Preparation of Pd-based catalyst with core-shell structure and application of Pd-based catalyst in catalytic combustion of low-concentration methane
By loading Pd onto CeO2 to form a Pd/CeO2@SiO2 core-shell structure catalyst, the problem of poor thermal stability of supported noble metal catalysts in the catalytic combustion of low-concentration methane was solved, achieving high efficiency, stability and low-temperature activity of the catalyst, making it suitable for practical applications.
Patent Information
- Application Number
- CN202410781400.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-11-05
AI Technical Summary
Existing supported noble metal catalysts exhibit poor thermal stability in the catalytic combustion of low-concentration methane, and are prone to migration and aggregation under high-temperature conditions, leading to catalyst deactivation. Furthermore, low-concentration CH4 emissions are harmful to the environment.
Using CeO2 as a carrier, Pd is loaded to form a core-shell structure of Pd/CeO2@SiO2. Ce(OH)CO3 precursor is prepared by hydrothermal synthesis, Pd particles are generated by NaBH4 reduction, and SiO2 shell is formed by tetraethyl orthosilicate and hexadecyltrimethylammonium bromide as template agents to protect the active center.
The thermal stability and low-temperature activity of the catalyst were improved. The Pd/CeO2@SiO2 catalyst maintained high catalytic activity after seven cycles of testing, with T50 decreasing to 325℃ and T90 decreasing to 385℃, effectively preventing the thermal decomposition and sintering of PdO.
Smart Images

Figure CN118892829A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of catalyst materials, and specifically relates to a catalyst for catalytic combustion of low-concentration methane, and further discloses a preparation method and application thereof. Background Art
[0002] As a typical representative of clean energy, natural gas is an important force in promoting the low-carbon transformation of my country's energy system. It can be predicted that China's dependence on and demand for natural gas will further increase in the future. However, the development of the natural gas industry also faces a series of challenges. For example, as a clean energy vehicle that replaces traditional petroleum fuel vehicles, the promotion and use of natural gas vehicles will help reduce "carbon emissions" in the transportation sector. However, the exhaust emissions of natural gas vehicles contain low-concentration CH4 that is not completely burned. These low-concentration CH4 are generally considered non-commercial. Because their extraction and processing costs are high and they are not easy to transport through existing transportation systems. Therefore, these gases are often directly discharged into the atmosphere as waste gas. The emission of untreated low-concentration CH4 will not only lead to resource waste and environmental pollution, but also have a negative impact on the climate, thus evolving into a severe environmental challenge. Because the greenhouse effect of CH4 far exceeds that of CO2, it is more than 20 times that of the same amount of CO2. Therefore, how to deal with these low-concentration CH4 has become an urgent problem to be solved.
[0003] Catalytic CH4 combustion is a heterogeneous oxidation reaction on the catalyst surface. It can not only greatly reduce the ignition temperature of CH4 combustion and improve the conversion efficiency, but also reduce the emission of toxic and harmful gases. Therefore, it has been recognized as an ideal combustion method. Most studies to date have shown that supported precious metal catalysts, especially Pd-based catalysts, have excellent activity and good low-temperature ignition performance in catalyzing low-concentration CH4 combustion. However, metal nanoparticles are thermodynamically unstable due to their high surface energy and are prone to migration-aggregation and deactivation during high-temperature catalysis. Therefore, how to improve the stability of precious metal catalysts is one of the hot topics in this field.
[0004] To address the above problems, the excellent redox properties of CeO2 were utilized to enhance the catalytic performance of Pd-based catalyst (Pd / CeO2) in the catalytic combustion reaction of low-concentration methane through doping and modification. The core-shell structure with Pd / CeO2 as the core and SiO2 as the shell effectively protected the active center and prevented the thermal decomposition and sintering of PdO under high temperature conditions. When Pd / CeO2@SiO2 was first run, T 50 is 360℃, T 90 is 405℃. After seven cycles of testing, T 50 Reduce to 325℃, T 90The temperature of Pd / CeO2@SiO2 was reduced to 385℃, which shows that Pd / CeO2@SiO2 has undergone reactivation and has significantly excellent thermal stability. This not only successfully developed a catalyst with both low-temperature activity and high-temperature stability, but also opened up new ideas for improving the thermal stability of Pd-based catalysts in low-concentration CH4 catalytic combustion reactions. Summary of the invention
[0005] To this end, the technical problem to be solved by the present invention is to provide a catalyst for catalytic combustion of low-concentration methane, the catalyst having excellent activity and long-lasting thermal stability;
[0006] The second technical problem to be solved by the present invention is to provide a preparation method and application of a catalyst for catalytic combustion of low-concentration methane.
[0007] In order to solve the above technical problems, the present invention discloses a catalyst for catalytic combustion of low-concentration methane, wherein the catalyst comprises CeO2 as a carrier, Pd loaded on the carrier; and a shell structure SiO2.
[0008] In the catalyst, the loading amount of Pd is 1 wt %.
[0009] The present invention also discloses a method for preparing the catalyst for catalytic combustion of low-concentration methane, comprising the following steps:
[0010] (1) Ce(OH)CO3 precursor was successfully prepared by hydrothermal synthesis of Ce(NO3)3·6H2O using polyethylene glycol as surfactant and urea as complexing agent, and the desired support was obtained by further calcination.
[0011] (2) adding Pd(NH3)4(NO3)2 solution as a Pd precursor to the carrier, generating Pd particles by NaBH4 reduction method, and loading them on the carrier. The reactants are aged and dried to obtain the desired Pd-loaded precursor;
[0012] (3) tetraethyl orthosilicate as a silicon source, hexadecyltrimethylammonium bromide as a template, and ammonia water as a catalyst are added to the Pd-loaded precursor. The desired core-shell structure was synthesized.
[0013] Specifically, in step (1):
[0014] The cerium source material is preferably cerium nitrate hexahydrate;
[0015] The complexing agent is preferably urea.
[0016] Specifically, in step (1):
[0017] The molar ratio of the complexing agent to the cerium source material is 70:1-75:1.
[0018] Specifically, in step (1):
[0019] Control the water heating temperature to 90℃-110℃;
[0020] Controlling the temperature of the drying step to be 70-90°C;
[0021] The temperature of the calcining step is controlled to be 550-650°C.
[0022] Specifically, in step (2),
[0023] The reducing agent is preferably NaBH4.
[0024] Specifically, in step (2):
[0025] The amount of Pd(NH3)4(NO3)2 is 1wt% of the carrier mass based on the amount of Pd;
[0026] The molar ratio of the reducing agent to the Pd source material is 3:1-1:1.
[0027] Specifically, in step (2):
[0028] Controlling the temperature of the aging step to be 30-40°C;
[0029] The temperature of the drying step is controlled to be 70-90°C.
[0030] Specifically, in step (3):
[0031] The molar ratio of tetraethyl orthosilicate to hexadecyltrimethylammonium bromide is 8:1-12:1
[0032] Specifically, in step (3):
[0033] The aging temperature is controlled at 30℃-40℃;
[0034] Controlling the temperature of the drying step to be 70-90°C;
[0035] The temperature of the calcining step is controlled to be 550-650°C.
[0036] The invention also discloses a catalyst for catalytic combustion of low-concentration methane prepared by the method.
[0037] The invention also discloses application of the catalyst in low-concentration methane catalytic combustion reaction.
[0038] The invention also discloses a low-concentration methane catalytic combustion reaction, comprising the step of carrying out a catalytic reaction with the catalyst.
[0039] The catalyst for catalytic combustion of low-concentration methane described in the present invention is that Ce(NO3)3·6H2O is used as a hydrothermal synthesis method to successfully prepare a Ce(OH)CO3 precursor under the condition of using polyethylene glycol as a surfactant and urea as a complexing agent, and further calcined to obtain a desired carrier; Pd(NH3)4(NO3)2 solution is added to the carrier as a Pd precursor, and Pd particles are generated by a NaBH4 reduction method and loaded on the carrier. The reactants are subjected to aging and drying treatments to obtain the desired Pd-loaded precursor; tetraethyl orthosilicate is added to the Pd-loaded precursor as a silicon source, hexadecyltrimethylammonium bromide as a template, and ammonia water as a catalyst, and the catalyst is added by The method can synthesize the required core-shell structure and can be applied to the catalytic combustion reaction of low-concentration methane. The catalyst shows outstanding stability during the continuous combustion reaction. That is, after seven consecutive operations, it can still maintain a high catalytic effect. The catalyst preparation process of the present invention is simple, can be operated for a long time, is suitable for practical application, and has good practical application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] In order to make the content of the present invention more clearly understood, the present invention is further described in detail below according to specific embodiments of the present invention in conjunction with the accompanying drawings, wherein:
[0041] Figure 1 This is a performance comparison result diagram of the core-shell structure Pd / CeO2@SiO2 catalyst of the present invention, Pd / CeO2 and Pd / SiO2 under the same conditions;
[0042] Figure 2 The catalyst Pd / CeO2@SiO2 of the present invention is used for the cyclic stability test of low-concentration methane catalytic combustion;
[0043] Figure 3 (a) and (c) are SEM images of the Pd / CeO2@SiO2 catalyst of the present invention before and after 7 cycles of reaction. Figure 3 (b) and (d) are the average sizes of microspheres before and after 7 cycles of the Pd / CeO2@SiO2 catalyst test;
[0044] Figure 4 (a) TEM and (b) HRTEM images of the Pd / CeO2@SiO2 catalyst of the present invention;
[0045] Figure 5 (a) TEM line scan image and (b) EDX image of the Pd / CeO2@SiO2 catalyst of the present invention. DETAILED DESCRIPTION
[0046] Example 1
[0047] 5 mmol Ce(NO3)3·6H2O and 9.6 g PEG-20000 were added to 180 mL deionized water. Then, 60 mL of 6 mol L -1 (NH2)2CO solution. Then, it was transferred to an autoclave and hydroheated at 100°C for 3 hours. After the autoclave was cooled, the white product was separated by centrifugation. Subsequently, it was centrifuged and washed to remove impurities. Finally, it was dried at 80°C for 12 hours and calcined at 600°C for 4 hours to obtain CeO2 balls. During the preparation process, the active ingredient Pd was loaded on the surface of the carrier by NaBH4 reduction method. First, 0.1mmol Pd(NH3)4(NO3)2 and 0.7mmol Na3C6H5O7·2H2O were dissolved in 30mL deionized water. Next, a certain amount of CeO2 carrier was added, and the CeO2 microspheres were fully dispersed by ultrasonic and stirring treatment (0.5 hours each). Then, 2mL of 0.1mol L -1 The mixture was stirred at room temperature for 12 hours. After stirring, the mixture was centrifuged and washed to obtain a Pd / CeO2 intermediate. Subsequently, the Pd / CeO2 intermediate was calcined at 600°C for 4 hours to obtain the final Pd / CeO2 catalyst.
[0048] Example 2
[0049] 0.1 mmol Pd(NH3)4(NO3)2 and 0.7 mmol Na3C6H5O7·2H2O were dissolved in 30 mL of deionized water. Then, a certain amount of SiO2 carrier was added, and the SiO2 microspheres were fully dispersed by ultrasonic and stirring treatment (0.5 h each). Then, 2 mL of 0.1 mol L -1 The NaBH4 solution was added and stirred at room temperature for 12 hours. After stirring, it was washed by centrifugation and calcined at 600°C for 4 hours to obtain the final Pd / SiO2 catalyst.
[0050] Example 3
[0051] According to the Pd / CeO2 intermediate prepared as in Example 1, 45 mg of CTAB and 400 μL of ammonia solution were added and uniformly dispersed in a mixed solvent consisting of 20 mL of deionized water and 50 mL of ethanol. Then, it was stirred at room temperature for 2 hours to ensure sufficient mixing. Thereafter, 300 μL of TEOS was slowly added, and the reaction was continued at room temperature for 6 hours to complete the coating process of the silicon shell layer. After the reaction was completed, centrifugal washing was performed to remove unreacted substances. Subsequently, it was dried at 80°C overnight. Finally, a calcination treatment was performed at 600°C for 4 hours to obtain the final core-shell structure, labeled as Pd / CeO2@SiO2.
[0052] Experimental example
[0053] In the following experimental examples of the present invention, the activity test results of the catalyst are Figure 1 As shown, the reaction gas is a standard gas composed of CH4, O2 and N2, which passes through a mass flow meter and a flow display. The catalyst activity test is carried out in a quartz tube fixed bed reactor. The inner diameter of the quartz tube is 6mm and the length is 310mm. 100mg of catalyst is placed in the constant temperature zone of the reaction tube, fixed on both sides with quartz wool, and heated by an electric furnace. A thermocouple is inserted in the furnace wall for temperature testing and control.
[0054] The feed gas is 1 vol% CH4, 10 vol% O2, and the rest is balanced by N2. The total gas flow rate is 50 mL / min, and the mass flow meters have been calibrated with soap film flow meters. The tail gas analysis uses a Pano A60 gas chromatograph for automatic sampling and online analysis. The gas chromatograph is set to cyclic automatic sampling, and the tail gas composition is analyzed online. The concentrations of CH4 and CO2 are measured by a hydrogen flame ionization detector (FID) equipped with a Ni converter, while the concentration of O2 is measured by a thermal conductivity detector (TCD). During the experiment, the gas composition at each temperature point needs to be stabilized for 30 minutes before detection.
[0055] 1. Effect of catalyst on low concentration methane conversion rate
[0056] Take 100 mg of the catalyst prepared in the above examples 1-3 and place it in the constant temperature zone of the fixed bed reactor quartz tube, fix it on both sides with quartz wool, and heat it with an electric furnace. Introduce the reaction gas in the above manner, the specific composition is: 1 vol% CH4, 10 vol% O2, and the rest is balanced by N2, the total gas flow rate is 50 mL / min, the reaction temperature range is controlled to be 250℃-600℃, and sampling is performed every 25℃. Each temperature point needs to be stabilized for 30 minutes before testing. The tail gas analysis adopts A60 gas chromatograph for automatic sampling and online analysis. The CH4 conversion rate X can be calculated by formula (1):
[0057]
[0058] The test results are attached. Figure 1 As shown in Figure 2, the effects of different catalysts on methane conversion were investigated. Pd / SiO2 showed the worst performance, with a CH4 conversion rate of only 33% even at a reaction temperature of 600°C. However, Pd / CeO2@SiO2 had a lower (T 50 is 360℃, T 90 The catalytic activity of Pd / CeO2 (T 50 330℃, T 90 390 °C), which may be because some active Pd species are covered by the SiO2 shell, preventing the active sites from being fully exposed, thereby limiting the contact of these active sites with the reactants.
[0059] 2. Catalyst used for low concentration methane catalytic combustion cycle stability test
[0060] Take 100mg of the above Pd / CeO2@SiO2 catalyst and place it in the constant temperature zone of the quartz tube of the fixed bed reactor, fix it with quartz wool on both sides, and heat it with an electric furnace. The reaction gas is introduced, the specific composition is: 1vol% CH4, 10vol% O2, and the rest is balanced with N2. The total gas flow rate is 50mL / min, and the reaction temperature range is controlled to be 250℃-600℃. Samples are taken every 25℃, and each temperature point needs to be stabilized for 30 minutes before testing. After the first round of tests is completed, the heating is stopped and it is waited for it to cool naturally to room temperature. After the temperature stabilizes, a new round of catalytic activity evaluation is carried out again under the same test conditions as the first test to ensure the consistency and comparability of subsequent tests, so as to determine the stability of the catalyst.
[0061] The test results are attached Figure 2 As shown in the figure, the catalyst of the present invention was used for the cyclic stability test of low-concentration methane catalytic combustion. The results show that Pd / CeO2@SiO2 is an efficient and stable catalyst with a low ignition temperature and excellent anti-sintering performance. It is worth noting that even after seven consecutive uses, the catalyst can still maintain high activity for CH4 catalytic combustion, and has good practical application prospects.
[0062] 3. Catalyst structure characterization
[0063] The Pd / CeO2@SiO2 with the best test effect was characterized, and its SEM images before and after 7 cycles of testing are shown in the attached figure. Figure 3As shown in (a) and (c), the SEM image shown in Figure (a) shows that the catalyst presents a uniform and monodisperse microsphere structure, with an average diameter of approximately 293 nm, which verifies the successful synthesis of CeO2 microspheres and also shows the high regularity of the catalyst surface morphology; as shown in Figure (c) after 7 cycles of testing, the SEM of Pd / CeO2@SiO2 maintained its microsphere structure, with no significant growth or change in size, and the average size of the microspheres increased to 296 nm; this result indicates that SiO2 added as a shell layer has a significant effect on maintaining the structural stability of Pd / CeO2 under high temperature reaction conditions, and effectively prevents the growth of microsphere size due to sintering, which is crucial to the performance and life of the catalyst. Figure 4 It can be seen from the TEM image shown in (a) that an amorphous SiO2 shell layer has been successfully grown on the surface of the CeO2 core. And this shell layer tightly wraps the core to form a clear core-shell interface. Further analysis by high-resolution HRTEM shows that obvious metal stripes can be observed in the HRTEM image in (b), and the lattice spacing is 0.31nm. This feature is consistent with the lattice spacing of the (111) crystal plane of CeO2. However, no lattice stripes attributable to the Pd species were observed in the HRTEM image, which indicates that Pd may exist in the material in a highly dispersed form, or its particle size is too small to be detected in HRTEM. In order to more accurately analyze the formation of the Pd / CeO2@SiO2 core-shell structure and its element distribution, the following experiments were carried out. Figure 5 Line scan analysis shown in (a). The line scan results show that the signal of Si is stronger at both ends of the microsphere and the thickness of the Si layer is about 15nm. At the same time, the signals of Ce and Pd elements are evenly distributed in the core area of the microsphere, further proving the core-shell structure with Pd / CeO2 as the core and SiO2 as the shell. Finally, the EDX element distribution in Figure (b) reveals that Pd, Ce, O and Si are evenly distributed on Pd / CeO2@SiO2, and there is no obvious aggregation of Pd particles. This shows that even after calcination at a temperature as high as 600℃ for 4 hours, the catalyst can still maintain its spherical morphology and highly dispersed Pd species, which are crucial properties for catalytic activity and stability.
[0064] The above results show that the hydrothermal method, deposition-precipitation method and The Pd / CeO2@SiO2 catalyst with a core-shell structure was successfully prepared by using a variety of synthesis strategies such as the SiO2 method. A series of characterization analyses confirmed that the formed SiO2 shell not only effectively encapsulated the Pd metal nanoparticles, but also effectively inhibited the migration and aggregation of these particles in a high-temperature environment. The cyclic stability test showed that compared with Pd / CeO2 without a SiO2 shell, Pd / CeO2@SiO2 exhibited outstanding stability during the continuous combustion reaction. That is, after seven consecutive runs, it can still maintain a high catalytic effect, T 50 From 360℃ to 325℃, T 90 It also dropped from 405°C to 385°C.
[0065] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.
Claims
1. A catalyst for catalytic combustion of low-concentration methane, characterized in that: The catalyst comprises CeO2 as a carrier, Pd loaded on the carrier, and a shell structure of SiO2; In the catalyst, the loading amount of Pd is 1 wt %.
2. A method for preparing the catalyst for catalytic combustion of low-concentration methane according to claim 1, characterized in that: The steps include: (1) Ce(OH)CO3 precursor was successfully prepared by hydrothermal synthesis of Ce(NO3)3·6H2O using polyethylene glycol as surfactant and urea as complexing agent, and then further calcined to obtain the desired support CeO2; (2) adding Pd(NH3)4(NO3)2 solution as a Pd precursor to the carrier, generating Pd particles by NaBH4 reduction method, and loading them on the carrier. The reactants are aged and dried to obtain the desired Pd-loaded precursor; (3) tetraethyl orthosilicate as a silicon source, hexadecyltrimethylammonium bromide as a template, and ammonia water as a catalyst are added to the Pd-loaded precursor. Method to synthesize the desired core-shell structure.
3. The method for preparing the catalyst for catalytic combustion of low-concentration methane according to claim 2, characterized in that: In the step (1): The molar ratio of the complexing agent to the cerium source material is 70:1-75:
1. Control the water heating temperature to 90℃-110℃; Controlling the temperature of the drying step to be 70-90°C; The temperature of the calcining step is controlled to be 550-650°C.
4. The method for preparing the catalyst for catalytic combustion of low-concentration methane according to claim 2, characterized in that: In the step (2): The amount of Pd(NH3)4(NO3)2 is 1wt% of the carrier mass based on the amount of Pd; The molar ratio of the reducing agent to the Pd source material is 3:1-1:
1.
5. The method for preparing the catalyst for catalytic combustion of low-concentration methane according to claim 2, characterized in that: In the step (2): Controlling the temperature of the aging step to be 30-40°C; The temperature of the drying step is controlled to be 70-90°C.
6. The method for preparing the catalyst for catalytic combustion of low-concentration methane according to claim 2, characterized in that: In the step (3): The molar ratio of tetraethyl orthosilicate to hexadecyltrimethylammonium bromide is 8:1-12:
1.
7. The method for preparing the catalyst for catalytic combustion of low-concentration methane according to claim 2, characterized in that: In the step (3): The aging temperature is controlled at 30℃-40℃; Controlling the temperature of the drying step to be 70-90°C; The temperature of the calcining step is controlled to be 550-650°C.
8. A catalyst for catalytic combustion of low-concentration methane prepared by the method according to any one of claims 2 to 7.
9. A low concentration methane catalytic combustion reaction, characterized in that: The method comprises the step of carrying out a catalytic reaction using the catalyst according to claim 1 or 8.
Citation Information
Patent Citations
Palladium-based core-shell-structure catalyst for catalytic combustion of low-concentration methane and preparation method of palladium-based core-shell-structure catalyst
CN113385217A
Catalyst for deoxidation of coalbed gas, preparation method and use thereof
WO2011009283A1
Cited By
An environmentally friendly catalyst for promoting efficient and clean combustion of pulverized coal and its preparation method
CN119771430A
Rare earth oxide modified supported palladium catalyst for catalyzing methane oxidation at low temperature and preparation method of rare earth oxide modified supported palladium catalyst
CN120155181A