Monolithic electric conduction and heat conduction manganese oxide catalyst as well as preparation method and application thereof

Through pulse electrodeposition and acid etching treatment, the problems of low loading and easy falling off of manganese oxide catalyst on the conductive support were solved, and a conductive thermal manganese oxide catalyst with high loading and stability were prepared, achieving efficient catalysis at low temperatures Effects of volatile organics and ozone.

CN118892823AActive Publication Date: 2024-11-05WUHAN INST OF PHOTOCHEMICAL TECH
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202410929285.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-05
Estimated Expiration
2044-07-11

AI Technical Summary

Technical Problem

In the prior art, the method of loading manganese oxide catalysts on metals and other conductive supports has problems such as low loading, easy shedding and harsh synthetic conditions.

Method used

The mixed solution of potassium permanganate and manganese sulfate is immersed in the conductive thermal carrier by pulse electrodeposition method, and the migration rate and reduction rate of manganese ions are adjusted by pulse voltage and frequency to achieve in situ growth of manganese oxide on the carrier and through acid The etching treatment improves the roughness of the support surface and the bonding tightness of the deposited layer, and prepares a large-scale conductive thermal manganese oxide catalyst with high loading and stability.

Benefits of technology

It significantly improves the loading and stability of the catalyst, enhances catalytic activity and durability, and can efficiently catalyze volatile organic compounds and ozone at low temperatures, and has mild process conditions and wider applicability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118892823A_ABST
    Figure CN118892823A_ABST
Patent Text Reader

Abstract

The invention provides an integral electric-conduction and heat-conduction manganese oxide catalyst as well as a preparation method and application thereof, and belongs to the technical field of nano materials. A pulse method and an electrodeposition method are combined, the ratio of potassium permanganate to manganese sulfate to water is adjusted, the manganese oxide catalyst is uniformly grown on an electric and heat-conducting carrier by controlling pulse voltage, frequency, duty ratio, conduction time and the like, and then the integral electric and heat-conducting manganese oxide catalyst is obtained through drying and roasting. The obtained monolithic catalyst has the advantages of excellent conductivity, high temperature rise speed, close contact between surface manganese oxide and a carrier, excellent stability and the like; the catalyst has a wide application prospect in the fields of petrochemical engineering, fine chemical engineering, tail gas catalytic oxidation-reduction reaction and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nano material preparation, and in particular relates to an integral conductive and thermal conductive manganese oxide catalyst and a preparation method and application thereof. Background Art

[0002] Manganese oxide catalysts have abundant lattice oxygen and surface oxygen, and show excellent low-temperature catalytic performance. Manganese oxide catalysts have good catalytic purification capabilities for most volatile organic compounds and ozone, and are widely used in the treatment of industrial air pollutants. However, since powdered or granular manganese oxide catalysts are subject to many restrictions in practical applications, their catalytic effects cannot be effectively exerted. In addition, in order to further promote the activation of lattice oxygen on the surface of manganese oxide and the ability of surface electron transfer, the catalyst surface can be electrified. Therefore, it is necessary to load manganese oxide onto a conductive carrier to prepare an integral conductive and thermally conductive manganese oxide catalyst, so that air pollutants and catalysts can be evenly contacted at a higher air velocity, with high catalyst utilization and high stability.

[0003] The method of synthesizing monolithic catalysts used in industry is mainly direct loading method. For example, patent CN105126822A uses impregnation method to prepare monolithic manganese oxide catalyst supported by honeycomb ceramics, and soaks cordierite honeycomb carrier in manganese oxide catalyst and pseudo-boehmite slurry, takes out and blows excess slurry with high-pressure air gun, and obtains monolithic manganese oxide catalyst after drying. This preparation method has simple process, easy control of reaction parameters, wide source of raw materials, low cost, and is easy to popularize, but the catalyst loaded by impregnation method has poor adhesion and is easy to fall off under high air velocity conditions. Patent CN117960181A uses metal aluminum fiber as substrate, and grows a layer of pseudo-boehmite in situ on the surface of metal aluminum fiber by hydrothermal method, and then loads active components and auxiliary components, avoiding the shortcomings of cumbersome steps, low loading amount of active components and uneven distribution of traditional coating method, and has the advantages of simple operation and components not easy to fall off, but the hydrothermal conditions of this method are relatively harsh and are not suitable for some metal carriers.

[0004] In summary, it can be seen that there is an urgent need to solve the problems of low loading capacity, easy shedding, and harsh synthesis conditions in the method of loading manganese oxide catalysts on metals and other conductive carriers. Summary of the invention

[0005] In order to solve the above technical problems, the present invention proposes an integral conductive and thermally conductive manganese oxide catalyst and a preparation method and application thereof.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] One of the technical solutions of the present invention:

[0008] A method for preparing an integral conductive and thermally conductive manganese oxide catalyst comprises the following steps:

[0009] The conductive and heat-conductive carrier is immersed in a mixed solution containing potassium permanganate and manganese sulfate, and then pulse electrodeposition is used to make manganese oxide grow in situ on the conductive and heat-conductive carrier, followed by drying and calcination to prepare a monolithic manganese oxide catalyst.

[0010] Beneficial effects: By applying pulse voltage, the migration rate and reduction rate of manganese ions on the surface of the conductive carrier can be significantly increased, so that more ions are reduced and deposited on the conductive carrier in a short time, thereby accelerating the growth rate of the material. At the same time, the pulse electrodeposition method restores the ion concentration near the carrier surface through the intermittent application of pulse current, thereby effectively reducing the concentration difference polarization phenomenon and ensuring the stability and uniformity of material growth. In addition, by changing the pulse frequency and duty cycle, the nucleation and growth of the crystal can be adjusted, the size of the grain structure can be further controlled, and the organizational structure and performance of the material can be enriched.

[0011] Preferably, the parameters in the pulse electrodeposition process are:

[0012] The pulse voltage is 10-220V, the pulse frequency is 2-300Hz, the duty cycle is 20-100%, and the power-on time is 1-6h.

[0013] Preferably, the electrically conductive and heat-conductive carrier is one or more of an electric heating wire, an electrically conductive PTC heater, and an electric heating rod.

[0014] Preferably, the conductive and thermally conductive carrier needs to be subjected to acid etching for 2-4 hours before being immersed in the mixed solution;

[0015] The acid solution used in the acid etching is one or more of hydrochloric acid, sulfuric acid, oxalic acid and acetic acid;

[0016] The volume concentration of the acid solution is 1-10%.

[0017] Beneficial effects: The present invention performs acid etching on the conductive and heat-conductive carrier, firstly to remove impurities and oxide layers on the surface of the carrier, and at the same time increase the roughness of its surface, which is beneficial to the attachment and growth of manganese ions during pulse electrodeposition, thereby increasing the contact area between the deposited layer and the carrier and improving the conductive and heat-conductive properties of the catalyst; secondly, the microstructure of the carrier surface after acid etching is changed, so that the bonding between the deposited layer and the carrier is tighter, which helps to reduce the peeling and cracking phenomena produced during pulse electrodeposition and improve the stability and durability of the catalyst.

[0018] Preferably, the mass ratio of potassium permanganate to manganese sulfate in the mixed solution is 1:0.5-1.

[0019] Beneficial effects: The present invention selects manganese ions of different valence states to exhibit different electrochemical properties and reaction activities during the electrodeposition process, providing the possibility of forming manganese oxides with specific crystal structures, morphologies and properties. In addition, manganese ions of different valence states can form complex compound structures during the electrodeposition process, which promote the transmission of electrons and are conducive to the catalytic reaction.

[0020] Furthermore, the mass volume ratio of potassium permanganate to deionized water in the mixed solution is 1 g: 100-120 mL;

[0021] The mass volume ratio of the manganese sulfate to deionized water is 1 g: 150-170 mL.

[0022] Preferably, the drying conditions are: drying temperature is 105° C., and drying time is 8-16 hours.

[0023] Preferably, the calcination conditions are: calcination temperature is 250-450° C., and calcination time is 5-10 hours.

[0024] Furthermore, during the calcination process, the calcination temperature is increased from the drying temperature to 250-450° C. at a heating rate of 1-5° C. / min, and then maintained at this temperature for 5-10 hours.

[0025] The second technical solution of the present invention:

[0026] An integral conductive and thermally conductive manganese oxide catalyst prepared by the above preparation method;

[0027] The loading amount of manganese oxide in the monolithic electrically conductive and thermally conductive manganese oxide catalyst is 1-3 wt.%, and the manganese oxide is nano-scale.

[0028] The third technical solution of the present invention:

[0029] The above-mentioned integral conductive and thermally conductive manganese oxide catalyst is used in the selective catalytic oxidation of VOCs and the decomposition of ozone.

[0030] Preferably, the VOCs include one or more of toluene, formaldehyde, and ethyl acetate.

[0031] Preferably, the VOCs selective catalytic oxidation adopts a low-temperature electric Joule catalytic oxidation method.

[0032] Preferably, the ozone decomposition condition is room temperature catalysis.

[0033] Compared with the prior art, the present invention has the following advantages and technical effects:

[0034] The present invention adopts a pulsed power-on in-situ growth method, which can enhance the temperature of the conductive and thermal conductive carrier and the active state of the surface electrons by adjusting the pulse voltage and current frequency, and further selectively capture the metal manganese ions to grow on the carrier surface. This method has mild conditions, fast surface catalyst growth rate, and high loading capacity, which is beneficial to improving its catalytic activity and stability.

[0035] The integral conductive and thermally conductive manganese oxide catalyst prepared by the present invention can catalyze the oxidation of VOCs such as toluene, formaldehyde, and ethyl acetate by electric Joule at low temperature, and catalyze the decomposition of ozone with high activity and high stability at room temperature. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:

[0037] Figure 1 This is a scanning transmission electron microscope (SEM) image of the monolithic conductive and thermally conductive manganese oxide catalyst prepared in Example 1 of the present invention;

[0038] Figure 2 This is an X-ray diffraction spectrum (XRD) diagram of the monolithic electrically conductive and thermally conductive manganese oxide catalyst prepared in Example 2 of the present invention;

[0039] Figure 3 This is a comparison chart of the activities of the monolithic electrically conductive and thermally conductive manganese oxide catalysts prepared in Examples 1 and 2 of the present invention and comparative samples 1-3 in catalytic ozone decomposition and toluene oxidation. DETAILED DESCRIPTION

[0040] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0041] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0042] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0043] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.

[0044] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0045] The present invention discloses a method for preparing an integral conductive and thermally conductive manganese oxide catalyst, comprising the following steps:

[0046] a. Weigh a certain amount of potassium permanganate and manganese sulfate respectively into a beaker, add deionized water, and stir with a magnetic stirrer until fully dissolved;

[0047] b. Slowly pour the manganese sulfate solution into the potassium permanganate solution and continue stirring until the solution in the beaker gradually becomes turbid to obtain a mixed solution;

[0048] c. immersing the acid-etched conductive and thermally conductive carrier into the mixed solution obtained in step b, and supplying power to the carrier through a pulse power supply, adjusting the pulse voltage, frequency, and duty cycle to allow manganese oxide to grow in situ on the carrier;

[0049] d. The product obtained in step c is placed in a forced air drying oven for drying, and the dried product is calcined in a muffle furnace to obtain a monolithic manganese oxide catalyst.

[0050] In some preferred embodiments, in step a, the mass volume ratio of potassium permanganate to deionized water is 1:100-120 mL, the mass ratio of manganese sulfate monohydrate to deionized water is 1:150-170 mL, and the mass ratio of potassium permanganate to manganese sulfate monohydrate is 1:0.5-1; the stirring speeds of the potassium permanganate solution and the manganese sulfate solution are both 40-80 r / min, and the stirring time is 30-60 min.

[0051] In some preferred embodiments, in step b, the stirring speed of the mixed solution is 40 to 80 r / min, and the stirring time is 60 to 120 min.

[0052] In some preferred embodiments, in step c, the conductive and heat-conductive carrier is one or more of a heating wire, a conductive PTC heater, and an electric heating rod;

[0053] The acid solution selected for acid etching is one or more of hydrochloric acid, sulfuric acid, oxalic acid, and acetic acid;

[0054] The pulse voltage is 10-220V, the pulse frequency is 0-300Hz, the duty cycle is 20-100%, and the power-on time is 1-6h.

[0055] In some preferred embodiments, in step d, the drying temperature in the drying oven is 105°C, and the drying time is 8-16h; the calcination temperature ranges from 250 to 450°C, the calcination time is 5 to 10h, and the heating rate is 1 to 5°C / min.

[0056] All raw materials used in the examples of the present invention were purchased commercially; potassium permanganate, manganese sulfate monohydrate and hydrochloric acid were purchased from Sinopharm Chemical Reagent Co., Ltd. and were analytically pure; oxalic acid was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd. and was analytically pure.

[0057] Unless otherwise specified, the “parts” used in the embodiments of the present invention are “parts by weight”.

[0058] The technical solution of the present invention is further illustrated by the following embodiments.

[0059] Example 1

[0060] (1) Weigh 3.5 g potassium permanganate and 2.5 g manganese sulfate monohydrate in a beaker, add 400 mL deionized water, and stir at 60 r / min for 30 min under a magnetic stirrer until fully dissolved;

[0061] (2) Slowly pour the manganese sulfate solution into the potassium permanganate solution and continue stirring at 60 r / min for 60 min until the solution in the beaker becomes turbid;

[0062] (3) Prepare oxalic acid with a volume concentration of 5% to etch the conductive PTC heater carrier for 4 hours, then immerse the carrier in the mixed turbid solution obtained in step (2), and power the carrier through a pulse power supply, adjusting the pulse voltage to 90V and the current density to 0.02A / mm 2 , the frequency is 100 Hz, the duty cycle is 50%, and the power is applied for 4 hours to make manganese oxide grow in situ on the carrier;

[0063] (4) The obtained product was placed in a forced air drying oven at 105° C. for 12 h, and the dried product was calcined in a muffle furnace at 350° C. for 5 h at a heating rate of 5° C. / min. After cooling to room temperature, the monolithic manganese oxide catalyst was obtained.

[0064] Example 2

[0065] (1) Weigh 3.5 g potassium permanganate and 2.5 g manganese sulfate monohydrate in a beaker, add 400 mL deionized water, and stir at 60 r / min for 30 min under a magnetic stirrer until fully dissolved;

[0066] (2) Slowly pour the manganese sulfate solution into the potassium permanganate solution and continue stirring at 60 r / min for 60 min until the solution in the beaker becomes turbid;

[0067] (3) Prepare hydrochloric acid with a volume concentration of 1% to etch the electric heating wire carrier for 2 hours, then immerse the carrier in the mixed turbid solution obtained in step (2), and power the carrier through a pulse power supply, adjusting the pulse voltage to 60V and the current density to 0.01A / mm 2 , the frequency is 200 Hz, the duty cycle is 60%, and the power is applied for 1 hour to make manganese oxide grow in situ on the carrier;

[0068] (4) The obtained product was placed in a forced air drying oven at 105° C. for 12 h, and the dried product was calcined in a muffle furnace at 450° C. for 5 h at a heating rate of 5° C. / min. After cooling to room temperature, the monolithic manganese oxide catalyst was obtained.

[0069] Comparative Example Preparation of Comparative Sample

[0070] Comparative sample 1: An integral conductive and thermally conductive manganese oxide catalyst was prepared according to steps (1) to (4) in Example 1, except that the conductive PTC heater carrier in step (3) was not subjected to acid etching treatment.

[0071] Comparative sample 2: An integral conductive and thermally conductive manganese oxide catalyst was prepared according to steps (1) to (4) in Example 2, except that the power supply in step (3) was DC power supply with a voltage of 60 V for 1 hour.

[0072] Comparative sample 3: An integral conductive and thermally conductive manganese oxide catalyst was prepared according to steps (1) to (4) in Example 2, except that the power supply in step (3) was ordinary AC power supply with a voltage of 60 V and a frequency of 50 Hz for 1 hour.

[0073] Effect verification

[0074] The monolithic conductive and thermally conductive manganese oxide catalysts prepared in Examples 1-2 and Comparative Samples 1-3 were respectively subjected to catalytic effect tests for catalytic ozone decomposition and toluene oxidation. The specific catalytic test conditions were:

[0075] (I) Catalytic ozone decomposition

[0076] [O3] = 100 ppm, N2 as balance gas, total flow rate 450 mL / min, volumetric space velocity 60000 h -1 .

[0077] (II) Catalytic oxidation of toluene

[0078] [C7H8] = 400ppm, [O2] = 10%, N2 as balance gas, total flow rate 450mL / min, volume space velocity 60000h -1 .

[0079] Since the catalytic effect of the integral conductive and thermally conductive manganese oxide catalyst on formaldehyde and ethyl acetate pollutants is roughly the same as that on toluene, only the experimental effect verification of catalytic toluene oxidation is given here.

[0080] Figure 1 This is a scanning transmission electron microscope (SEM) image of the monolithic conductive and thermally conductive manganese oxide catalyst prepared in Example 1 of the present invention. Figure 1 It can be seen from the left picture that the synthesized manganese oxide catalyst has an obvious needle-like structure.

[0081] Figure 2 This is the X-ray diffraction spectrum (XRD) of the monolithic conductive and thermally conductive manganese oxide catalyst prepared in Example 2 of the present invention. Figure 2 It can be seen that the present invention successfully synthesized the manganese oxide catalyst, and the catalyst has high crystallinity.

[0082] Figure 3 The activity comparison diagram of the monolithic conductive and thermally conductive manganese oxide catalyst prepared in Examples 1 and 2 of the present invention and comparative samples 1-3 for catalytic ozone decomposition and toluene oxidation, wherein (a) is catalytic ozone decomposition and (b) is catalytic toluene oxidation. Figure 3 It can be seen that the manganese oxide catalyst grown in situ by pulse energization after acid etching exhibits more excellent catalytic performance, specifically: in (a), the catalyst prepared by Examples 1-2 of the present invention can make the catalytic effect of ozone reach nearly 100% at a temperature of about 70°C, while the ozone decomposition rate of Comparative Samples 1-3 under this temperature condition is less than 80%, and the catalytic efficiency of Comparative Sample 2 is less than 50%, and its catalytic efficiency is much lower than that of Examples 1-2 of the present invention; in (b), the catalyst prepared by Examples 1-2 of the present invention can make the catalytic effect of toluene oxidation reach nearly 100% at a temperature of about 250°C, while the catalytic effect of Comparative Samples 1-3 is only 50-60%. If the same effect as that of Examples 1-2 of the present invention is to be achieved, the temperature must be increased to 400-500°C, which further increases the difficulty and complexity of the operation, and the high temperature may also affect the structure and performance of the catalyst, further proving that the catalyst prepared by Examples 1-2 of the present invention has low temperature, low energy consumption, high efficiency and high stability.

[0083] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.

Claims

1. A method for preparing a monolithic conductive and thermally conductive manganese oxide catalyst, characterized in that: The following steps are involved: The conductive and heat-conductive carrier is immersed in a mixed solution containing potassium permanganate and manganese sulfate, and then pulse electrodeposition is used to make manganese oxide grow in situ on the conductive and heat-conductive carrier, followed by drying and calcination to prepare a monolithic manganese oxide catalyst.

2. The method for preparing a monolithic conductive and thermally conductive manganese oxide catalyst according to claim 1, characterized in that: The parameters in the pulse electrodeposition process are: The pulse voltage is 10-220V, the pulse frequency is 2-300Hz, the duty cycle is 20-100%, and the power-on time is 1-6h.

3. The method for preparing a monolithic conductive and thermally conductive manganese oxide catalyst according to claim 1, characterized in that: The conductive and heat-conductive carrier is one or more of an electric heating wire, a conductive PTC heater, and an electric heating rod.

4. The method for preparing a monolithic conductive and thermally conductive manganese oxide catalyst according to claim 1, characterized in that: The conductive and heat-conductive carrier needs to be subjected to acid etching treatment before being immersed in the mixed solution; The acid solution used in the acid etching is one or more of hydrochloric acid, sulfuric acid, oxalic acid and acetic acid.

5. The method for preparing a monolithic conductive and thermally conductive manganese oxide catalyst according to claim 1, characterized in that: The mass ratio of potassium permanganate to manganese sulfate in the mixed solution is 1:0.5-1.

6. The method for preparing a monolithic conductive and thermally conductive manganese oxide catalyst according to claim 1, characterized in that: The drying conditions are as follows: drying temperature is 105° C., and drying time is 8-16 hours.

7. The method for preparing a monolithic conductive and thermally conductive manganese oxide catalyst according to claim 1, characterized in that: The calcination conditions are as follows: the calcination temperature is 250-450° C. and the calcination time is 5-10 hours.

8. The method for preparing a monolithic conductive and thermally conductive manganese oxide catalyst according to claim 7, characterized in that: During the calcination process, the calcination temperature is increased from the drying temperature to 250-450° C. at a heating rate of 1-5° C. / min.

9. An integral electrically conductive and thermally conductive manganese oxide catalyst, characterized in that: Prepared by the preparation method according to any one of claims 1 to 8; The loading amount of manganese oxide in the monolithic electrically conductive and thermally conductive manganese oxide catalyst is 1 to 3 wt.%.

10. Use of the integral electrically conductive and thermally conductive manganese oxide catalyst as claimed in claim 9 in selective catalytic oxidation of VOCs and ozone decomposition.

Citation Information

Patent Citations

  • Preparation method of monolithic low-concentration nitrogen monoxide normal-temperature manganese oxide catalyst

    CN105126822A

  • Monolithic catalyst for hydrogen production by reforming methanol steam as well as preparation method and application of monolithic catalyst

    CN117960181A

  • Method for preparing manganese dioxide serving as cathode material of super capacitor and secondary battery

    CN102157269A

  • Preparation method of nano-manganese dioxide electrode

    CN102664107A

  • Platinum-manganese oxide supported alumina catalyst and preparation method and application thereof