Preparation method of biomass N, P and S multi-element doped graphitized carbon material

By using ferrocene formic acid grafting and humic acid doping methods in lead-carbon batteries, N, P, S multi-doped graphitized carbon materials were prepared, which solved the poor conductivity of biomass carbon materials and the rapid hydrogen evolution reaction. The problem is that the conductivity and charge and discharge stability of lead-carbon batteries are improved, and the cycle life of the batteries is extended.

CN118894526AActive Publication Date: 2024-11-05FUJIAN XINSEN CARBON

Patent Information

Application Number
CN202410929205.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-05
Estimated Expiration
2044-07-11

AI Technical Summary

Technical Problem

Biomass carbon materials have poor electrical conductivity in lead-carbon batteries, resulting in unstable charging and discharging performance, and excessively fast hydrogen evolution reaction, affecting battery life.

Method used

The alkali-activated biomass powder was grafted using ferrocene formic acid as a grafting agent, and carbonized and graphitized in an inert atmosphere by combining humic acid, organic resin microspheres, and phosphoric acid to prepare N, P, S multi-compartment doping The graphitized carbon material improves conductivity and charge and discharge stability, and inhibits hydrogen evolution reaction.

Benefits of technology

It significantly improves the conductivity and charge and discharge stability of carbon materials, extends the polarization potential of hydrogen evolution reaction, and enhances the cycle life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118894526A_ABST
    Figure CN118894526A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a biomass N, P and S multi-element doped graphitized carbon material, which comprises the following steps: 1) under an ice bath condition, uniformly mixing ferrocenecarboxylic acid, an organic solvent, 4-dimethylaminopyridine (DMAP) and alkali activated biomass powder, dropwise adding a dicyclohexylcarbodiimide (DCC) solution, reacting under a stirring condition after dropwise adding, filtering and washing after the reaction is finished, and drying to obtain an N, P and S multi-element doped graphitized carbon material; drying to obtain modified biomass powder; 2) uniformly mixing the modified biomass powder, humic acid, organic resin microspheres and alkali liquor, and performing first drying, carbonization, cooling, rinsing, second drying, graphitization, cooling, acid pickling, water washing and third drying to obtain the biomass graphitized carbon material. And the lead-carbon battery can obtain cycle life and hydrogen evolution inhibition effect when being applied to the lead-carbon battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of biomass graphitized carbon materials, and specifically relates to a method for preparing a biomass N, P, S multi-component doped graphitized carbon material. Background Art

[0002] Lead-carbon battery is a capacitor-type lead-acid battery, which is a technology evolved from traditional lead-acid batteries. It is a battery that combines lead and carbon materials at the negative electrode of the lead-acid battery. It has a long cycle life under partial state of charge and high-rate charge and discharge conditions, and shows good application prospects in energy storage and hybrid vehicles. Lead-carbon batteries are divided into internal parallel type and internal mixed type according to the form of the negative electrode. The internal parallel type is to connect the lead negative electrode and the carbon negative electrode in a certain form in parallel, and then combine them with the PbO2 positive electrode plate to form a battery cell; the internal mixed type is to add carbon material as an additive to the negative electrode lead paste in a certain mass fraction or manner, and produce lead-carbon negative electrode plates according to conventional manufacturing processes. Considering the cost and process operability, the internal mixed type has received more widespread attention.

[0003] Carbon materials for lead-carbon batteries include high-purity graphite, high-surface-area activated carbon, carbon nanotubes, acetylene black, graphene, etc., and their mechanisms of action are believed to mainly include the following: conductive mechanism, steric mechanism, balanced charging mechanism, and capacitance mechanism. The main raw materials for preparing carbon materials include coal, petroleum, and petroleum derivatives. With the continuous transformation and utilization of the natural environment by humans, as well as social progress and economic development, the world is facing a serious energy crisis. Since biomass carbon materials are widely available and belong to renewable resources, the use of biomass to prepare carbon materials for lead-carbon batteries is a current research hotspot. For example, the biomass porous carbon material and its preparation method and its application in lead-acid batteries disclosed in patent CN115367750B, the modified carbon material, its preparation method, negative lead paste, plate, and lead-carbon battery disclosed in patent CN105958076B.

[0004] Biomass carbon materials are also often used as additives in the form of internal mixing, which can not only slow down the accumulation and growth of lead sulfate crystals and inhibit the irreversible sulfation of the negative electrode, but also reduce the hydrogen evolution overpotential caused by the addition of carbon materials and delay the hydrogen evolution reaction of the negative electrode plate through the above-mentioned technologies such as removing lignin or doping with high hydrogen evolution overpotential metal salts. However, compared with petroleum-based and coal-based carbon materials, biomass carbon materials come from biomass, such as straw and wood. These materials have complex chemical structures, cell structures and diverse chemical compositions, resulting in poor conductivity of carbon materials prepared from biomass, and more unstable charge and discharge performance of lead-carbon batteries.

[0005] Therefore, it is necessary to use biomass to develop a carbon material that can slow down the accumulation and growth of lead sulfate crystals, inhibit the hydrogen evolution reaction, and also has excellent conductivity and charge and discharge stability. Summary of the invention

[0006] In order to solve the above technical problems, the present invention provides a method for preparing a biomass graphitized carbon material. First, ferrocenecarboxylic acid is used as a grafting agent to graft alkali-activated biomass powder to obtain a modified biomass powder uniformly grafted with ferrocenecarboxylic acid. Then, the modified biomass powder, humic acid, organic resin microspheres, and phosphoric acid are used as raw materials to carry out carbonization, graphitization and other reactions under an inert atmosphere to prepare a N, P, and S multi-doped graphitized carbon material. On the one hand, the iron in the grafting agent can improve the graphitization degree of the carbon material, increase its pore volume, develop its pore structure, reduce the total amount of oxygen-containing functional groups, make the structure more solid, and further improve its conductivity and charge and discharge stability. On the other hand, the N, P, and S doped in the graphitized carbon material help to shift the polarization potential of the hydrogen evolution reaction negatively, thereby inhibiting hydrogen evolution.

[0007] In order to achieve the above purpose, the following technical solutions are adopted:

[0008] A method for preparing a biomass N, P, S multi-element doped graphitized carbon material comprises the following steps:

[0009] 1) Under ice bath conditions, ferrocenecarboxylic acid, an organic solvent, 4-dimethylaminopyridine (DMAP), and alkali-activated biomass powder are mixed evenly, and a dicyclohexylcarbodiimide (DCC) solution is added dropwise, and the mixture is reacted under stirring conditions. After the reaction is completed, the mixture is filtered, washed, and dried to obtain a modified biomass powder;

[0010] 2) The modified biomass powder, humic acid, organic resin microspheres and alkali solution are uniformly mixed, dried for the first time, carbonized, cooled, rinsed, dried for the second time, graphitized, cooled, acid washed, washed with water, and dried for the third time to obtain a biomass graphitized carbon material.

[0011] Furthermore, the preparation method of the alkali-activated biomass powder in step 1) is not particularly limited and can be any commonly used method in the art. Specifically, the dry biomass is crushed into particles, washed, and dried to obtain biomass powder, the biomass powder and alkali solution are added to a reactor, the temperature is increased to react, and after the reaction is completed, the reaction is cooled to room temperature, filtered, washed, and dried to obtain alkali-activated biomass powder.

[0012] Furthermore, the biomass is selected from one or a combination of two or more of rice husks, coconut shells, wood chips, bamboo, rice straw, corn cobs, walnut shells, bagasse, and pistachio shells; the average particle size of the particles is 1-3 mm, the washing is washing with water 1-3 times, and the drying is vacuum drying at 80-100° C. to constant weight.

[0013] Furthermore, the concentration of the alkali solution is 0.5-0.8 mol / L, and the alkali solution is selected from one or a combination of sodium hydroxide solution and potassium hydroxide solution; the mass volume ratio of the biomass powder and the alkali solution is 1g: (15-20) mL, the temperature is raised to 180-200°C, the reaction time is 1-3h, the washing is washed with water to neutrality, and the drying is vacuum drying at 100-120°C to constant weight. The purpose of the alkali activation step is to increase the reactivity of the hydroxyl groups on the biomass powder.

[0014] Step 1) The organic solvent is selected from one or a combination of two or more of dichloromethane, benzene and toluene. The amount of ferrocenecarboxylic acid is 5-8wt% of the alkali-activated biomass powder, the alkali-activated biomass powder is 5-10wt% of the organic solvent, the molar ratio of ferrocenecarboxylic acid, DMAP and DCC is 4-5:4-5:4-5, the concentration of the DCC solution is 0.4-0.6mol / L, and the solvent of the DCC solution is the same as the above organic solvent. The dropping time is 0.5-1.5h, the reaction temperature is 20-30°C, and the reaction time is 12-24h. The washing is washed alternately with saturated sodium bicarbonate solution and water for 1-3 times, and the drying is dried at 60-90°C to constant weight. Step 1) In the presence of DCC as a dehydrating agent and DMAP as a catalyst, ferrocenecarboxylic acid is used as a grafting agent to graft the alkali-activated biomass powder to obtain a modified biomass powder uniformly grafted with ferrocenecarboxylic acid. Iron has a catalytic effect and can increase the graphitization degree of the carbon material, increase its pore volume, develop the pore structure, reduce the total amount of oxygen-containing functional groups, make the structure more solid, and further improve the conductivity and charge and discharge stability.

[0015] Step 2) The organic resin microspheres are selected from one or a combination of polystyrene microspheres and polytetrafluoroethylene microspheres, and the average particle size of the organic resin microspheres is 100-500 μm. The modified biomass powder and the organic resin microspheres both shrink in volume during the carbonization step, but the shrinkage rates are different, forming pores; the alkali solution concentration is 40-50wt%, and the alkali solution is selected from one or a combination of sodium hydroxide and potassium hydroxide.

[0016] Step 2) The mass ratio of the modified biomass powder, humic acid, organic resin microspheres, and alkali solution is 80-90:10-15:30-35:150-180. Humic acid is a macromolecular organic substance widely present in nature and is widely used in agriculture, forestry, animal husbandry, petroleum, chemical industry, building materials, medicine and health, environmental protection and other fields. Humic acid is a type of organic substance formed and accumulated by the decomposition and transformation of animal and plant remains, mainly plant remains, and a series of geochemical processes. The elements that make up humic acid are carbon, hydrogen, oxygen, nitrogen, sulfur and a small amount of phosphorus. Humic acid is mixed with modified biomass powder and the like to undergo carbonization, graphitization and other reactions to prepare N, P, S-doped graphitized carbon materials, which helps to shift the polarization potential of the hydrogen evolution reaction negatively and inhibit hydrogen evolution. The inventors found that humic acid and modified biomass powder have a synergistic effect in inhibiting hydrogen evolution. The ratio of the two should not be too high or too low. Too high or too low is not conducive to inhibiting hydrogen evolution. It is speculated that the graphitization caused by the grafting agent and the above-mentioned heteroatoms will change the surface chemical properties of the carbon material. Too high or too low a ratio is conducive to H evolution. + adsorption and reaction.

[0017] Step 2) The first drying is drying at 150-180°C to constant weight. The carbonization is heating carbonization at 450-600°C for 2-3h. The cooling is natural cooling to room temperature. The rinsing is rinsing with water to recover the alkali solution. The second drying is drying at 120-150°C to constant weight. The graphitization is reacted for 4-8h in an inert gas atmosphere at a temperature of 1750-1900°C. The acid washing is rinsing the graphitized product 1-5 times with a concentration of 0.1-0.5mol / L dilute hydrochloric acid, and the water washing is rinsing the product after acid washing 1-5 times; the third drying temperature is 95-105°C to constant weight. Acid washing is to remove iron to prevent iron from having adverse effects on the final carbon material, and can also produce more porous structures.

[0018] The present invention also provides a biomass N, P, S multi-doped graphitized carbon material prepared by the above method. Preferably, the biomass N, P, S multi-doped graphitized carbon material has a graphitization degree of I D / I G Between 0.50-0.61.

[0019] The present invention also provides a negative electrode lead paste for a lead-carbon battery, using the biomass N, P, S multi-component doped graphitized carbon material as a negative electrode lead paste additive.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] The invention firstly uses ferrocenecarboxylic acid as a grafting agent to graft alkali-activated biomass powder to obtain modified biomass powder uniformly grafted with ferrocenecarboxylic acid, and then uses the modified biomass powder, humic acid, organic resin microspheres and phosphoric acid as raw materials to carry out carbonization, graphitization and other reactions under an inert atmosphere to prepare N, P and S doped graphitized carbon material; on the one hand, the iron in the grafting agent can improve the graphitization degree of the carbon material, increase the pore volume, develop the pore structure, reduce the total amount of oxygen-containing functional groups, make the structure more solid, and further improve the conductivity and charge and discharge stability; on the other hand, the N, P and S doped in the graphitized carbon material are helpful to negatively shift the polarization potential of the hydrogen evolution reaction, so that hydrogen evolution is inhibited.

[0022] The inventors found that humic acid and modified biomass powder have a synergistic effect in inhibiting hydrogen evolution. It is speculated that the graphitization caused by the grafting agent and the doped heteroatoms will change the surface chemical properties of the carbon material. By adjusting the ratio of the two, H evolution can be inhibited. + adsorption and reaction. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is an electron microscope photo of the biomass graphitized carbon material prepared in Example 1;

[0024] Figure 2 This is a graph showing the specific surface area test data of the biomass graphitized carbon material prepared in Example 1;

[0025] Figure 3 This is the pore size distribution diagram of the specific surface area test of the biomass graphitized carbon material prepared in Example 1. DETAILED DESCRIPTION

[0026] The present invention will be further described below in conjunction with specific embodiments, but is not limited to the contents of the specification. Unless otherwise specified, the "parts" described in the embodiments of the present invention are all parts by weight. The reagents used are all commercially available reagents in the art.

[0027] The average particle size of polystyrene microspheres was 200 μm and they were purchased from Shanghai Yiyuan Biotechnology Co., Ltd.

[0028] Example 1

[0029] 1) 200 g of dried coconut shell was crushed into particles with an average particle size of 2.5 mm, washed twice with water, and dried at 90° C. to constant weight to obtain 200 g of biomass powder. 200 g of biomass powder and 4 L of 0.5 mol / L sodium hydroxide solution were added to a reactor, heated to 200° C. for reaction for 2 h, cooled to room temperature after the reaction, filtered, washed with water until the pH was neutral, and dried at 90° C. to constant weight to obtain alkali-activated biomass powder;

[0030] 2) Under ice bath conditions, 0.04 mol of ferrocenecarboxylic acid, 1150 g of dichloromethane, 0.04 mol of 4-dimethylaminopyridine (DMAP), and 115 g of alkali-activated biomass powder were mixed evenly, and 0.1 L of 0.5 mol / L dicyclohexylcarbodiimide (DCC) solution (solvent dichloromethane) was added dropwise for 1 h. The mixture was stirred at 25 ° C for 15 h. After the reaction was completed, the mixture was filtered, washed alternately with saturated sodium bicarbonate solution and water for 3 times, and dried at 90 ° C to constant weight to obtain modified biomass powder;

[0031] 3) 90 g of modified biomass powder, 10 g of humic acid, 35 g of polystyrene microspheres, and 180 g of 50 wt% sodium hydroxide solution were mixed evenly, dried at 150 ° C for the first time for 18 h to constant weight, carbonized at 600 ° C for 2 h, cooled naturally to room temperature, rinsed with water to remove the alkali solution, dried at 150 ° C for the second time to constant weight, graphitized at 1800 ° C for 6 h under argon atmosphere, cooled naturally to room temperature, rinsed the graphitized product 3 times with 0.3 mol / L dilute hydrochloric acid, and then rinsed with water 3 times, dried at 150 ° C for the third time to constant weight to obtain a biomass graphitized carbon material.

[0032] Example 2

[0033] The rest is the same as Example 1, except that in step 2), the amount of alkali-activated biomass powder used is 184 g, and the amount of dichloromethane used is 1840 g.

[0034] Example 3

[0035] The rest is the same as Example 1, except that the amount of modified biomass powder used in step 3) is 80 g.

[0036] Example 4

[0037] The rest is the same as Example 1, except that the amount of modified biomass powder used in step 3) is 70 g.

[0038] Example 5

[0039] The rest is the same as Example 1, except that the amount of modified biomass powder used in step 3) is 100 g.

[0040] Example 6

[0041] The rest is the same as Example 1, except that 3) 80g of modified biomass powder, 15g of humic acid, 30g of polystyrene microspheres, and 150g of 50wt% sodium hydroxide solution are mixed evenly, dried for the first time at 150°C for 18h to constant weight, carbonized at 600°C for 2h, naturally cooled to room temperature, rinsed with water to remove the alkali solution, dried for the second time at 150°C to constant weight, graphitized at 1800°C under argon atmosphere for 6h, naturally cooled to room temperature, the graphitized product is rinsed 3 times with 0.3mol / L dilute hydrochloric acid, then rinsed 3 times with water, dried for the third time at 150°C to constant weight to obtain a biomass graphitized carbon material.

[0042] Comparative Example 1

[0043] The rest is the same as Example 1, except that humic acid is not added in step 3).

[0044] Comparative Example 2

[0045] 1) 200 g of dried coconut shell was crushed into particles with an average particle size of 2.5 mm, washed twice with water, and dried at 90° C. to constant weight to obtain 200 g of biomass powder. 200 g of biomass powder and 4 L of 0.5 mol / L sodium hydroxide solution were added to a reactor, heated to 200° C. for reaction for 2 h, cooled to room temperature after the reaction, filtered, washed with water until the pH was neutral, and dried at 90° C. to constant weight to obtain alkali-activated biomass powder;

[0046] 2) 90g alkali-activated biomass powder, 10g humic acid, 35g polystyrene microspheres, and 180g 50wt% sodium hydroxide solution were mixed evenly, dried at 150°C for the first time for 18h to constant weight, carbonized at 600°C for 2h, cooled naturally to room temperature, rinsed with water to remove the alkali solution, dried for the second time at 150°C to constant weight, graphitized at 1800°C under argon atmosphere for 6h, cooled naturally to room temperature, rinsed the graphitized product 3 times with 0.3mol / L dilute hydrochloric acid, then rinsed with water 3 times, dried for the third time at 150°C to constant weight to obtain a biomass graphitized carbon material.

[0047] Comparative Example 3

[0048] The rest is the same as Example 1, except that ferrocenecarboxylic acid is added in the form of a blend:

[0049] 1) 200 g of dried coconut shell was crushed into particles with an average particle size of 2.5 mm, washed twice with water, and dried at 90° C. to constant weight to obtain 200 g of biomass powder. 200 g of biomass powder and 4 L of 0.5 mol / L sodium hydroxide solution were added to a reactor, heated to 200° C. for reaction for 2 h, cooled to room temperature after the reaction, filtered, washed with water until the pH was neutral, and dried at 90° C. to constant weight to obtain alkali-activated biomass powder;

[0050] 2) 90g alkali-activated biomass powder, 7.2g ferrocenecarboxylic acid, 10g humic acid, 35g polystyrene microspheres, and 180g 50wt% sodium hydroxide solution were mixed evenly, dried at 150°C for the first time for 18h to constant weight, carbonized at 600°C for 2h, cooled naturally to room temperature, rinsed with water to remove the alkali solution, dried at 150°C for the second time to constant weight, graphitized at 1800°C under argon atmosphere for 6h, cooled naturally to room temperature, rinsed the graphitized product 3 times with 0.3mol / L dilute hydrochloric acid, then rinsed with water 3 times, dried at 150°C for the third time to constant weight to obtain a biomass graphitized carbon material.

[0051] Application Example 1

[0052] A. Preparation of pole piece: Grind the biomass graphitized carbon material of Example 1: PVDF: acetylene black in a mortar at a mass ratio of 8:1:1, then add appropriate amount of N-methylpyrrolidone and ethanol to prepare a slurry, then evenly coat it on a 10 mm × 20 mm titanium foil, and vacuum dry it for 24 hours to obtain a pole piece.

[0053] B Assemble lead-carbon battery:

[0054] (1) Paste: 50 g of lead powder, 10 g of lead oxide, 0.7 g of the biomass graphitized carbon material prepared in Example 1, 0.8 g of barium sulfate, 0.2 g of acetylene black, 0.8 g of sodium lignosulfonate, 0.8 g of barium stearate, and 0.9 mL of water were stirred for 10 min to obtain a lead paste.

[0055] (2) Apply lead paste evenly to the positive and negative grids (the lead-calcium alloy negative grid was purchased from Baoding Meilun Nonferrous Metals Co., Ltd., and the lead dioxide positive grid was purchased from Baoji Changli Special Metals Co., Ltd. The size of the positive and negative grids is 70mm×50mm×2mm.), dry in an oven at 65℃ for 8h, and then dry at 75℃ for 6h to obtain the positive and negative plates of the lead-carbon battery. Add 150mL of 1.035g / cm 3 Sulfuric acid, insert the positive and negative plates on both sides of the beaker, separate them with industrial battery AGM, simulate lead-carbon battery, connect it to LAND5.8 battery test system, and perform formation to obtain qualified positive and negative plates. Among them, the formation conditions are: first stand for 2 hours, then charge at 0.05C constant current for 1 hour, then charge at 0.1C constant current for 20 hours; after standing for 2 hours, discharge at 0.1C constant current for 1 hour, then charge at 0.1C constant current for 10 hours, charge at 0.2C constant current for 12 hours, and finally charge at 0.1C constant current for 4 hours.

[0056] (3) Lead-carbon batteries are assembled in the form of 1 positive and 2 negative plates: welding of positive and negative plates, battery acid filling (sulfuric acid density 1.27g / cm 3), battery sealing, battery detection machine activation.

[0057] Application Example 2-6, Comparative Application Example 1-2

[0058] The rest is the same as Application Example 1, except that the biomass graphitized carbon material is prepared according to Example 2-6.

[0059] The biomass graphitized carbon materials prepared in the above examples and comparative examples were tested for specific surface area and resistivity. The pole pieces and lead-carbon batteries prepared in the application examples and comparative application examples were tested for the following other performances: For simplicity, the examples and application examples were tested with the same application example number, and the results are shown in Table 1.

[0060] 1. Specific surface area and pore size: measured by NOVA 1000e pore structure specific surface area tester. The sample was degassed at 350℃ for 2h, and liquid nitrogen was used as the adsorption medium at 77K and relative pressure (P / P0) 10 -6 N2 adsorption was carried out in the range of -1, and the specific surface area was calculated by BET equation.

[0061] 2. Hydrogen evolution performance: The electrode prepared as above was used as the working electrode, a saturated calomel electrode was used as the reference electrode, and a Pt sheet was used as the counter electrode. In a 1 mol / L sulfuric acid solution, a classic three-electrode system was used to perform a linear scanning test on the working electrode using the CHI660A electrochemical workstation of Shanghai Chenhua Instrument Co., Ltd. The scanning range was 0 to -2 V, and the scanning rate was 1 mV / s. The hydrogen evolution performance of the material can be determined based on the linear scanning voltammetric curve.

[0062] 3. Cycle performance: In order to study the charge and discharge voltage and cycle characteristics of the battery under the HRPSoC state, a cycle test experiment was carried out. The battery tester model used in the experiment is BTS-5V / 6A, produced by Shenzhen Xinwei Electronics Co., Ltd. The charge and discharge system used in the test is as follows: First, the battery is left for 30 minutes, discharged at a current of 2A for 84 minutes, reaching 50% of the theoretical capacity, that is, 50% SoC. After leaving it for 5 minutes, the following steps are cycled: 4A current charging for 1 minute, leaving it for 1 minute, 4A current discharging for 1 minute, and leaving it for 1 minute. The upper and lower limits of the charge and discharge voltage are set to 2.9V and 1.7V respectively. When any of the aforementioned cut-off voltages of the battery is reached, the cycle is terminated, and the number of cycles at the termination is recorded.

[0063] 4. Raman spectroscopy analysis: The degree of graphitization of biomass graphitized carbon materials is analyzed by testing the Raman spectrum of the materials, ranging from 500-3000cm -1 The main characteristic band of Raman spectrum of carbon-based materials is located at 1340cm -1 The D peaks at around 1570 cm -1 The G peaks on the left and right are caused by disordered carbon atoms and sp2 The symmetric stretching vibration of the hybrid carbon atoms is generated, and the intensity ratio of these two characteristic peaks is I D / I G The value can be used to evaluate the degree of graphitization. The smaller the value, the higher the corresponding degree of graphitization.

[0064] Table 1 Performance test

[0065]

[0066]

[0067] From the test results of graphitization degree in Table 1, it can be seen that the grafted ferrocenecarboxylic acid is beneficial to improve the graphitization degree of carbon materials, reduce resistivity and improve conductivity. From the test results of hydrogen evolution performance, it can be seen that humic acid and modified biomass powder have an obvious synergistic effect of inhibiting hydrogen evolution. It is speculated that the graphitization caused by the grafting agent and the doped heteroatoms will change the surface chemical properties of the carbon material. By adjusting the ratio of the two, the H evolution can be inhibited. + The adsorption and reaction of the battery are improved, the hydrogen evolution reaction is inhibited, the charge and discharge stability is improved, and the corresponding cycle life is increased.

[0068] The present invention adopts biomass as the carbon source for preparing carbon material, which not only saves cost but also helps to improve the performance of lead-carbon batteries.

Claims

1. A method for preparing biomass N, P, S multi-element doped graphitized carbon material, characterized in that: The steps include: 1) Under ice bath conditions, ferrocenecarboxylic acid, an organic solvent, 4-dimethylaminopyridine (DMAP), and alkali-activated biomass powder are mixed evenly, and a dicyclohexylcarbodiimide (DCC) solution is added dropwise, and the mixture is reacted under stirring conditions. After the reaction is completed, the mixture is filtered, washed, and dried to obtain a modified biomass powder; 2) The modified biomass powder, humic acid, organic resin microspheres and alkali solution are uniformly mixed, dried for the first time, carbonized, cooled, rinsed, dried for the second time, graphitized, cooled, acid washed, washed with water, and dried for the third time to obtain a biomass graphitized carbon material.

2. The preparation method according to claim 1, characterized in that: Step 1) The amount of ferrocenecarboxylic acid is 5-8wt% of the alkali-activated biomass powder, the alkali-activated biomass powder is 5-10wt% of the organic solvent, and the molar ratio of ferrocenecarboxylic acid, DMAP, and DCC is 4-5:4-5:4-5.

3. The preparation method according to claim 1, characterized in that: Step 1) The organic solvent is selected from one or a combination of two or more of dichloromethane, benzene and toluene; the concentration of the DCC solution is 0.4-0.6 mol / L, and the solvent of the DCC solution is the same as the above organic solvent.

4. The preparation method according to claim 1, characterized in that: Step 1) The dropping time is 0.5-1.5h, the reaction temperature is 20-30°C, and the reaction time is 12-24h.

5. The preparation method according to claim 1, characterized in that: Step 2) The mass ratio of the modified biomass powder, humic acid, organic resin microspheres and alkali solution is 80-90:10-15:30-35:150-180.

6. The preparation method according to claim 1, characterized in that: Step 2) The organic resin microspheres are selected from polystyrene microspheres, polytetrafluoroethylene microspheres, or a combination of both, and the average particle size of the organic resin microspheres is 100-500 μm.

7. The preparation method according to claim 1, characterized in that: Step 2) The concentration of the alkali solution is 40-50wt%, and the alkali solution is selected from sodium hydroxide, potassium hydroxide, or a combination of the two.

8. The preparation method according to claim 1, characterized in that: Step 2) The first drying is performed at 150-180°C until constant weight; the carbonization is performed at 450-600°C for 2-3 hours; the second drying is performed at 120-150°C until constant weight; the graphitization is performed in an inert gas atmosphere at a temperature of 1750-1900°C for 4-8 hours; the third drying temperature is 95-105°C until constant weight.

9. The biomass N, P, S multi-doped graphitized carbon material prepared by the preparation method according to any one of claims 1 to 8; preferably, the biomass N, P, S multi-doped graphitized carbon material has a graphitization degree of 1 D / I G Between 0.50-0.

61.

10. A negative electrode lead paste for a lead-carbon battery, using the biomass N, P, S multi-component doped graphitized carbon material as an additive for the negative electrode lead paste.

Citation Information

Patent Citations

  • Preparation method of activated carbon for multi-element co-doped lead-carbon batteries

    CN106853968A

  • Preparation method of modified mulberry stem biomass charcoal adsorbent

    CN109092247A

  • Preparation method of self-supporting heteroatom doped sludge carbon electrode material

    CN111647907A

  • Preparation method and application of iron-modified carbon microsphere / carbon nanosheet composite porous carbon based on hydrothermal carbonization of moso bamboos

    CN112194132A

  • Application of modified rice husk-based capacitor carbon in lead-carbon battery

    CN114566721A

Cited By

  • Activated carbon for high-magnification supercapacitor and preparation method

    CN121215442A