Molecular sieve confinement metal catalyst capable of synchronously decomposing NO and N2O and preparation method thereof

By using the dual-active central molecular sieve limited domain metal catalyst prepared by desilicate recrystallization and ion exchange method under medium and low temperature conditions, the problem of high cost of joint removal of NO and N2O in the prior art is solved, and efficient and economical catalysis is achieved Decomposition effect and improve the stability and toxicity of the catalyst.

CN118892860APending Publication Date: 2024-11-05SHANXI UNIV
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410952738.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The prior art requires the use of a large number of reducing agents when removing NO, NO2 and N2O from industrial exhaust gas, resulting in high operating costs and difficulty in achieving joint decomposition and removal of NO and N2O in the medium and low temperature range.

Method used

A dual active center molecular sieve restriction metal catalyst is prepared by desilicate recrystallization and ion exchange method. Transition metal ions and oxides such as Mn, Ni, Co, Fe, Cu can be used as active components, and can be used at medium and low temperatures. Directly catalyze the decomposition of NO and N2O into N2 and O2, without the need to add reducing gases such as CH4, NH3 or CO.

Benefits of technology

Direct catalytic decomposition of NO and N2O under medium and low temperature conditions is achieved, which reduces operating costs and improves the economic and safety of the catalyst. The catalyst has excellent anti-aggregation and anti-impact gas toxicity properties, which is suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004947675870000081
    Figure BDA0004947675870000081
  • Figure BDA0004947675870000091
    Figure BDA0004947675870000091
Patent Text Reader

Abstract

The invention relates to a molecular sieve confinement metal catalyst capable of synchronously decomposing NO and N2O and a preparation method of the molecular sieve confinement metal catalyst, and belongs to the technical field of denitration catalyst preparation. The preparation method comprises the following steps: firstly, encapsulating one or more of manganese oxide, nickel oxide and cobalt oxide nanoparticles in a molecular sieve bulk phase by adopting a desilicication recrystallization method so as to catalyze N2O decomposition; and introducing one or more of Fe < 2 + >, Co < 2 + > and Cu < 2 + > into the ion exchange site of the molecular sieve through an ion exchange process to catalyze NO decomposition. The obtained catalyst takes MFI type and BEA type molecular sieves as carriers and transition metal oxides and transition metal ions as active components, can efficiently and synchronously catalyze the decomposition of NO and N2O within the range of 400-500 DEG C under the condition that reducing gases such as CH4, NH3 or CO are not added, has excellent agglomeration resistance and impurity gas resistance, and has great application potential in the field of industrial tail gas denitration.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of denitration catalyst preparation, and specifically relates to a molecular sieve confined metal catalyst capable of simultaneously decomposing NO and N2O and a preparation method thereof. Background Art

[0002] Nitrogen oxides are one of the main air pollutants, including nitrogen and oxygen combinations such as nitric oxide (NO), nitrogen dioxide (NO2) and nitrous oxide (N2O), of which NO accounts for more than 80%. NO and NO2 can induce acid rain, especially under light conditions, they can generate highly toxic photochemical smog through a series of photochemical reactions, which is extremely harmful to the environment. N2O is a non-carbon dioxide strong greenhouse gas, with a warming latent heat of 298 times that of CO2 and 28 times that of CH4, and can exist stably in the atmosphere for more than 150 years, exacerbating the greenhouse effect. Nitrogen oxides in the stratosphere can also react with ozone, leading to the formation of ozone holes. Thermal power generation, motor vehicle exhaust emissions, agricultural fertilizer production and use, and upstream and downstream industries of nitric acid are the main sources of anthropogenic nitrogen oxide emissions, and are also one of the main reasons for the imbalance of the natural nitrogen cycle, accelerated environmental pollution and climate change. As early as 2020, my country proposed the dual carbon strategy of "carbon peak and carbon neutrality", requiring the acceleration of low-carbon emission reduction and the promotion of green economic development.

[0003] Currently, nitrogen oxides in industrial exhaust are mainly removed by selective catalytic reduction (SCR technology). This method uses NH3, CO and CH4 as reducing agents to reduce NO X Selectively reduced to non-toxic and harmless N2 and H2O, the removal efficiency can reach more than 80%. However, it is difficult to remove N2O with SCR technology, and another reactor is required to decompose N2O into N2 and O2 through a high-temperature catalytic process. This method of graded removal of nitrogen oxides not only has high construction and operating costs, but also greatly increases the risk of system operation. Therefore, the development of a combined removal technology for NO, NO2 and N2O is of great significance for reducing the cost of reducing industrial exhaust nitrogen oxide emissions and helping my country achieve its "dual carbon" goals.

[0004] Chinese patent CN 106423184 A discloses a technical solution for the combined removal of NO, NO2 and N2O. The solution uses vanadium pentoxide and cobalt-based composite metal oxides as catalysts. It can directly catalyze the decomposition and removal of N2O in the range of 300-450°C, while NO and NO2 are removed through SCR denitration reaction. The total nitrogen oxide removal rate can reach more than 80%. Chinese patent CN115739172 A discloses a catalyst for the synergistic removal of N2O and NO and its preparation method. The invention uses NH4-type Beta and NH4-type ZSM-5 molecular sieves as carriers, introduces one of the active components Fe, Co and Cu by impregnation, and mixes with pseudo-boehmite and sesbania powder for extrusion molding. Under the action of the catalyst, part of N2O can react with NO to generate N2 and NO2, and the generated NO2 is further removed by rapid SCR reaction. In the range of 400-600°C, the nitrogen oxide removal rate can reach more than 90%. Chinese patent CN 102574108 A also discloses a mixed metal oxide catalyst for decomposing nitrogen oxides. The catalyst of the invention uses hydrotalcite containing alkali metals as a precursor, selects non-precious metals such as Ni, Co and Fe for intercalation treatment, and obtains a composite metal oxide catalyst through high-temperature calcination. When CO is selected as a reducing agent, the obtained catalyst can completely reduce NO and N2O to N2 and H2O at 250°C.

[0005] Although there is currently NO X There are reports on the combined removal technology of NO and N2O, but most of these technologies are a combination of N2O decomposition technology and SCR denitrification technology. A large amount of reducing agent is required in the reaction process, and the operating cost is still high. X The combined decomposition and removal technology of N2O needs to be developed urgently. Summary of the invention

[0006] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide a molecular sieve confined metal catalyst that can simultaneously decompose NO and N2O and a preparation method thereof. The present invention adopts desiliconization recrystallization + ion exchange method to couple the catalyst, and the obtained catalyst has a double active center, which directly catalyzes the decomposition of NO and N2O into N2 and O2 in the medium and low temperature range, and the reaction process does not require the addition of reducing gases such as CH4, NH3 or CO.

[0007] To achieve the above object, the technical solution of the present invention is as follows:

[0008] A method for preparing a molecular sieve confined metal catalyst capable of simultaneously decomposing NO and N2O comprises the following steps:

[0009] Step 1: one or more of Mn salt, Ni salt and Co salt solution are added dropwise to the molecular sieve sample, and then dried and calcined after being allowed to stand for a long time;

[0010] Step 2: immerse the sample calcined in step 1 in an alkali solution, stir it thoroughly, and then crystallize, wash, dry and calcine it;

[0011] Step 3: Mix one or more aqueous solutions of Fe salt, Co salt and Cu salt with the sample calcined in step 2, stir thoroughly and centrifuge, then immerse the solid sample after centrifugation in the same metal salt aqueous solution, stir thoroughly and centrifuge, repeat this process for multiple times, and then dry and calcine to obtain the molecular sieve confined metal catalyst.

[0012] Furthermore, in steps 1 and 3, the Mn salt, Ni salt, Co salt, Fe salt and Cu salt are corresponding nitrates, sulfates, chlorides or acetates; the metal ion concentration in the aqueous solution of Mn salt and Ni salt is 0.2-1.5 mol / L, the metal ion concentration in the aqueous solution of Fe salt and Cu salt is 0.01-0.8 mol / L, and the metal ion concentration in the aqueous solution of Co salt is 0.05-1.5 mol / L.

[0013] Furthermore, in step 2, the alkali solution is a quaternary ammonium base or a mixed base thereof with an inorganic base, wherein the quaternary ammonium base includes tetrapropylammonium hydroxide and tetraethylammonium hydroxide, the inorganic base includes sodium hydroxide and potassium hydroxide, and the cation concentration in the quaternary ammonium base is 0.3 to 1 mol L -1 The concentration of hydroxide ions in the inorganic base is 0 to 0.7 mol L -1 Furthermore, the alkali solution also contains quaternary ammonium salts, including tetrapropylammonium bromide and tetraethylammonium bromide, and the cation concentration in the quaternary ammonium salts is 0 to 1 mol L -1 .

[0014] Furthermore, in step 1, the molecular sieve is a Na-type, NH4-type or H-type BEA or MFI molecular sieve; the silicon-aluminum ratio of the molecular sieve is 27 to 200; the solid-liquid ratio of the molecular sieve to the metal salt solution is 1 g / 5 mL to 1 g / 0.9 mL; and the standing conditions are 25 to 60° C. for 3 to 24 hours.

[0015] Furthermore, in step 2, the solid-liquid ratio of the molecular sieve to the alkali solution is 1 g / 50 mL to 1 g / 10 mL; the stirring conditions are 27 to 80° C., 0.5 to 12 h; and the crystallization conditions are 120 to 200° C., 3 to 24 h.

[0016] Furthermore, in step 3, the solid-liquid ratio of the molecular sieve to the metal salt aqueous solution is 1g / 50mL-1g / 20mL; the stirring conditions are 20-80°C, 0.5-6h; the number of repetitions is 2-5 times; the drying conditions in steps 1-3 are 80-120°C, 6-12h; and the calcination conditions are 450-550°C, 2-6h.

[0017] A molecular sieve confined metal catalyst prepared by the preparation method as described above, with BEA type or MFI type molecular sieve as carrier, transition metal ions located at the ion exchange sites of the molecular sieve framework and transition metal oxides encapsulated in the molecular sieve body phase as active components; wherein the transition metal ions are Fe 2+ 、Co 2+ and Cu 2+ One or more of the transition metal oxides, and the transition metal oxides are one or more of manganese oxides, nickel oxides and cobalt oxides.

[0018] Furthermore, the content of the transition metal ion accounts for 0.5-1.5wt% of the total mass of the catalyst, and the content of the transition metal oxide accounts for 5-30wt% of the total mass of the catalyst.

[0019] An application of the molecular sieve confined metal catalyst as described above in the combined removal of NO and N2O.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] (1) The present invention realizes the direct catalytic decomposition of NO and N2O in a medium-low temperature environment by constructing a molecular sieve confined metal catalyst containing dual active centers, avoiding the use of reducing gases such as CH4, CO and NH3. It is more economical and safer than traditional SCR denitrification technology, and is more environmentally friendly;

[0022] (2) The catalyst of the present invention uses structurally stable MFI and BEA molecular sieves as carriers, and the active species transition metal ions and transition metal oxides are distributed in the micro-nano confined space provided by the molecular sieves, and has excellent anti-agglomeration and anti-poisoning properties against impurity gases;

[0023] (3) The catalyst of the present invention is prepared by coupling desiliconization recrystallization and ion exchange, and the preparation process is simple, the conditions are mild, and it is suitable for large-scale industrial production. DETAILED DESCRIPTION

[0024] In order to facilitate the understanding of the present invention, the present invention will be described more fully below. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.

[0025] Example 1

[0026] (1) Weigh 2 g of H-type ZSM-5 molecular sieve (Si / Al=46) and set aside; weigh 0.52 g of cobalt nitrate hexahydrate and dissolve it in 1.8 mL of deionized water and set aside; prepare 0.3 mol / L tetrapropylammonium hydroxide aqueous solution and 0.05 mol / L copper nitrate aqueous solution and set aside;

[0027] (2) adding a cobalt nitrate aqueous solution dropwise into the weighed H-type ZSM-5 molecular sieve, standing at 40°C for 6 hours, drying in a forced air drying oven at 80°C for 6 hours, and finally calcining in a muffle furnace at 500°C for 4 hours to obtain a ZSM-5 catalyst loaded with Co3O4 nanoparticles;

[0028] (3) The calcined sample was immersed in 40 mL of 0.3 mol L -1 The sample was placed in a tetrapropylammonium hydroxide aqueous solution and stirred vigorously at 30°C for 30 min, then placed in a 100 mL polytetrafluoroethylene hydrothermal crystallization kettle and hydrothermally crystallized at 170°C for 24 h, and then the crystallized sample was washed by centrifugation with deionized water until the pH of the centrifuge was 7;

[0029] (4) The wet sample after centrifugation was dried in a forced air drying oven at 100°C for 12 h and then calcined in a muffle furnace at 550°C for 6 h;

[0030] (5) Add the calcined sample to 60 mL of a 0.05 mol / L copper nitrate aqueous solution and stir thoroughly at 30 °C for 6 h. Then separate the wet solid sample by centrifugation. Repeat this process twice.

[0031] (6) The obtained wet solid sample was dried in a forced air drying oven at 100°C for 12 h, and then calcined in a muffle furnace at 500°C for 4 h to obtain Co3O4-Cu with a Co3O4 and Cu mass percentage of 5.5% and 1.0% respectively (measured by XRF). 2+ / ZSM-5 molecular sieve catalyst;

[0032] (7) The prepared catalyst was heated to 0.1% N2O, 0.03% NO / N2, and a space velocity of 10000 h -1 The activity was evaluated under the conditions of , the catalyst loading was 300 mg, the catalyst particle size was 40-60 mesh, the reaction temperature started from 240°C, and data was collected every 20°C increase in temperature. The evaluation results are shown in Table 1.

[0033] Example 2

[0034] The H-type ZSM-5 molecular sieve used in step (1) of Example 1 was replaced with an H-type Beta molecular sieve with the same silicon-aluminum ratio, the mass of cobalt nitrate hexahydrate was increased from 0.52 g to 1.56 g, and the other catalyst preparation conditions remained unchanged to obtain Co3O4-Cu with a Co3O4 and Cu mass percentage of 16.5% and 0.9% respectively (measured by XRF). 2+ / Beta molecular sieve catalyst. The catalyst activity evaluation conditions were the same as those in Example 1, and the evaluation results are shown in Table 1.

[0035] Example 3

[0036] The H-type ZSM-5 molecular sieve used in step (1) of Example 1 was replaced with an H-type Beta molecular sieve with the same silicon-aluminum ratio, the mass of cobalt nitrate hexahydrate increased from 0.52 g to 1.56 g, and the alkali solution in step (3) increased from 0.3 mol L -1 The tetrapropylammonium hydroxide aqueous solution was replaced with 0.3 mol L -1 tetrapropylammonium hydroxide aqueous solution and 0.1 mol L -1 The solid-liquid ratio of the molecular sieve to the alkali solution in step (3) was changed from 1 g / 20 mL to 1 g / 50 mL, and the other catalyst preparation conditions remained unchanged to obtain Co3O4-Cu with a Co3O4 and Cu mass percentage of 14.5% and 1.3% (measured by XRF), respectively. 2+ / Beta molecular sieve catalyst. The catalyst activity evaluation conditions were the same as those in Example 1, and the evaluation results are shown in Table 1.

[0037] Example 4

[0038] The H-type ZSM-5 molecular sieve used in step (1) of Example 1 was replaced with an H-type Beta molecular sieve with the same silicon-aluminum ratio, and the 0.52 g of cobalt nitrate hexahydrate used in step (1) was replaced with 0.64 g of nickel nitrate hexahydrate. The other catalyst preparation conditions remained unchanged to obtain NiO-Cu with NiO and Cu mass percentages of 6.5% and 1.1% respectively (measured by XRF). 2+ / Beta molecular sieve catalyst. The catalyst activity evaluation conditions were the same as those in Example 1, and the evaluation results are shown in Table 1.

[0039] Example 5

[0040] The catalyst preparation conditions were the same as those in Example 3. The reaction space velocity during the catalyst activity evaluation was increased from 10000 h / min in Example 1 to -1 Increase to 60000h -1 , the other evaluation conditions remain unchanged, and the evaluation results are shown in Table 1.

[0041] Example 6

[0042] The catalyst preparation conditions were the same as those in Example 3. The reaction atmosphere for the catalyst activity evaluation conditions was changed from 0.1% N2O, 0.03% NO / N2 in Example 1 to 0.1% N2O, 0.05% NO, 1.0% O2 / N2, and the other evaluation conditions remained unchanged. The evaluation results are shown in Table 1.

[0043] Comparative Example 1

[0044] (1) Dissolve 10.00 g of cobalt nitrate hexahydrate in 75 mL of deionized water for later use;

[0045] (2) preparing a 1 mol / L aqueous ammonium carbonate solution, and adding it dropwise to the aqueous cobalt nitrate solution prepared in step (1) until the solution pH = 9, stirring continuously for 1 hour, and aging at room temperature for 3 hours;

[0046] (3) Using deionized water to filter and wash the precipitate obtained by aging until the pH of the filtrate is 7;

[0047] (4) drying the wet solid sample obtained by washing in an oven at 120° C. for 6 h, and calcining it in a muffle furnace at 400° C. for 2 h, thereby obtaining a Co3O4 catalyst;

[0048] (5) The catalytic performance of the Co3O4 catalyst was evaluated using the reaction conditions in Example 1. The evaluation results are shown in Table 1.

[0049] Comparative Example 2

[0050] (1) Prepare a 0.05 mol / L copper nitrate aqueous solution for later use;

[0051] (2) Weigh 2 g of H-type Beta molecular sieve and immerse it in 60 mL of 0.05 mol / L copper nitrate aqueous solution, stir vigorously at 30° C. for 12 h, then wash it three times with deionized water by centrifugation, and dry it in an oven at 100° C. for 12 h;

[0052] (3) The dried sample was calcined at 500°C for 4 h in a muffle furnace to obtain Cu 2+ Ion exchanged Cu 2+ / Beta molecular sieve catalyst, wherein the mass of Cu accounts for 1.0% of the total mass of the catalyst;

[0053] (4) Using the reaction conditions in Example 1 to evaluate Cu 2+ The catalytic performance of the / Beta molecular sieve catalyst is evaluated and shown in Table 1.

[0054] Comparative Example 3

[0055] The 0.05 mol / L copper nitrate aqueous solution used in Comparative Example 2 was replaced with a 0.08 mol / L cobalt nitrate aqueous solution, and the other catalyst preparation conditions were the same as those in Comparative Example 2 to prepare Co 2+ Ion exchanged Co 2+ / Beta molecular sieve catalyst, wherein the mass of Co accounts for 1.3% of the total mass of the catalyst. The catalyst activity evaluation conditions are the same as those in Example 1, and the evaluation results are shown in Table 1.

[0056] Table 1 lists the catalytic activity evaluation results of the catalysts in Examples 1-6 and Comparative Examples 1-3. 2+ The / Beta catalyst can simultaneously catalyze the decomposition conversion rates of N2O and NO at 440°C to reach 100% and 80% respectively. Its catalytic activity is significantly better than that of single-component metal oxide catalysts and single-active component molecular sieve catalysts, and it has excellent resistance to O2 inhibition.

[0057] Table 1 Evaluation results of catalytic activity of catalysts in Examples 1-6 and Comparative Examples 1-3

[0058]

[0059]

[0060] The above description is only for better explaining the embodiments of the present invention, and is not intended to limit the present invention. Any modification or equivalent substitution that does not depart from the spirit and scope of the present invention shall fall within the scope of the present invention.

Claims

1. A method for preparing a molecular sieve confined metal catalyst capable of simultaneously decomposing NO and N2O, characterized in that: The following steps are involved: Step 1: one or more of Mn salt, Ni salt and Co salt solution are added dropwise to the molecular sieve sample, and then dried and calcined after being allowed to stand for a long time; Step 2: immerse the sample calcined in step 1 in an alkali solution, stir it thoroughly, and then crystallize, wash, dry and calcine it; Step 3: Mix one or more aqueous solutions of Fe salt, Co salt and Cu salt with the sample calcined in step 2, stir thoroughly and centrifuge, then immerse the solid sample after centrifugation in the same metal salt aqueous solution, stir thoroughly and centrifuge, repeat this process for multiple times, and then dry and calcine to obtain the molecular sieve confined metal catalyst.

2. The method for preparing a molecular sieve confined metal catalyst capable of simultaneously decomposing NO and N2O according to claim 1, characterized in that: In steps 1 and 3, the Mn salt, Ni salt, Co salt, Fe salt and Cu salt are corresponding nitrates, sulfates, chlorides or acetates; the metal ion concentration in the aqueous solution of Mn salt and Ni salt is 0.2-1.5 mol / L, the metal ion concentration in the aqueous solution of Fe salt and Cu salt is 0.01-0.8 mol / L, and the metal ion concentration in the aqueous solution of Co salt is 0.05-1.5 mol / L.

3. The method for preparing a molecular sieve confined metal catalyst capable of simultaneously decomposing NO and N2O according to claim 1, characterized in that: In step 2, the alkali solution is a quaternary ammonium base or a mixed base thereof with an inorganic base, wherein the quaternary ammonium base includes tetrapropylammonium hydroxide and tetraethylammonium hydroxide, the inorganic base includes sodium hydroxide and potassium hydroxide, and the cation concentration in the quaternary ammonium base is 0.3 to 1 mol L -1 The concentration of hydroxide ions in the inorganic base is 0 to 0.7 mol L -1 .

4. The method for preparing a molecular sieve confined metal catalyst capable of simultaneously decomposing NO and N2O according to claim 3, characterized in that: The alkali solution also contains quaternary ammonium salts, which include tetrapropylammonium bromide and tetraethylammonium bromide. The cation concentration in the quaternary ammonium salts is 0 to 1 mol L -1 .

5. The method for preparing a molecular sieve confined metal catalyst capable of simultaneously decomposing NO and N2O according to claim 1, characterized in that: In step 1, the molecular sieve is a Na-type, NH4-type or H-type BEA or MFI molecular sieve; the silicon-aluminum ratio of the molecular sieve is 27-200; the solid-liquid ratio of the molecular sieve to the metal salt solution is 1g / 5mL-1g / 0.9mL; and the standing conditions are 25-60°C for 3-24h.

6. The method for preparing a molecular sieve confined metal catalyst capable of simultaneously decomposing NO and N2O according to claim 1, characterized in that: In step 2, the solid-liquid ratio of the molecular sieve to the alkali solution is 1 g / 50 mL to 1 g / 10 mL; the stirring conditions are 27 to 80° C., 0.5 to 12 h; and the crystallization conditions are 120 to 200° C., 3 to 24 h.

7. The method for preparing a molecular sieve confined metal catalyst capable of simultaneously decomposing NO and N2O according to claim 1, characterized in that: In the step 3, the solid-liquid ratio of the molecular sieve to the metal salt aqueous solution is 1g / 50mL-1g / 20mL; the stirring conditions are 20-80°C, 0.5-6h; the number of repetitions is 2-5 times; the drying conditions in the steps 1-3 are 80-120°C, 6-12h; and the roasting conditions are 450-550°C, 2-6h.

8. A molecular sieve confined metal catalyst prepared by the preparation method according to any one of claims 1 to 7, characterized in that: BEA or MFI molecular sieves are used as carriers, and transition metal ions located at the ion exchange sites of the molecular sieve framework and transition metal oxides encapsulated in the molecular sieve body phase are active components; wherein the transition metal ions are Fe 2+ 、Co 2+ and Cu 2+ One or more of the transition metal oxides are manganese oxides, nickel oxides and cobalt oxides.

9. The molecular sieve confined metal catalyst according to claim 8, characterized in that: The content of the transition metal ions accounts for 0.5-1.5 wt% of the total mass of the catalyst, and the content of the transition metal oxide accounts for 5-30 wt% of the total mass of the catalyst.

10. Use of the molecular sieve confined metal catalyst according to claim 8 or 9 in the combined removal of NO and N2O.

Citation Information

Patent Citations

  • Process of direct copper exchange into na+-form of chabazite molecular sieve, and catalysts, systems and methods

    CA2784703A1

  • Ferro-cobalt bimetallic catalyst for catalyzing nitrous oxide (N2O) decomposition

    CN102380410A

  • High-silica molecular sieve catalyst used for nitrous oxide decomposition

    CN105749959A

  • Confined molecular sieve denitrification catalyst and preparation method thereof

    CN109433254A

  • Oxide-molecular sieve composite catalyst as well as preparation method and application thereof

    CN114768861A