Composite dispersion liquid of single-walled carbon nanotubes and preparation method of composite dispersion liquid
By using a composite dispersion of toluene and ethanol and a high-temperature furnace treatment, combined with oxygen and carbon dioxide calcination purification technology, the problems of unstable gas flow and low purity in floating catalytic method are solved, and the yield and quality of single-wall carbon nanotubes are improved. , and realizes an environmentally friendly production process.
Patent Information
- Application Number
- CN202410945205.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-05
AI Technical Summary
In the preparation of single-wall carbon nanotubes, the existing floating catalytic method has problems such as unstable gas flow, changes in the feed port temperature, low product purity, low GD content and low yield when the gas and liquid are mixed with feed.
Using a composite dispersion of toluene and ethanol as the carbon source, combined with preheating treatment of methane and argon, single-wall carbon nanotubes were prepared through a high-temperature furnace, and purified under calcination of oxygen and carbon dioxide, and used acid stirring to remove impurities. Improve product quality and yield.
The production rate and product quality of single-wall carbon nanotubes are improved, the cost is reduced, and the recycling of carbon dioxide is realized, greenhouse gas emissions are reduced, and the product's GDP ratio is improved.
Smart Images

Figure CN118894522A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of single-walled carbon nanotube material synthesis, and in particular to a composite dispersion of single-walled carbon nanotubes and a preparation method thereof. Background Art
[0002] By using chemical vapor deposition to react carbon source gas with a catalyst in a vertical tube furnace, single-walled carbon nanotubes with the characteristics of light weight, pressure resistance, temperature resistance, wear resistance, high aspect ratio, high modulus and high strength can be efficiently prepared. These single-walled carbon nanotubes can be used to improve metal materials and polymer materials to produce materials with high strength, lightning resistance, invisibility, and low temperature and icing resistance. In addition, due to their unique physical properties, single-walled carbon nanotubes are also widely used in chip technology, lithium-ion batteries, aerospace materials, rubber and plastics. In general, chemical vapor deposition and vertical tube furnaces are closely integrated, interdependent and interact with each other to achieve the process of efficiently preparing single-walled carbon nanotubes.
[0003] The existing floating catalytic method has some problems in the preparation process. For example, when the gas and liquid are mixed and fed, the gas is easily expanded by heat and the airflow is unstable, resulting in constant changes in the temperature of the feed port, which in turn affects the volatilization of the liquid and the quality of the product. The product purity of single-walled carbon nanotubes prepared from the existing carbon source materials is low, and the GD ratio content is low, or the yield of the prepared single-walled carbon nanotubes is not high, making it difficult to further improve the production rate and product quality. Summary of the invention
[0004] The present application is made in view of the above-mentioned problems, and its purpose is to provide a composite dispersion of single-walled carbon nanotubes and a preparation method thereof.
[0005] The first aspect of the present application provides a composite dispersion of single-walled carbon nanotubes, comprising a carbon source in a mixed solvent formed by mixing toluene and ethanol in a certain proportion, a metal compound catalyst, a co-catalyst and an etchant to form a dispersion.
[0006] In any embodiment, the metal compound is one or more of ferric chloride, ferrocene, cobalt chloride, and cobaltocene; the co-catalyst is one or more of thiophenol, thiophene, and selenophene; and the etchant is one or more of water, ethylene glycol, and methanol.
[0007] In any embodiment, the metal compound, liquid carbon source, promoter and etchant are used in a ratio of 5-10 g: 60-180 mL: 2-5 mL: 10-15 mL.
[0008] In any embodiment, the ratio of toluene to ethanol is 3-5:1.
[0009] The second aspect of the present application also provides a method for preparing single-walled carbon nanotubes, comprising the following steps:
[0010] S1. Before feeding the dispersion liquid, the liquid needs to be continuously heated and stirred to ensure that it is evenly mixed;
[0011] S2, using methane as the reducing gas and argon as the protective gas, the two enter the gas mixing tank for preheating according to a flow ratio within a certain range;
[0012] S3, introducing the uniformly mixed dispersion into a high-temperature furnace at a certain injection speed, and collecting samples at regular intervals to obtain a crude product;
[0013] S4. Purify the crude product.
[0014] In any embodiment, the heating temperature in step S1 is controlled at 60°C-80°C.
[0015] In any embodiment, in step S2, the gas mixing tank is preheated to obtain a mixed gas with a temperature of 500-800° C. and a pressure of 0.1-0.3 MPa.
[0016] In any embodiment, the ratio of the reducing gas to the protective gas is 2000-5000:2500 sccm.
[0017] In any embodiment, the dispersion feed injection rate is 53.3-60 μL / min.
[0018] In any embodiment, the temperature of the furnace tube of the high temperature furnace in step S3 is 1150-1250°C.
[0019] In any embodiment, the purification process includes: S41. calcining the crude product in oxygen for a period of time; S42. adding a certain concentration of carbon dioxide in a horizontal tube furnace and further reacting under high temperature conditions; S43. stirring with a certain concentration of acid at a certain temperature for a period of time to obtain a pure powder product.
[0020] In any embodiment, the step S41 is performed by air calcination at 1400-1600°C.
[0021] In any embodiment, in step S42, calcination is continued at 1400-1600° C. by introducing 1000-1200 sccm of carbon dioxide (CO 2 ) for 1-2 hours.
[0022] In any embodiment, in step S41, the heating rate is 8°C / min, the gas flow rate of oxygen introduced is about 200-400sccm, and the air oxidation time is 1-2h.
[0023] In any embodiment, the acid in step S43 is 3-6M concentrated hydrochloric acid or concentrated sulfuric acid, and the mixture is heated and stirred at 60-80° C. for 5-10 hours.
[0024] The beneficial effects of the present application: a compound of toluene and ethanol system is used to obtain a high GD and a high yield; the crude product is further calcined for 1-2 hours by introducing 1000-1200sccm of carbon dioxide (CO2) at 1400-1600°C; at high temperature, a small amount of carbon dioxide gas will decompose into double the amount of carbon monoxide. Compared with the traditional method of directly introducing carbon monoxide, this method is more cost-effective. Iron oxide impurities react with carbon monoxide to generate metallic iron (Fe) and carbon dioxide (CO2), and carbon dioxide can be discharged with the tail gas, which can further realize the collection and recycling of carbon dioxide gas, reduce greenhouse gas emissions, and be more environmentally friendly; in hydrochloric acid (HCl) or sulfuric acid (H2SO4) solution, iron (Fe) is easier to remove than iron oxide (FeO2 or Fe2O3). The preparation method of single-walled carbon nanotubes of the present application has a high production rate, and the prepared product is of good quality and low cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a scanning electron micrograph of the purified product of Example 1 of the present application;
[0026] Figure 2 This is the Raman image of the purified product in Example 1 of the present application;
[0027] Figure 3 This is a scanning electron micrograph of the purified product of Example 2 of the present application;
[0028] Figure 4 This is the Raman image of the purified product in Example 2 of the present application;
[0029] Figure 5 This is a scanning electron micrograph of the purified product of Example 3 of the present application;
[0030] Figure 6 This is the Raman image of the purified product in Example 3 of the present application;
[0031] Figure 7 This is a scanning electron microscope image of the purified product of Comparative Example 1;
[0032] Figure 8 This is the Raman image of the purified product in Comparative Example 1;
[0033] Fig. 9 This is a scanning electron microscope image of the purified product of Comparative Example 2.
[0034] Fig.10 This is the Raman image of the purified product in Comparative Example 2.
[0035] Fig.11 This is a scanning electron microscope image of the purified product of Comparative Example 3.
[0036] Fig.12 This is the Raman image of the purified product in Comparative Example 3.
[0037] Fig.13 This is a scanning electron microscope image of the purified product of Comparative Example 4.
[0038] Fig.14 This is the Raman image of the purified product in Comparative Example 4. DETAILED DESCRIPTION
[0039] Hereinafter, an embodiment of a composite dispersion of single-walled carbon nanotubes and a method for preparing the same will be specifically disclosed with appropriate reference to the accompanying drawings. However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repeated descriptions of actually the same structures may be omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate understanding by those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0040] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0041] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0042] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0043] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0044] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0045] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0046] A method for preparing single-walled carbon nanotubes using a solvent compound system mainly includes three steps: first, toluene and ethanol are mixed in different proportions to form a mixed solvent as a carbon source to disperse a metal compound catalyst, a co-catalyst that can provide a sulfur source compound, and an etchant for reducing the amorphous carbon content to form a dispersion liquid, and before the liquid is fed, the liquid needs to be continuously heated and stirred to ensure that it is evenly mixed.
[0047] Secondly, methane is used as the reducing gas and argon as the protective gas. The two are preheated in the gas mixing tank according to a flow ratio within a certain range to keep the temperature constant after the gas flow enters the furnace tube. The dispersion is introduced into the high-temperature furnace at a certain injection speed, and samples are collected every 30 minutes. The growth temperature of single-walled carbon nanotubes is high, but the temperature required for its deposition is much lower than the growth temperature. Prevent excessive carbon tubes from accumulating in the high-temperature zone for a long time and carbonizing, resulting in a decrease in the quality of single-walled carbon nanotubes.
[0048] Finally, the crude product is purified. First, the crude product is continuously calcined in oxygen for a period of time to remove the amorphous carbon on the surface. Amorphous carbon reacts with oxygen under high temperature conditions to generate carbon dioxide and is discharged from the horizontal tube furnace. However, at this time, some iron impurities in the crude single-walled carbon nanotubes are oxidized into iron oxide. Secondly, a certain concentration of carbon dioxide is added to the horizontal tube furnace. Under high temperature conditions, carbon dioxide can be decomposed into carbon monoxide for reducing iron oxide into metallic iron. Under the treatment conditions of hydrochloric acid or sulfuric acid, metallic iron is easier to remove than valence-stable iron oxide. Finally, the crude powder treated by the above steps is stirred for a period of time at a certain temperature using a certain concentration of concentrated acid or concentrated hydrochloric acid to obtain a pure powder product.
[0049] The specific experimental process is as follows:
[0050] Experimental steps:
[0051] 1-3g of metal compound, 60-180mL of liquid carbon source (wherein the ratio of toluene to ethanol is 3-5:1), 2-5mL of co-catalyst and 0.5-1.5mL of etchant are mixed according to the amount. Then, methane reducing gas with a flow rate of 5000-8000sccm and nitrogen protective gas with a flow rate of 2500sccm are injected into the mixing tank for heating to reach and maintain the ideal temperature and pressure, the temperature is 500-800℃ and the pressure is 0.1-0.3MPa. Next, open the outlet pipe valve of the mixing tank to allow the mixed gas to enter the furnace tube. Use a flow rate of 60-80μL / min to introduce the dispersion into a high-temperature furnace at 1200-1250℃, and take a sample every 30 minutes. This is because the generated single-walled carbon nanotubes are mainly deposited on the top of the furnace tube and inside the collection tank, and their temperature is lower than that in the middle of the reactor. The formation temperature of single-walled carbon nanotubes is usually 1150-1200℃, but the deposition temperature needs to be lower, about 500-800℃. If the sample is not taken in time, the product will continue to deposit in the high temperature area, causing the product to become brittle. Therefore, in order to prevent too many carbon nanotubes from accumulating in the high temperature area for a long time and causing the quality of single-walled carbon nanotubes to deteriorate, samples need to be taken every 30 minutes.
[0052] First, the crude product is calcined for 1-2 hours at a high temperature of 1400-1600°C with oxygen at a flow rate of 200-400sccm. The purpose of this step is to remove amorphous carbon on the surface and improve the graphitization degree of the product. In this process, oxygen acts as an oxidant to oxidize amorphous carbon into carbon dioxide (CO2) or carbon monoxide (CO), which is then taken away to achieve the removal of amorphous carbon. In addition, amorphous carbon particles or flaky impurities are also removed during the calcination process, exposing more surface area, so that the peak area ratio of the G peak to the D peak (GD ratio) in the Raman test is greater than 90. Next, in order to remove the iron oxide impurities formed during the air calcination process, the crude product is calcined for another 1-2 hours at a temperature of 1400-1600°C with carbon dioxide (CO) at a flow rate of 1000-1200sccm. At this time, iron oxide reacts with carbon monoxide to generate metallic iron (Fe) and carbon dioxide (CO2), and the generated carbon dioxide can be recycled in the purification process of single-walled carbon nanotubes. Then, the crude product is placed in a 3-6M hydrochloric acid (HCl) or sulfuric acid (H2SO4) solution and stirred at 60-80°C for 5-10 hours. This process can effectively remove iron (Fe), while iron oxide (FeO2 or Fe2O3) is not easily soluble in hydrochloric acid due to its high stability, and the reaction rate is slow, which affects the efficiency of metal impurity removal. However, through the previous carbon monoxide reduction step, the iron oxide is converted into elemental iron, which greatly improves the effect and speed of metal removal in the subsequent pickling process.
[0053] In one embodiment of the present application, a composite dispersion of single-walled carbon nanotubes is proposed, including a carbon source in a mixed solvent formed by mixing toluene and ethanol in a certain proportion, a metal compound catalyst, a co-catalyst and an etchant to form a dispersion.
[0054] The traditional floating catalytic method for preparing single-walled carbon nanotubes is to mix gas and liquid and feed them simultaneously. However, the gas is easily expanded when heated and the airflow is not stable enough, which will cause the temperature of the feed port to change continuously, affecting the volatilization of the liquid and resulting in the undesirable consequences of low product yield and poor quality. In order to reduce the impact of the volatilization factor of the liquid, the present invention uses toluene, which has a higher solubility for metal compound solids, as a solvent to prepare single-walled carbon nanotubes by floating catalytic method.
[0055] Toluene, which has a higher solubility of metal compounds in solid form, can carry more catalysts into the reaction system, so the output can be greatly improved. The study found that there are benzene rings in toluene. During the experimental process of checking the Raman standard spectrum, it was found that the benzene rings provide a carbon source, which will lead to the production of carbon impurity graphite, resulting in a serious decrease in the average GD ratio of batch output products. Ethanol catalysts can produce fewer carbon impurities, but the production rate is relatively slow because the solubility of metal compounds in ethanol is relatively low, and ethanol can only carry less catalyst into the reaction system. Even if the dispersion prepared by ethanol solvent is injected into the tubular furnace at a rate approximately three times that of toluene solvent, the insufficient carbon source content of ethanol itself leads to a slower production rate, and the product is less per unit time. Therefore, the present application creatively uses the two in a compounded manner, and studies the effects of the compounding ratio and injection rate on the yield and product quality.
[0056] In some embodiments, the metal compound is one or more of ferric chloride, ferrocene, cobalt chloride, and cobaltocene; the co-catalyst is one or more of thiophenol, thiophene, and selenophene; and the etchant is one or more of water, ethylene glycol, and methanol.
[0057] In some embodiments, the metal compound, liquid carbon source, promoter and etchant are used in a ratio of 5-10 g: 60-180 mL: 2-5 mL: 10-15 mL.
[0058] Metal compounds have higher solubility in toluene solvent; toluene, which has higher solubility of metal compounds in solid form, can carry more catalysts into the reaction system, so the yield can be greatly increased. However, there are benzene rings in toluene. During the experimental process of checking the Raman standard spectrum, it was found that if too much toluene is added, too many benzene rings provide a carbon source, which will lead to the production of carbon impurity graphite, so the average GD ratio of batch output products will be seriously reduced. Ethanol catalysts can produce fewer carbon impurities, but the production rate is relatively slow because the solubility of metal compounds in ethanol is low, and ethanol can only carry a small amount of catalyst into the reaction system. If too much ethanol is added, the yield will drop significantly.
[0059] Adding too much co-catalyst will result in an excessively high sulfur content in the system, with the sulfur wrapping around the outside of the iron atom cluster, causing the catalyst to deactivate.
[0060] The G / D ratio of Raman spectrum has always been one of the important criteria for measuring the quality of single-walled carbon nanotube products. The higher the G / D ratio of Raman spectrum, the better the product quality of single-walled carbon nanotubes. Adding too little etchant will lead to a high content of amorphous carbon. Although adding too much etchant will etch more amorphous carbon and reduce the peak area of D peak in Raman spectrum, it will also etch more graphite carbon, so the intensity of its G peak will decrease more seriously, and the GD ratio will still be low.
[0061] In some embodiments, the ratio of toluene to ethanol is 3-5:1.
[0062] This ratio is used to improve production rate and quality, and other auxiliary means are to control the liquid feed rate. Normally, if the liquid feed rate is too fast, the product quality will deteriorate, and if the liquid feed rate is too slow, the output will be low. For any dispersion prepared with a liquid carbon source, an injection rate that is too fast can also cause the furnace tube to explode due to the rapid vaporization of the liquid. Among them, the injection rate of the feed liquid of the dispersion prepared with ethanol as the solvent is 120μL / min, and the injection rate of the dispersion prepared with toluene as the solvent is 40μL / min. After repeated experiments, the feed rate range of the dispersion prepared with a mixed solvent was 53.3-60μL / min.
[0063] In one embodiment of the present application, the present application proposes a method for preparing single-walled carbon nanotubes, comprising the following steps:
[0064] S1. Before feeding the dispersion liquid, the liquid needs to be continuously heated and stirred to ensure that it is evenly mixed;
[0065] S2, using methane as the reducing gas and argon as the protective gas, the two enter the gas mixing tank for preheating according to a flow ratio within a certain range;
[0066] S3, introducing the uniformly mixed dispersion into a high-temperature furnace at a certain injection speed, and collecting samples at regular intervals to obtain a crude product;
[0067] S4. Purify the crude product.
[0068] In some embodiments, the heating temperature in step S1 is controlled at 60°C-80°C.
[0069] Too low a temperature will slow down the dissolution of solids in the solvent, lead to insufficient solubility of metal compounds in the carbon source solvent, and result in low catalyst dispersion. Higher temperatures will lead to faster evaporation of the solvent, increase the volatility of the liquid carbon source, and may lead to safety hazards, especially in poorly ventilated conditions.
[0070] In some embodiments, in step S2, the gas mixing tank is preheated to obtain a mixed gas with a temperature of 500-800° C. and a pressure of 0.1-0.3 MPa.
[0071] The system inside the furnace tube is in a state of slightly positive pressure, which increases the pressure inside the furnace body and promotes the rapid deposition of single-walled carbon nanotubes.
[0072] In some embodiments, the ratio of the reducing gas to the protective gas is 2000-5000:2500 sccm.
[0073] In some embodiments, the dispersion feed injection rate is 53.3-60 μL / min.
[0074] Too fast an injection rate will lead to a significant increase in production, while a slower injection rate will improve the stability of the product Raman value. At the same time, a faster liquid feed rate is often accompanied by a larger gas flow rate.
[0075] In some embodiments, the temperature of the furnace tube of the high temperature furnace in step S3 is 1150-1250°C.
[0076] According to the iron-carbon alloy phase diagram, the maximum solubility of carbon in austenite is about 2.11% when the temperature is maintained at 1148°C. (Austenite is the interstitial solid solution of C in γ-Fe, with a solubility from 0 to 2.11%. At 912°C on the phase diagram, pure iron undergoes an allotropic transformation from α-Fe to γ-Fe, called the A3 transformation, and from a body-centered cubic structure to a face-centered cubic structure.) However, in actual experiments, it was found that a higher temperature is often required to significantly increase the yield of single-walled carbon nanotubes. At 1180°C, the yield using the same formula is twice that at 1150°C. By experimentally obtaining 1200-1250°C, more single-walled carbon nanotubes will be produced.
[0077] In some embodiments, the purification process includes: S41. calcining the crude product in oxygen for a period of time; S42. adding a certain concentration of carbon dioxide in a horizontal tube furnace and further reacting under high temperature conditions; S43. stirring with a certain concentration of acid at a certain temperature for a period of time to obtain a pure powder product.
[0078] In some embodiments, the step S41 is performed by air calcination at 1400-1600°C.
[0079] In this temperature range, calcination can effectively remove some organic and metal impurities on the surface of carbon nanotubes; it helps to improve the mechanical properties of carbon nanotubes because high temperature can promote the arrangement and structural optimization of carbon nanotubes. The calcination process can also increase the conductivity of carbon nanotubes.
[0080] Too high a temperature may cause damage to the carbon nanotube structure. Thermal decomposition at high temperatures may destroy the tubular structure of carbon nanotubes, leading to degradation of the carbon nanotube morphology. It may cause more defects to form on the surface of carbon nanotubes, thereby reducing their electrical and mechanical properties. High temperatures may also cause agglomeration between carbon nanotubes, affecting their dispersibility and application performance.
[0081] If the temperature is too low, surface impurities and catalysts may not be completely removed, affecting the purity of carbon nanotubes. If the temperature is too low, the morphology of carbon nanotubes may be poorly developed, such as uneven tube diameter or more defects. Calcination time at low temperature may take longer, resulting in increased costs and reduced production efficiency.
[0082] In some embodiments, in step S42, calcination is continued at 1400-1600° C. by introducing 1000-1200 sccm of carbon dioxide (CO 2 ) for 1-2 hours.
[0083] If too little carbon dioxide is added, the iron oxide impurities will not be fully removed, and it will be more difficult to remove the iron oxide in the subsequent pickling process. Iron oxide impurities are more stable than metal impurities and are not easy to remove by reaction with acid. If too much carbon dioxide is added, it will lead to cost waste and environmental pollution caused by greenhouse gas emissions.
[0084] In some embodiments, in step S41, the heating rate is 8°C / min, the gas flow rate of oxygen introduced is about 200-400sccm, and the air oxidation time is 1-2h.
[0085] A heating rate that is too slow will shorten the production time and greatly affect the progress of industrial mass production. A heating rate that is too fast will cause the temperature inside the furnace to be unstable, fluctuating, affecting the output and deposition of the product.
[0086] Too high an oxygen content may reduce the thermal stability of carbon nanotubes, making them susceptible to oxidation reactions in high temperature environments, thereby reducing the stability and durability of their structure. It may also accelerate the corrosion of graphite carbon in carbon nanotubes, resulting in poor product quality. Too low an oxygen content may make it impossible to effectively purify carbon nanotubes, and residual impurities may affect their performance and applications. Too low an oxygen content may result in insufficient removal of amorphous carbon in carbon nanotubes.
[0087] In some embodiments, the acid in step S43 is 3-6 M concentrated hydrochloric acid or concentrated sulfuric acid, and the heating and stirring are continued at 60-80° C. for 5-10 h.
[0088] Too high agitation temperature may cause the pickling solution to evaporate faster, which may increase the acid concentration and cause excessive corrosion to the treated material.
[0089] Too low agitation temperature may cause the pickling reaction rate to be too slow, prolong the processing time, increase costs and resource consumption. It may make it difficult for the substance to fully contact with the processing solution in a low temperature environment, affecting the purification effect.
[0090] Example
[0091] Hereinafter, the embodiments of the present application will be described. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific techniques or conditions are indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be obtained commercially.
[0092] Embodiment 1:
[0093] First, 3g of metal compound, 180mL of liquid carbon source (wherein the ratio of toluene to ethanol is 3:1), 5mL of co-catalyst and 1.5mL of etchant are sequentially mixed. Next, 8000sccm of methane reducing gas and 2500sccm of nitrogen protective gas are injected into the mixing tank for heating to achieve the ideal temperature and pressure of 500-800℃ and 0.1-0.3MPa. Then, the outlet valve of the mixing tank is opened to allow the mixed gas to enter the furnace tube, and the dispersion is introduced into a 1250℃ high-temperature furnace at a flow rate of 60μL / min, and samples are taken every 30min.
[0094] Subsequently, the crude product was calcined at 1400°C for 2 hours with oxygen at a flow rate of 400 sccm to remove surface amorphous carbon and improve the degree of graphitization of the product. The crude product was then calcined at 1400°C for 2 hours with carbon dioxide (CO2) at a flow rate of 1200 sccm to remove iron oxide impurities. The crude product was then placed in a 6M hydrochloric acid (HCl) solution and stirred at 60°C for 8 hours to remove iron (Fe).
[0095] After weighing and Raman testing, it was found that the embodiment 1 solution 6h could produce 7.2021g of single-walled net product, and the Raman G / D was as high as 162.4.
[0096] Embodiment 2:
[0097] First, 3g of metal compound, 180mL of liquid carbon source (where the ratio of toluene to ethanol is 4:1), 5mL of co-catalyst and 1.5mL of etchant are sequentially mixed. Next, 8000sccm of methane reducing gas and 2500sccm of nitrogen protective gas are injected into the mixing tank for heating to achieve the ideal temperature and pressure of 500-800℃ and 0.1-0.3MPa. Then, the outlet valve of the mixing tank is opened to allow the mixed gas to enter the furnace tube, and the dispersion is introduced into a 1250℃ high-temperature furnace at a flow rate of 56μL / min, and samples are taken every 30min.
[0098] Subsequently, the crude product was calcined at 1400°C for 2 hours with oxygen at a flow rate of 400 sccm to remove surface amorphous carbon and improve the degree of graphitization of the product. The crude product was then calcined at 1400°C for 2 hours with carbon dioxide (CO2) at a flow rate of 1200 sccm to remove iron oxide impurities. The crude product was then placed in a 6M hydrochloric acid (HCl) solution and stirred at 60°C for 8 hours to remove iron (Fe).
[0099] After weighing and Raman testing, it was found that the embodiment 1 solution 6h could produce 8.6458g of single-walled net product, and the Raman G / D was as high as 134.2.
[0100] Embodiment 3:
[0101] First, 3g of metal compound, 180mL of liquid carbon source (wherein the ratio of toluene to ethanol is 5:1), 5mL of co-catalyst and 1.5mL of etchant are sequentially mixed. Next, 8000sccm of methane reducing gas and 2500sccm of nitrogen protective gas are injected into the mixing tank for heating to achieve the ideal temperature and pressure of 500-800℃ and 0.1-0.3MPa. Then, the outlet valve of the mixing tank is opened to allow the mixed gas to enter the furnace tube, and the dispersion is introduced into a 1250℃ high-temperature furnace at a flow rate of 53.3μL / min, and samples are taken every 30min.
[0102] Subsequently, the crude product was calcined at 1400°C for 2 hours with oxygen at a flow rate of 400 sccm to remove surface amorphous carbon and improve the degree of graphitization of the product. The crude product was then calcined at 1400°C for 2 hours with carbon dioxide (CO2) at a flow rate of 1200 sccm to remove iron oxide impurities. The crude product was then placed in a 6M hydrochloric acid (HCl) solution and stirred at 60°C for 8 hours to remove iron (Fe).
[0103] After weighing and Raman testing, it was found that the comparative example 1 solution could produce 10.0865g of single-walled net product in 6 hours, and the Raman G / D was 129.1.
[0104] Comparative Example 1:
[0105] The scheme of Comparative Example 1 is the same as the method of Example 1, except that the liquid carbon source is pure toluene and the injection rate of the dispersion is 40 μL / min.
[0106] After weighing and Raman testing, it was found that the comparative example 1 solution could produce 11.5320g of single-walled net product in 6 hours, and the Raman G / D was 85.6.
[0107] Comparative Example 2:
[0108] The scheme of Comparative Example 2 is the same as that of Example 1, except that the liquid carbon source is pure ethanol and the injection rate of the dispersion is 120 μL / min.
[0109] After weighing and Raman testing, it was found that the comparative example 2 solution could produce 5.7721g of single-walled net product in 6h, and the Raman G / D was 121.3.
[0110] Comparative Example 3:
[0111] The scheme of Comparative Example 2 is the same as the method of Example 1, except that the liquid carbon source is 180 mL of liquid carbon source, wherein the ratio of toluene to ethanol is 2:1, and the injection rate of the dispersion is 66.4 μL / min.
[0112] After weighing and Raman testing, it was found that the comparative example 2 solution could produce 7.011g of single-walled net product in 6 hours, and the Raman G / D was 146.8.
[0113] Comparative Example 4:
[0114] The scheme of Comparative Example 2 is the same as the method of Example 1, except that the liquid carbon source is 180 mL of liquid carbon source, wherein the ratio of toluene to ethanol is 6:1, and the injection rate of the dispersion is 51.4 μL / min.
[0115] After weighing and Raman testing, it was found that the comparative example 2 solution could produce 7.198g of single-walled net product in 6 hours, and the Raman G / D was 90.1.
[0116] However, from the scanning electron micrograph of the pure single-walled carbon nanotubes, it can be observed that the carbon nanotubes prepared from pure toluene are slightly more than those prepared from ethanol. This may be because during the reaction, the carbon source provided by the aromatic ring produces more carbon impurities that do not form single-walled carbon nanotubes.
[0117] By comparing Example 1, Example 2 and Example 3, it can be observed that the production rate of single-walled carbon nanotubes in Example 1 is significantly greater than that in Example 2 and Example 3. As the content of benzyl alcohol increases, the color of the carbon tubes in the scanning electron microscope image gradually darkens, which may be due to the difficulty in removing a small amount of carbon impurities after benzyl alcohol provides a carbon source. The GD ratio between Example 1, Example 2 and Example 3 shows a gradually decreasing trend. This may be due to the fact that during the reaction, the carbon source provided by the aromatic ring produces more carbon impurities that generate non-single-walled carbon nanotubes, which gradually reduces the degree of graphitization of the product. However, from the perspective of output, there is a gradually increasing trend between Example 1, Example 2 and Example 3. This may be due to the high carbon content of toluene, and the carbon utilization rate of preparing single-walled carbon nanotubes is also high, so the rate of producing single-walled carbon nanotubes is faster. However, if the toluene content in the solvent is too high, it will also cause some carbon impurities produced by it to be difficult to remove. Therefore, among the above-mentioned many examples, Example 2 is more suitable as an alternative for industrial mass production.
[0118] Comparative Example 1 is to prepare single-walled carbon nanotubes using pure toluene as the liquid carbon source. Although the output is faster than that of ethanol solvent, the GD ratio is not good. It can be observed from the scanning electron microscope that after the purification of this method, a small amount of carbon impurities are still difficult to remove. Comparative Example 2 is to prepare single-walled carbon nanotubes using pure ethanol as the liquid carbon source. Although the output is higher than the GD of toluene solvent, its output rate is too slow. Ethanol has a low carbon content and a lower carbon utilization rate in the process of preparing single-walled carbon nanotubes. Although high-quality output of single-walled carbon nanotubes can be achieved, the current output of this solution is not high and it is difficult to achieve industrial mass production. Therefore, the present invention combines the advantages of preparing single-walled carbon nanotubes with two solvents, mixes the two as a carbon source solvent, and significantly improves the output and quality of single-walled carbon nanotubes.
[0119] Although the GD ratio in Comparative Example 3 is better, its output is lower than that in Example 1. This shows that adding too little benzyl alcohol affects the output of single-walled carbon nanotubes per unit time. In Comparative Example 4, although more crude products are obtained by adding too much benzyl alcohol, it may be because more carbon impurities are generated after benzyl alcohol provides a carbon source. Therefore, after purification, the output of the single-walled carbon nanotube net product in Comparative Example 4 is not only not increased, but also decreased. In addition, the carbon impurities generated by excessive benzyl alcohol as a carbon source, according to the purification method practice of the present invention, the experimental effect obtained is worse than that of Example 1, which is also one of the reasons why the GD ratio of the single-walled carbon nanotube net product output by this method is not high.
[0120] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.
Claims
1. A composite dispersion of single-walled carbon nanotubes, characterized in that: The invention comprises a carbon source of a mixed solvent formed by mixing toluene and ethanol in a certain proportion, a metal compound catalyst, a co-catalyst and an etchant to form a dispersion.
2. The composite dispersion of single-walled carbon nanotubes according to claim 1, characterized in that: The metal compound is one or more of ferric chloride, ferrocene, cobalt chloride, and cobaltocene; the cocatalyst is one or more of thiophenol, thiophene, and selenophene; and the etchant is one or more of water, ethylene glycol, and methanol.
3. A composite dispersion of single-walled carbon nanotubes according to claim 1 or 2, characterized in that: The usage ratio of the metal compound, liquid carbon source, co-catalyst and etchant is 5-10g:60-180mL:2-5mL:10-15mL; the ratio of toluene to ethanol is 3-5:
1.
4. A method for preparing single-walled carbon nanotubes, comprising the following steps: S1. Before feeding the dispersion liquid, the liquid needs to be continuously heated and stirred to ensure that it is evenly mixed; S2, using methane as the reducing gas and argon as the protective gas, the two enter the gas mixing tank for preheating according to a flow ratio within a certain range; S3, introducing the uniformly mixed dispersion into a high-temperature furnace at a certain injection speed, and collecting samples at regular intervals to obtain a crude product; S4. Purify the crude product.
5. The method for preparing single-walled carbon nanotubes according to claim 4, characterized in that: In step S2, the gas mixing tank is preheated to obtain a mixed gas with a temperature of 500-800° C. and a pressure of 0.1-0.3 MPa.
6. The method for preparing single-walled carbon nanotubes according to claim 4, characterized in that: The dispersion feed injection speed is 53.3-60 μL / min.
7. The method for preparing single-walled carbon nanotubes according to claim 4, characterized in that: In step S3, the temperature of the furnace tube of the high temperature furnace is 1150-1250°C.
8. The method for preparing single-walled carbon nanotubes according to claim 4, characterized in that: The purification process includes: S41. calcining the crude product in oxygen for a period of time; S42. adding a certain concentration of carbon dioxide in a horizontal tube furnace and further reacting under high temperature conditions; S43. stirring with a certain concentration of acid at a certain temperature for a period of time to obtain a pure powder product.
9. The method for preparing single-walled carbon nanotubes according to claim 8, characterized in that: In the step S41, air calcination is performed at 1400-1600°C; in the step S41, the heating rate is 8°C / min, the gas flow rate of oxygen introduced is about 200-400sccm, and the air oxidation time is 1-2h.
10. The method for preparing single-walled carbon nanotubes according to claim 8, characterized in that: In the step S42, 1000-1200 sccm of carbon dioxide (CO2) is continuously introduced at 1400-1600° C. for calcination for 1-2 hours.