one preferred embodiment, the step of stirring and heating the obtained mixed solution in S2 to completely evaporate the solvent includes: stirring under magnetic stirring conditions at 20-80°C for 5-10 hours, and then placing the mixture in an oven at 60-80°C to completely evaporate the solvent.
[0029] The present invention also discloses a modified lithium-ion battery negative electrode carbon adsorbent prepared by the method described above.
[0030] The present invention also discloses a modified lithium-ion battery negative electrode carbon adsorbent, which uses the impurity-removed lithium-ion battery negative electrode carbon slag as a carrier, loads aluminum oxide and cerium oxide, and heat-treats in air atmosphere to obtain the modified lithium-ion battery negative electrode carbon adsorbent.
[0031] The graphite content in the purified lithium-ion battery negative electrode carbon residue is ≥99 wt.%.
[0032] This invention also discloses the application of the modified lithium-ion battery negative electrode carbon adsorbent in the removal of fluoride ions from wastewater.
[0033] The pH value of the wastewater is 4 ≤ pH ≤ 8, and the adsorption time is 1-24h.
[0034] Preferably, in the acid leaching step, the concentration of concentrated sulfuric acid is 10-18.4 mol / L.
[0035] Preferably, in the water immersion step, the sintered carbon slag is mixed with water at a liquid-solid ratio of 1g:10-15ml.
[0036] Preferably, in the water immersion step, solid-liquid separation can be performed by vacuum filtration, and the purified carbon residue can be obtained after drying and grinding.
[0037] Preferably, in S2, the aluminum salt is any one of aluminum chloride hexahydrate, aluminum sulfate octadechydrate, aluminum nitrate nonahydrate, and sodium aluminate, and the cerium salt is any one of cerium chloride heptahydrate, cerium sulfate tetrahydrate, and cerium nitrate hexahydrate.
[0038] In S2, the alcohol solution is any one of methanol, isopropanol, ethanol, and n-propanol.
[0039] In S3, the dried mixture is ground evenly, heated to 150-250℃ at a rate of 1-10℃ / min and calcined for 1-4 hours, and then cooled to room temperature at a rate of 1-10℃ / min to obtain the calcined material.
[0040] The modified lithium-ion battery anode carbon adsorbent prepared in S3 has a particle size of no more than 150 μm. Excessively large particle size hinders dispersion in aqueous solution and affects adsorption efficiency.
[0041] Further, in S1, the lithium-ion battery negative electrode carbon slag to be processed includes one or more of the following: lithium iron phosphate battery carbon slag, lithium cobalt oxide battery carbon slag, lithium manganese oxide battery carbon slag, lithium nickel oxide battery carbon slag, ternary lithium battery carbon slag, and lithium iron phosphate battery carbon slag.
[0042] Further, in S1, the lithium-ion battery negative electrode waste carbon residue to be treated has a fixed carbon content of 70-85 wt.%, a volatile matter content of 5-10 wt.%, and an ash content of 5-15 wt.%; the ash contains one or more of Si, Ni, Mn, Co, Al, Na, Fe, and P.
[0043] This invention involves uniformly mixing concentrated sulfuric acid with lithium-ion battery negative electrode carbon slag and calcining it at a low temperature. This allows metallic impurities such as Co, Ni, Fe, Mn, Fe, Al, and Na to react with sulfuric acid to form soluble sulfates, which are then dissolved during subsequent water bath leaching and removed by washing and filtration, resulting in carbon slag material with high purity.
[0044] The adsorbent prepared according to the present invention has a large specific surface area provided by waste carbon slag. Alumina and cerium oxide are loaded on the surface of the carbon slag, which solves the problems of agglomeration of alumina and cerium oxide and the problem of easy secondary pollution in water. At the same time, the surface is rich in a large number of hydroxyl active groups, and the active sites of aluminum ions and cerium ions are fully exposed, which greatly improves the adsorption effect and enables the rapid adsorption and removal of fluoride ions.
[0045] This invention provides the application of the adsorbent prepared as described above in the removal of fluoride ions from water. This adsorbent exists in water as carbon particles and is insoluble in water. Rapid solid-liquid separation can be achieved through sedimentation or filtration, without causing secondary pollution to the water body. When used to adsorb fluoride ions in water, it can rapidly adsorb and remove fluoride ions with an initial concentration of approximately 50 mg / L, reducing it to below 5 mg / L, meeting the discharge standards for industrial fluoride-containing wastewater. The separated adsorbent can be recycled through alkali soaking and drying. This modified carbon slag adsorbent solves the problem of solid waste resource treatment for lithium-ion battery negative electrode carbon slag and is also beneficial to the sustainable development of graphite resources.
[0046] Compared with the prior art, the beneficial effects of the present invention are:
[0047] (1) The present invention has low energy consumption, simple preparation process, low production cost, and can also take into account the defluorination adsorption effect.
[0048] (2) This invention modifies the negative electrode carbon slag of lithium-ion batteries into a defluorination adsorbent, providing a promising path for the recycling and resource utilization of graphite and increasing the added value of waste carbon slag treatment.
[0049] (3) The surface of the adsorbent prepared by the present invention is rich in hydroxyl active groups and metal ion active sites. The loading of aluminum and cerium oxides on carbon solves the problem of secondary water pollution caused by the easy aggregation and difficulty in separation of aluminum and cerium oxides.
[0050] (4) The adsorbent prepared by the present invention can achieve solid-liquid separation quickly through sedimentation or filtration, and can be recycled after being soaked in alkali and dried, and has a wide range of application prospects. Attached Figure Description
[0051] Figure 1 This is an SEM image of the carbon slag after impurity removal in Example 1;
[0052] Among them, (a) 400 times, (b) 1000 times, and (c) 3000 times.
[0053] Figure 2 This is a SEM image of the modified lithium-ion battery negative electrode carbon residue defluorinating agent prepared in Example 1.
[0054] Among them, (a) 600 times, (b) 1500 times, and (c) 4000 times.
[0055] Figure 3 This is the EDS diagram of the modified lithium-ion battery negative electrode carbon slag adsorbent prepared in Example 1. Detailed Implementation
[0056] The present invention will be further described below with reference to specific embodiments. The described embodiments are only some embodiments of the present invention, and not all embodiments.
[0057] Example 1
[0058] A method for preparing a modified defluorinating agent for lithium-ion battery negative electrode carbon slag includes the following steps:
[0059] S1. Take 40g of waste lithium-ion battery carbon residue from a domestic factory, with a fixed carbon content of 83.62wt.%, volatile matter of 7.72wt.%, and ash content of 8.66%. After drying the carbon residue, crush it to 150um (100 mesh) using a crusher to obtain fine carbon residue.
[0060] S2. Pour the fine carbon slag and concentrated sulfuric acid of 18.4 mol / L with a carbon slag liquid-solid ratio of 0.8 ml:g into a graphite crucible, stir and mix evenly, and then put the mixture into a pit furnace and keep it at 250℃ for 3 hours.
[0061] S3. After complete cooling, the sintered carbon slag is subjected to water immersion treatment at a temperature of 60℃ for 3 hours, with a liquid-to-solid ratio of 15ml:1g. After immersion, the carbon slag is washed with deionized water until neutral, filtered, dried at 60℃, and ground uniformly for subsequent processing. The purified carbon slag is tested according to the graphite chemical analysis method (GB / T-2008), yielding a carbon material with a carbon content of 99.56%. The SEM image of the purified carbon slag is shown below. Figure 1 As shown.
[0062] S4. Take 2g of purified carbon residue and mix it with 3.38g of aluminum nitrate nonahydrate and 1.30g of cerium nitrate hexahydrate in 30ml of anhydrous ethanol. Keep the mixture at 65℃ and 500rpm under magnetic stirring for 8h. Then put the mixture into an oven at 60℃ until the ethanol is completely evaporated.
[0063] S5. Grind the evaporated mixture evenly, heat it to 200℃ at a heating rate of 5℃ / min and calcine for 3 hours. After cooling to room temperature, obtain the calcined material.
[0064] S6. Grind the obtained calcined material evenly to a particle size of no more than 150 μm (100 mesh) to obtain the modified lithium-ion battery negative electrode carbon slag adsorbent.
[0065] The morphology of the modified lithium-ion battery anode carbon slag adsorbent synthesized in Example 1 was characterized by scanning electron microscopy as follows: Figure 2 As shown, the element distribution is as follows Figure 3As shown, 100 ml of a solution with a fluoride ion concentration of 50 mg / L was prepared using NaF. The adsorbent synthesized in Example 1 was added to the solution at a concentration of 1 g / L. A static adsorption experiment was conducted at 25 °C. After adsorption was completed, the fluoride ion concentration in the filtrate was measured by filtration. The results showed that the modified lithium-ion battery negative electrode carbon residue adsorbent exists in the aqueous solution in particulate form and can reduce the initial fluoride concentration of 50 mg / L to 2.52 mg / L, meeting the industrial fluoride-containing wastewater discharge standard. Rapid solid-liquid separation can be achieved through sedimentation or filtration.
[0066] Example 2
[0067] A method for preparing a modified defluorinating agent for lithium-ion battery negative electrode carbon slag includes the following steps:
[0068] S1. Take 40g of waste lithium-ion battery carbon residue from a domestic factory, with a fixed carbon content of 83.62wt.%, volatile matter of 7.72wt.%, and ash content of 8.66%. After drying the carbon residue, crush it to 150um (100 mesh) using a crusher to obtain fine carbon residue.
[0069] S2. Pour fine carbon slag and concentrated sulfuric acid of 18.4 mol / L with a carbon slag liquid-solid ratio of 1 ml:g into a graphite crucible, stir and mix evenly, and then put the mixture into a pit furnace and keep it at 200℃ for 3 hours.
[0070] S3. After complete cooling, the sintered carbon slag is subjected to water immersion treatment at a temperature of 60℃ for 3 hours, with a liquid-to-solid ratio of 15ml:1g. After immersion, the carbon slag is washed with deionized water until neutral, filtered, dried at 60℃, and ground uniformly for subsequent processing. The purified carbon slag is tested according to the graphite chemical analysis method (GB / T-2008), yielding a carbon material with a carbon content of 99.28%.
[0071] S4. Take 2g of purified carbon residue and mix it with 3.38g of aluminum nitrate nonahydrate and 1.95g of cerium nitrate hexahydrate in 30ml of anhydrous ethanol. Keep the mixture at 65℃ and 500rpm under magnetic stirring for 8h. Then put the mixture into an oven at 80℃ until the ethanol is completely evaporated.
[0072] S5. Grind the evaporated mixture evenly, heat it to 200℃ at a heating rate of 5℃ / min and calcine for 3 hours. After cooling to room temperature, obtain the calcined material.
[0073] S6. Grind the obtained calcined material evenly to a particle size of no more than 150 μm (100 mesh) to obtain the modified lithium-ion battery negative electrode carbon slag adsorbent.
[0074] A 100 ml solution with a fluoride ion concentration of 50 mg / L was prepared using NaF. The adsorbent synthesized in Example 2 was added to the solution at a concentration of 1 g / L. A static adsorption experiment was conducted at 25 °C. After adsorption was completed, the fluoride ion concentration in the filtrate was measured by filtration. The results showed that the modified lithium-ion battery negative electrode carbon residue adsorbent exists in the aqueous solution in particulate form and can reduce the initial fluoride concentration of 50 mg / L to 4.36 mg / L, meeting the industrial fluoride-containing wastewater discharge standard. Rapid solid-liquid separation can be achieved through sedimentation or filtration.
[0075] Example 3
[0076] A method for preparing a modified defluorinating agent for lithium-ion battery negative electrode carbon slag includes the following steps:
[0077] S1. Take 40g of waste lithium-ion battery carbon residue from a domestic factory, with a fixed carbon content of 83.62wt.%, volatile matter of 7.72wt.%, and ash content of 8.66%. After drying the carbon residue, crush it to 150um (100 mesh) using a crusher to obtain fine carbon residue.
[0078] S2. Pour the fine carbon slag and concentrated sulfuric acid of 18.4 mol / L with a carbon slag liquid-solid ratio of 0.8 ml:g into a graphite crucible, stir and mix evenly, and then put the mixture into a pit furnace and keep it at 280℃ for 3 hours.
[0079] S3. After complete cooling, the sintered carbon slag is subjected to water immersion treatment at a temperature of 50℃ for 3 hours, with a liquid-to-solid ratio of 15ml:1g. After immersion, the carbon slag is washed with deionized water until neutral, filtered, dried at 60℃, and ground uniformly for subsequent processing. The purified carbon slag is tested according to the graphite chemical analysis method (GB / T-2008), yielding a carbon material with a carbon content of 99.83%.
[0080] S4. Take 2g of purified carbon residue and mix it with 3.75g of aluminum nitrate nonahydrate and 1.74g of cerium nitrate hexahydrate in 30ml of anhydrous ethanol. Keep the mixture at 65℃ and 500rpm under magnetic stirring for 8h. Then put the mixture into an oven at 80℃ until the ethanol is completely evaporated.
[0081] S5. Grind the evaporated mixture evenly, heat it to 220℃ at a heating rate of 5℃ / min and calcine for 3 hours. After cooling to room temperature, obtain the calcined material.
[0082] S6. Grind the obtained calcined material evenly to a particle size of no more than 150 μm (100 mesh) to obtain the modified lithium-ion battery negative electrode carbon slag adsorbent.
[0083] A 100 ml solution with a fluoride ion concentration of 50 mg / L was prepared using NaF. The adsorbent synthesized in Example 3 was added to the solution at a concentration of 1 g / L. A static adsorption experiment was conducted at 25 °C. After adsorption was completed, the fluoride ion concentration in the filtrate was measured by filtration. The results showed that the modified lithium-ion battery negative electrode carbon residue adsorbent exists in the aqueous solution in particulate form and can reduce the initial fluoride concentration of 50 mg / L to 2.88 mg / L, meeting the industrial fluoride-containing wastewater discharge standard. Rapid solid-liquid separation can be achieved through sedimentation or filtration.
[0084] Example 4
[0085] S4. Take 2g of the impurity-removed carbon residue from Example 1, mix it with 0.74g of sodium aluminate and 1.30g of cerium nitrate hexahydrate in 30ml of anhydrous ethanol, keep the mixture at 65℃ and 500rpm under magnetic stirring for 6h, and then put the mixture into an oven at 80℃ until the ethanol is completely evaporated.
[0086] S5. Grind the evaporated mixture evenly, heat it to 220℃ at a heating rate of 5℃ / min and calcine for 5 hours. After cooling to room temperature, obtain the calcined material.
[0087] S6. Grind the obtained calcined material evenly to a particle size of no more than 150um (100 mesh) to obtain the modified lithium-ion battery negative electrode carbon slag defluorinating agent.
[0088] Prepare a 100ml solution with a fluoride ion concentration of 50mg / L using NaF. Add the adsorbent synthesized in Example 4 to the solution at a concentration of 1g / L. Perform a static adsorption experiment at 25℃. After adsorption is complete, filter and measure the fluoride ion concentration in the filtrate. The results show that the fluoride concentration can only be reduced from the initial concentration of 50mg / L to 27.30mg / L.
[0089] Example 5
[0090] S4. Take 2g of the purified carbon residue from Example 1, 6.0g of aluminum sulfate octadecylhydrate, and 1.30g of cerium nitrate hexahydrate and dissolve them in 30ml of anhydrous ethanol. Keep the mixture at 65℃ and 500rpm under magnetic stirring for 8h. Then put the mixture into an oven at 80℃ until the solvent is completely evaporated.
[0091] S5. Grind the evaporated mixture evenly, heat it to 200℃ at a heating rate of 5℃ / min and calcine for 5 hours. After cooling to room temperature, obtain the calcined material.
[0092] S6. Grind the obtained calcined material evenly to a particle size of no more than 150um (100 mesh) to obtain the modified lithium-ion battery negative electrode carbon slag defluorinating agent.
[0093] Prepare a 100ml solution with a fluoride ion concentration of 50mg / L using NaF. Add the adsorbent synthesized in Example 5 to the solution at a concentration of 1g / L. Perform a static adsorption experiment at 25℃. After adsorption is complete, filter and measure the fluoride ion concentration in the filtrate. The results show that the fluoride concentration can only be reduced from the initial concentration of 50mg / L to 23.48mg / L.
[0094] Example 6
[0095] S4. Take 2g of the purified carbon residue from Example 1, 2.17g of aluminum chloride hexahydrate, and 1.30g of cerium nitrate hexahydrate and dissolve them in 30ml of anhydrous ethanol. Keep the mixture at 65℃ and 500rpm under magnetic stirring for 6h. Then put the mixture into an oven at 80℃ until the solvent is completely evaporated.
[0096] S5. Grind the evaporated mixture evenly, heat it to 200℃ at a heating rate of 5℃ / min and calcine for 5 hours. After cooling to room temperature, obtain the calcined material.
[0097] S6. Grind the obtained calcined material evenly to a particle size of no more than 150um (100 mesh) to obtain the modified lithium-ion battery negative electrode carbon slag defluorinating agent.
[0098] Prepare a 100ml solution with a fluoride ion concentration of 50mg / L using NaF. Add the adsorbent synthesized in Example 6 to the solution at a concentration of 1g / L. Perform a static adsorption experiment at 25℃. After adsorption is complete, filter and measure the fluoride ion concentration in the filtrate. The results show that the fluoride concentration can only be reduced from the initial concentration of 50mg / L to 30.19mg / L.
[0099] Example 7
[0100] S1. Take waste lithium-ion battery carbon residue from a domestic factory, with a fixed carbon content of 83.62 wt.%, volatile matter of 7.72 wt.%, and ash content of 8.66%. After drying the carbon residue, crush it to 150 μm (100 mesh) using a crusher to obtain fine carbon residue.
[0101] S2. Take 15g of fine carbon slag and put it into a ball mill jar. Add zirconia balls at a ball-to-material ratio of 20:1. Then place it in a planetary high-energy ball mill. The ball milling speed is 350rpm and the ball milling time is 2h to obtain activated carbon slag.
[0102] S3. Take 2g of ball-milled carbon residue and mix it with 3.38g of aluminum nitrate nonahydrate and 1.30g of cerium nitrate hexahydrate in 30ml of anhydrous ethanol. Keep the mixture at 65℃ and 500rpm under magnetic stirring for 8h. Then put the mixture into an oven at 60℃ until the ethanol is completely evaporated.
[0103] S4. Grind the evaporated mixture evenly, heat it to 200℃ at a heating rate of 5℃ / min and calcine for 3 hours. After cooling to room temperature, obtain the calcined material.
[0104] S5. Grind the obtained calcined material evenly to a particle size of no more than 150 μm (100 mesh) to obtain the modified lithium-ion battery negative electrode carbon slag adsorbent.
[0105] A 100 ml solution with a fluoride ion concentration of 50 mg / L was prepared using NaF. The adsorbent synthesized in Example 7 was added to the solution at a concentration of 0.5 g / L. A static adsorption experiment was conducted at 25 °C. After adsorption was complete, the fluoride ion concentration in the filtrate was measured by filtration. The results showed that the modified lithium-ion battery negative electrode carbon residue adsorbent existed in the aqueous solution in particulate form, reducing the initial fluoride concentration from 50 mg / L to 20.21 mg / L, with an adsorption capacity of 59.58 mg / g. Rapid solid-liquid separation can be achieved through sedimentation or filtration.
[0106] Comparative Example 1
[0107] 40g of waste lithium-ion battery carbon residue from a domestic factory was taken, containing 83.62wt.% fixed carbon, 7.72wt.% volatile matter, and 8.66% ash. The residue was dried and then crushed to 150µm (100 mesh) to obtain fine carbon residue. A 100ml solution of NaF with a fluoride ion concentration of 50mg / L was prepared. The fine carbon residue was added to the solution at a concentration of 1g / L, and a static adsorption experiment was conducted at 25℃. After adsorption, the filtrate was filtered, and the fluoride ion concentration was measured. The results showed that the residual fluoride ion concentration was 45.61mg / L.
[0108] Comparative Example 2
[0109] Take the impurity-removed carbon residue obtained in Example 1, prepare 100 ml of a fluoride ion concentration of 50 mg / L with NaF, add the impurity-removed carbon residue to the solution at a rate of 1 g / L, and conduct a static adsorption experiment at 25 °C. After the adsorption is completed, filter and measure the fluoride ion concentration in the filtrate. The results show that the residual fluoride ion concentration is 42.07 mg / L.
[0110] Comparative Example 3
[0111] Repeat Example 1, except that in S2, the insulation temperatures of the pit furnace are 150℃, 180℃, 210℃, and 280℃.
[0112] The carbon content of the purified carbon slag was tested according to the graphite chemical analysis method (GB / T-2008) and the results are shown in the table below:
[0113] Temperature ℃ 150 180 210 250 280 Carbon content % 85.38 89.20 93.66 99.56 99.83
[0114] The low insulation temperature means that the concentrated sulfuric acid does not react completely with the impurities in the carbon slag, leaving impurities in the carbon slag, which is not conducive to the subsequent treatment of fluoride-containing wastewater.
[0115] Comparative Example 4
[0116] Repeat Example 1, except that in S3, the water immersion temperature is 40°C and 80°C, and the water immersion time is 1 hour and 3 hours.
[0117] The carbon content of the purified carbon slag was tested according to the graphite chemical analysis method (GB / T-2008) and the results are shown in the table below:
[0118]
[0119] Comparative Example 5
[0120] Repeat Example 1, except that in S4, cerium nitrate hexahydrate is not added.
[0121] The results showed that the synthesized modified lithium-ion battery negative electrode carbon residue defluorinating agent existed in water in particulate form, reducing the initial concentration of fluoride solution from 50 mg / L to 17.43 mg / L.
[0122] Comparative Example 6
[0123] Example 1 was repeated, except that in S4, the amount of cerium nitrate hexahydrate added was 0.009 mol, 0.0045 mmol, and 0.002 mol, respectively.
[0124] Prepare 100 ml of NaF solution with a fluoride ion concentration of 50 mg / L. Add 1 g / L of defluorinating agent to the solution and conduct a static adsorption experiment at 25 °C. After adsorption is complete, filter and measure the fluoride ion concentration in the filtrate. The results are shown in the table below:
[0125]
[0126] Compared to the adsorption capacity (1.55 mg / g) of the cerium / aluminum modified montmorillonite fluoride removal adsorbent disclosed in CN106824058A, the adsorption capacity in this embodiment is 47.27 mg / g under the condition of Al / Ce molar ratio of 3:1. This embodiment shows a significantly improved adsorption capacity, reduced aluminum and cerium salt usage, and eliminates the need for pH adjustment with alkali, thus saving on adsorbent costs.
[0127] Comparative Example 7
[0128] Repeat Example 1, except that in S5, the temperature is increased to 150°C, 250°C, 300°C and 350°C respectively at a heating rate of 5°C / min.
[0129] Prepare 100 ml of NaF solution with a fluoride ion concentration of 50 mg / L. Add the obtained defluorinating agent at a concentration of 1 g / L to the solution. Conduct a static adsorption experiment at 25 °C. After adsorption is complete, filter and measure the fluoride ion concentration in the filtrate. The results are shown in the table below:
[0130]
[0131] When the temperature is raised to around 200℃, aluminum and cerium salts decompose into amorphous structures, which is conducive to the adsorption of fluoride ions. As the temperature continues to rise, aluminum and cerium salts decompose completely, their structures are destroyed, and their adsorption capacity decreases.
[0132] Comparative Example 8
[0133] Repeat Example 1, except that in S4, replace 30 ml of anhydrous ethanol solution with 30 ml of deionized water.
[0134] 100 ml of a fluoride ion concentration of 50 mg / L was prepared using NaF. The adsorbent prepared in Comparative Example 8 was added to the solution at a concentration of 1 g / L. A static adsorption experiment was conducted at 25 °C. After adsorption was completed, the fluoride ion concentration in the filtrate was measured by filtration. The results showed that the initial fluoride concentration of 50 mg / L could be reduced to 9.62 mg / L, which met the industrial fluoride wastewater discharge standard.
[0135] This invention utilizes purified lithium-ion battery negative electrode carbon slag as a carrier, loading aluminum oxide and cerium oxide, and then heat-treating it in air to obtain a highly efficient defluorination adsorbent. The material prepared by this method not only achieves the disposal of solid waste such as waste carbon slag but also transforms it into a valuable resource. The resulting adsorbent exhibits excellent adsorption performance for fluoride-containing wastewater. More importantly, the preparation process of the adsorbent material is simple, relatively low-cost, easy to operate, and convenient for recycling and reuse, making it an adsorbent material with great potential for practical applications.
Claims
1. A method for preparing a modified negative electrode carbon adsorbent for lithium ion batteries, It is characterized in that The following steps are involved: S1. Drying, crushing and screening the negative electrode carbon residue of lithium-ion batteries to obtain fine carbon residue; S2, dissolving the fine carbon residue, aluminum salt and cerium salt in water or alcohol solution at a ratio of 2 g: (0.001-0.009) mol: (0.001-0.009) mol, stirring and heating the obtained mixed solution to completely evaporate the solvent; S3, grinding the mixture obtained in S2 uniformly and roasting to obtain.
2. The preparation method according to claim 1, It is characterized in that The fine carbon slag in S1 is ball-milled, and the particle size of the fine carbon slag after ball-milling is not greater than 150um.
3. The preparation method according to claim 1, It is characterized in that The fine carbon slag in S1 is treated by acid leaching and water leaching, including: Acid leaching: Mix the fine carbon slag and concentrated sulfuric acid evenly, and roast the obtained slurry at a temperature of 150-280℃ for 1-4h; Water soaking: After being completely cooled, the sintered carbon slag obtained by roasting is soaked in water, solid-liquid separated, washed and dried to obtain impurity-removed carbon slag. Preferably, the slurry obtained in the acid leaching step is calcined at a temperature of 210-280°C, and more preferably, the calcination temperature is 250-280°C.
4. The preparation method according to claim 3, It is characterized in that The ratio of fine carbon slag to concentrated sulfuric acid in the acid leaching step is 1g:(0.1-1.5)ml.
5. The preparation method according to claim 3, It is characterized in that The water immersion step involves water immersion, solid-liquid separation, washing, and drying of the sintered carbon slag obtained by roasting, including: The sintered carbon slag obtained by roasting is soaked in water at 40-80°C for 1-3h, solid-liquid separation is performed, and the residue is washed with deionized water until neutral. The washed residue is placed in an oven at 60-80°C for drying to obtain impurity-removed carbon slag.
6. The preparation method according to claim 1, It is characterized in that The calcination temperature in S3 is 150-250°C, and the calcination time is 1-4h.
7. The preparation method according to claim 1, It is characterized in that The step of stirring and heating the obtained mixed solution in S2 to completely evaporate the solvent comprises: stirring for 5-10 hours under magnetic stirring conditions at 20-80° C., and then placing the mixture in an oven at 60-80° C. to completely evaporate the solvent.
8. A modified lithium ion battery negative electrode carbon adsorbent prepared by the method according to any one of claims 1 to 7.
9. A modified lithium-ion battery negative electrode carbon adsorbent, Features: Using the impurity-removed negative electrode carbon residue of lithium ion battery as a carrier, loading aluminum oxide and cerium oxide, and heat-treating in an air atmosphere to obtain a modified negative electrode carbon adsorbent for lithium ion battery; The graphite content in the negative electrode carbon slag of the lithium ion battery after impurities removal is ≥99wt.%.
10. Use of the modified lithium ion battery negative electrode carbon adsorbent according to claim 8 or 9 in removing fluoride ions from wastewater.
Citation Information
Patent Citations
Preparation method of high-efficiency manganese and cerium composite adsorbent for removing fluorine in drinking water
CN101791533A
Preparation method of nano titanium dioxide adsorbent and application thereof
CN103071448A
Cerium / aluminum modified montmorillonite fluoride removal adsorbing agent and preparation method thereof
CN106824058A
Preparation method of fluorine ion adsorbent
CN115722195A
Method for preparing porous graphite by using waste lithium ion battery carbon residue
CN116639686A