Cover plate and preparation method thereof, display panel and display device

By setting a reinforcement sublayer in the ultra-thin glass cover to improve its strain limit, the problem of insufficient bending performance and impact resistance of the ultra-thin glass cover is solved, and higher impact resistance and bending performance are achieved, reducing the The cracking situation improves the performance of the display panel and display device.

CN118894640APending Publication Date: 2024-11-05BOE TECHNOLOGY GROUP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410917895.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The bending performance and impact resistance of ultra-thin glass covers are insufficient, and they are prone to fragmentation.

Method used

An ultra-thin glass layer including a base sublayer and a reinforcement sublayer is adopted. The reinforcement sublayer is arranged on the outside of the base sublayer, and its internal stress is greater than that of the base sublayer. The reinforcement sublayer is formed by laser irradiation to increase the strain limit, and an impact resistance is prepared. Cover with better performance and bending performance.

Benefits of technology

It effectively improves the impact resistance and bending performance of the cover plate, reduces the occurrence of rupture, and thus improves the performance of the display panel and display device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118894640A_ABST
    Figure CN118894640A_ABST
Patent Text Reader

Abstract

The embodiment of the invention provides a cover plate and a preparation method thereof, a display panel and a display device. Wherein the cover plate comprises an ultra-thin glass layer; the ultra-thin glass layer comprises a basic sub-layer and a reinforced sub-layer; the reinforced sub-layer is arranged on the outer side of the basic sub-layer; the internal stress of the strengthening sub-layer is larger than that of the basic sub-layer. When the cover plate is bent or impacted, the outer surface of the ultra-thin glass layer is impacted firstly, the internal stress of the reinforcing sub-layer is larger than that of the basic sub-layer, and the reinforcing sub-layer is arranged on the outer side of the basic sub-layer, so that the reinforcing sub-layer can resist larger external tensile stress and impact force, the strain limit of the ultra-thin glass layer is improved, and the service life of the ultra-thin glass layer is prolonged. Therefore, the impact resistance and the bending performance of the cover plate are improved, and the occurrence of the condition that the cover plate is broken is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of display technology, and in particular to a cover plate and a preparation method thereof, a display panel, and a display device. Background Art

[0002] With the rapid development of electronic technology, foldable display devices are becoming more and more popular among consumers. The display panel of the display device can use an ultra-thin glass (UTG) cover plate, which is superior to a transparent polyimide cover plate in many aspects. However, the ultra-thin glass cover plate has insufficient bending performance and impact resistance and is prone to breakage. Summary of the invention

[0003] The purpose of the embodiments of the present invention is to provide a cover plate and a method for manufacturing the same, a display panel, and a display device, so as to improve the impact resistance and bending performance of the cover plate, thereby reducing the occurrence of the cover plate cracking. The specific technical solution is as follows:

[0004] An embodiment of the first aspect of the present application proposes a cover plate, which includes an ultra-thin glass layer; the ultra-thin glass layer includes a base sublayer and a strengthening sublayer; the strengthening sublayer is arranged on the outside of the base sublayer; the internal stress of the strengthening sublayer is greater than the internal stress of the base sublayer.

[0005] In some embodiments of the present application, the ultra-thin glass layer has a bending area and a non-bending area; the bending area extends along the first direction and is located between two adjacent non-bending areas;

[0006] At least a portion of the reinforcement sublayer is located in the bending region.

[0007] In some embodiments of the present application, the base sublayer includes: a first surface and a second surface disposed opposite to each other;

[0008] The strengthening sublayer is arranged outside the first surface and / or the second surface, and the orthographic projection of the strengthening sublayer on the base sublayer covers the bending area.

[0009] In some embodiments of the present application, the first surface and / or the second surface are recessed inwardly at positions corresponding to the strengthening sublayer to form a groove;

[0010] The strengthening sublayer is formed in the groove.

[0011] In some embodiments of the present application, a side of the strengthening sublayer away from the basic sublayer is lower than a notch of the groove accommodating the strengthening sublayer.

[0012] In some embodiments of the present application, the base sublayer further includes: a third surface; the third surface surrounds the first surface and the second surface and is connected to an edge of the first surface and an edge of the second surface respectively;

[0013] The strengthening sublayer is arranged on the outer side of the third surface and covers the third surface.

[0014] In some embodiments of the present application, when the ultra-thin glass layer is in a flattened state, the cross-sectional shape of the ultra-thin glass layer along the second direction and the thickness direction of the cover plate is a rectangle, a dumbbell, or an octagon;

[0015] The second direction, the first direction, and a thickness direction of the cover plate are perpendicular to each other.

[0016] In some embodiments of the present application, the strengthening sublayer includes: at least one first strengthening region, a second strengthening region, and a third strengthening region;

[0017] At least one of the first strengthening region, the second strengthening region and the third strengthening region is arranged in sequence in a manner that the first strengthening region, the second strengthening region, the first strengthening region and the third strengthening region are arranged in sequence as a period;

[0018] The internal stresses of the first strengthened region, the third strengthened region and the second strengthened region increase sequentially.

[0019] In some embodiments of the present application, the thickness of the ultra-thin glass layer ranges from 30 μm to 200 μm;

[0020] The thickness of the strengthening sublayer ranges from 0.1 μm to 40 μm;

[0021] The numerical range of the internal stress of the strengthening sublayer is: 10MPa-1000Mpa;

[0022] The difference in internal stress between the strengthening sublayer and the base sublayer has a numerical range of 400 MPa to 800 MPa.

[0023] The total thickness of the strengthening sublayer located in the bending zone is less than or equal to two-thirds of the thickness of the ultra-thin glass layer in the bending zone.

[0024] In some embodiments of the present application, the cover plate further includes: a protective layer;

[0025] In the thickness direction of the cover plate, the protection layer and the ultra-thin glass are stacked and cover the ultra-thin glass layer.

[0026] The embodiment of the second aspect of the present application provides a method for preparing a cover plate, which is used to prepare the cover plate of any embodiment of the first aspect, including the step of preparing an ultra-thin glass layer;

[0027] The step of preparing the ultra-thin glass layer comprises:

[0028] Provide ultra-thin glass;

[0029] At least one preset area of ​​the ultra-thin glass is irradiated with laser, so that the ultra-thin glass in the preset area is melted under the action of the laser; the ultra-thin glass after laser irradiation is cooled, so that the ultra-thin glass in the preset area is formed into the strengthening sublayer; the remaining part of the ultra-thin glass is formed into the basic sublayer, forming the ultra-thin glass layer including the basic sublayer and the strengthening sublayer.

[0030] In some embodiments of the present application, the method of using laser to irradiate at least one preset area of ​​the ultra-thin glass so that the ultra-thin glass in the preset area melts under the action of the laser; cooling the ultra-thin glass after laser irradiation so that the ultra-thin glass in the preset area forms the strengthening sublayer; and forming the remaining part of the ultra-thin glass into the basic sublayer, forming the ultra-thin glass layer including the basic sublayer and the strengthening sublayer, comprises:

[0031] Starting from the first end of the preset area along the preset moving direction, the preset area is sequentially irradiated with a laser line until the second end of the preset area along the preset moving direction; so that after each irradiation and cooling, a laser enhanced sub-area corresponding to the laser line irradiation area can be formed in the preset area, and in the first direction, adjacent laser enhanced sub-areas have overlapping areas;

[0032] A plurality of the laser-enhanced sub-regions form the enhanced sub-layer; and the region not irradiated by the laser forms the basic sub-layer.

[0033] In some embodiments of the present application, the preset area includes: a bending area;

[0034] The method comprises: irradiating at least one preset area of ​​the ultra-thin glass with a laser so that the ultra-thin glass in the preset area is melted under the action of the laser; cooling the ultra-thin glass after the laser irradiation so that the ultra-thin glass in the preset area is formed into the strengthening sublayer; and forming the remaining part of the ultra-thin glass into the basic sublayer, thereby forming the ultra-thin glass layer including the basic sublayer and the strengthening sublayer, comprising:

[0035] Using laser to irradiate the bending area of ​​the ultra-thin glass, so that the ultra-thin glass in the bending area is melted under the action of the laser; cooling the ultra-thin glass after laser irradiation, so that the ultra-thin glass in the bending area is formed into the strengthening sublayer; the remaining part of the ultra-thin glass is formed into the basic sublayer, forming the ultra-thin glass layer including the basic sublayer and the strengthening sublayer;

[0036] The method of preparing the cover plate further includes: preparing a protective layer on the ultra-thin glass layer.

[0037] In some embodiments of the present application, before the laser is used to irradiate at least one preset area of ​​the ultra-thin glass, the ultra-thin glass in the preset area is melted under the action of the laser; the ultra-thin glass after laser irradiation is cooled, so that the ultra-thin glass in the preset area is formed into the strengthening sublayer; the remaining part of the ultra-thin glass is formed into the basic sublayer, and before the ultra-thin glass layer including the basic sublayer and the strengthening sublayer is formed, the method further includes:

[0038] Performing a patterning process on the bending area of ​​the ultra-thin glass to form a groove;

[0039] The strengthening sublayer is formed in the groove.

[0040] An embodiment of the third aspect of the present application provides a display panel, comprising a cover plate according to any embodiment of the first aspect, and a polarizing layer, a light-emitting layer and a supporting layer arranged in sequence in a direction away from the cover plate.

[0041] An embodiment of a fourth aspect of the present application provides a display device, comprising a display panel of any embodiment of the third aspect.

[0042] Beneficial effects of the embodiments of the present invention:

[0043] The cover plate of the embodiment of the present application includes an ultra-thin glass layer, and the ultra-thin glass layer includes a base sublayer and a strengthened sublayer; the strengthened sublayer is arranged on the outside of the base sublayer; when the cover plate is bent or impacted, the outer surface of the ultra-thin glass layer is impacted first, because the internal stress of the strengthened sublayer is greater than the internal stress of the base sublayer, and the strengthened sublayer is arranged on the outside of the base sublayer, the strengthened sublayer can resist greater external tensile stress and impact force, thereby improving the strain limit of the ultra-thin glass layer, thereby improving the impact resistance and bending performance of the cover plate, and further reducing the occurrence of cover plate cracking.

[0044] The cover plate prepared by the cover plate preparation method of the embodiment of the present application includes an ultra-thin glass layer, and the ultra-thin glass layer includes a base sublayer and a strengthening sublayer; the strengthening sublayer is arranged on the outside of the base sublayer; when the cover plate is bent or impacted, the outer surface of the ultra-thin glass layer is impacted first, because the internal stress of the strengthening sublayer is greater than the internal stress of the base sublayer, and the strengthening sublayer is arranged on the outside of the base sublayer, the strengthening sublayer can resist greater external tensile stress and impact force, thereby improving the strain limit of the ultra-thin glass layer, thereby improving the impact resistance and bending performance of the cover plate, thereby reducing the occurrence of cover plate cracks, and thereby improving the performance of the display panel.

[0045] The display panel of the embodiment of the present application includes a cover plate of any embodiment of the first aspect, the cover plate includes an ultra-thin glass layer, the ultra-thin glass layer includes a base sublayer and a strengthening sublayer; the strengthening sublayer is arranged on the outside of the base sublayer; when the cover plate is bent or impacted, the first thing to be impacted is the outer surface of the ultra-thin glass layer. Since the internal stress of the strengthening sublayer is greater than the internal stress of the base sublayer, and the strengthening sublayer is arranged on the outside of the base sublayer, the strengthening sublayer can resist greater external tensile stress and impact force, thereby improving the strain limit of the ultra-thin glass layer, thereby improving the impact resistance and bending performance of the cover plate, thereby reducing the occurrence of cover plate cracks, and thereby improving the performance of the display panel.

[0046] The display device of the embodiment of the present application comprises the display panel of any embodiment of the third aspect, the display panel comprises the cover plate of any embodiment of the first aspect, the cover plate comprises an ultra-thin glass layer, the ultra-thin glass layer comprises a base sublayer and a strengthening sublayer; the strengthening sublayer is arranged on the outside of the base sublayer; when the cover plate is bent or impacted, the first thing to be impacted is the outer surface of the ultra-thin glass layer, because the internal stress of the strengthening sublayer is greater than the internal stress of the base sublayer, and the strengthening sublayer is arranged on the outside of the base sublayer, the strengthening sublayer can resist greater external tensile stress and impact force, thereby improving the strain limit of the ultra-thin glass layer, thereby improving the impact resistance and bending performance of the cover plate, thereby reducing the occurrence of cover plate breakage, and thereby improving the performance of the display device.

[0047] Of course, it is not necessary to achieve all of the advantages described above at the same time to implement any product or method of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are only some embodiments of the present invention. For ordinary technicians in this field, other embodiments can also be obtained based on these drawings.

[0049] Figure 1This is a schematic structural diagram of an ultra-thin glass layer according to a first embodiment of the present application;

[0050] Figure 2 for Figure 1 A top view of

[0051] Figure 3 A schematic diagram of the laser line path when preparing the ultra-thin glass layer in an embodiment of the present application;

[0052] Figure 4 for Figure 1 A local enlarged schematic diagram of P;

[0053] Figure 5 This is a schematic structural diagram of an ultra-thin glass layer according to a second embodiment of the present application;

[0054] Figure 6 This is a schematic structural diagram of an ultra-thin glass layer according to a third embodiment of the present application;

[0055] Figure 7 This is a schematic structural diagram of an ultra-thin glass layer according to a fourth embodiment of the present application;

[0056] Figure 8 This is a schematic structural diagram of an ultra-thin glass layer according to a fifth embodiment of the present application;

[0057] Fig. 9 This is a schematic structural diagram of an ultra-thin glass layer according to a sixth embodiment of the present application;

[0058] Fig.10 This is a schematic diagram of the structure of the cover plate of an embodiment of the present application;

[0059] Fig.11 This is a flow chart of a method for preparing a cover plate according to the first embodiment of the present application;

[0060] Fig.12a This is a process flow chart of preparing a cover plate according to the first embodiment of the present application (step 1 and step 2);

[0061] Figure 12b This is a process flow chart of preparing a cover plate according to the first embodiment of the present application (steps 3 and 5);

[0062] Fig.13 Schematic diagram of the structure of the display panel according to the embodiment of the present application.

[0063] Description of reference numerals:

[0064] Cover plate 10; polarizing layer 20; light-emitting layer 30; supporting layer 40; ultra-thin glass layer 100; base sublayer 110; first surface 111; second surface 112; third surface 113; groove 114; strengthening sublayer 120; first strengthening area 121; second strengthening area 122; third strengthening area 123; bending area 101; non-bending area 102; protective layer 200; ultra-thin glass 1; laser strengthening subarea 11; non-overlapping area 11-1; overlapping area 11-2; fourth surface 12; fifth surface 13; sixth surface 14; preset area M; laser emitter 2; laser line 21. DETAILED DESCRIPTION

[0065] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field based on this application belong to the scope of protection of the present invention.

[0066] With the rapid development of electronic technology, foldable display devices are becoming more and more popular among consumers. The display panel of the display device can use an ultra-thin glass (UTG) cover plate, which is superior to the transparent polyimide cover plate in many aspects. However, the bending performance and impact resistance of the ultra-thin glass cover plate are insufficient and it is easy to break. In order to solve the above technical problems, the embodiments of the present application propose a cover plate and a preparation method thereof, a display panel, and a display device.

[0067] like Figure 1 As shown, Figure 1 This is a structural schematic diagram of the ultra-thin glass layer 100 of the first embodiment of the present application. The embodiment of the first aspect of the present application proposes a cover plate 10, including the ultra-thin glass layer 100; specifically, the ultra-thin glass layer 100 includes a base sublayer 110 and a strengthening sublayer 120; the strengthening sublayer 120 is arranged on the outside of the base sublayer 110; the internal stress of the strengthening sublayer 120 is greater than the internal stress of the base sublayer 110.

[0068] The cover plate 10 of the embodiment of the present application includes an ultra-thin glass layer 100, and the ultra-thin glass layer 100 includes a base sublayer 110 and a strengthening sublayer 120; the strengthening sublayer 120 is arranged on the outside of the base sublayer 110; when the cover plate 10 is bent or impacted, the outer surface of the ultra-thin glass layer 100 is impacted first. Since the internal stress of the strengthening sublayer 120 is greater than the internal stress of the base sublayer 110, and the strengthening sublayer 120 is arranged on the outside of the base sublayer 110, the strengthening sublayer 120 can resist greater external tensile stress and impact force, thereby improving the strain limit of the ultra-thin glass layer 100, thereby improving the impact resistance and bending performance of the cover plate 10, and further reducing the occurrence of cracks in the cover plate 10.

[0069] It should be noted that if Figure 1 and Figure 2 As shown, Figure 1 Schematic diagram of the structure of the ultra-thin glass layer 100 of the first embodiment of the present application. Figure 2 for Figure 1 For the sake of convenience, we define the first direction as the width direction of the cover plate 10, the second direction as the length direction of the cover plate 10, and the first direction, the second direction and the thickness direction of the cover plate 10 are perpendicular to each other. In some other embodiments of the present application, the first direction may also be the length direction of the cover plate 10, and the second direction may be the width direction of the cover plate 10, and the present application does not limit this.

[0070] In the first embodiment of the present application, Figure 1 and Figure 2 As shown, the ultra-thin glass layer 100 has a bending area 101 and a non-bending area 102; the bending area 101 extends along the first direction and is located between two adjacent non-bending areas 102; at least part of the strengthening sublayer 120 is located in the bending area 101. At least part of the strengthening sublayer 120 is located in the bending area 101. Since the internal stress of the strengthening sublayer 120 is greater than the internal stress of the base sublayer 110, the strengthening sublayer 120 can better resist the tensile stress during bending, thereby improving the strain limit of the cover plate 10, and the bending performance is better, while improving the impact resistance of the bending area 101, thereby reducing the occurrence of the cover plate 10 being broken.

[0071] The ultra-thin glass layer 100 can be bent along the bending area 101, so that the ultra-thin glass layer 100 has a folded state and a flattened state; Figure 1The flattened state of the ultra-thin glass layer 100 is shown, and the bending area 101 is flattened, so that the non-bending area 102 and the bending area 101 are located in the same plane; when the ultra-thin glass layer 100 is in a folded state, the two non-bending areas 102 located on both sides of the bending area 101 are superimposed together. In order to achieve the folding and flattening of the display device, the bending area 101 of the ultra-thin glass layer 100, the bending area of ​​the cover plate 10 (not shown in the figure), and the bending area of ​​the display panel (not shown in the figure) should all be set accordingly.

[0072] In the first embodiment of the present application, Figure 1 and Figure 2 As shown, the base sublayer 110 includes a first surface 111 and a second surface 112 that are arranged opposite to each other; the strengthening sublayer 120 is arranged outside the first surface 111 and the second surface 112, and is at least partially located in the bending area 101. The strengthening sublayer 120 is arranged outside at least part of the first surface 111 and the second surface 112, which can further improve the bending performance of the cover plate 10. It can be understood that the strengthening sublayers 120 on the first surface 111 and the second surface 112 can be symmetrically arranged, so that the stress on both sides of the ultra-thin glass layer 100 is more even, which can prevent the ultra-thin glass layer 100 from warping.

[0073] In the first embodiment of the present application, Figure 1 As shown, the base sublayer 110 also includes a third surface 113 ; the third surface 113 surrounds the first surface 111 and the second surface 112 , and is connected to the edge of the first surface 111 and the edge of the second surface 112 respectively, that is, the third surface 113 can be the side of the ultra-thin glass layer 100 .

[0074] In the first embodiment of the present application, Figure 1 and Figure 2 As shown, the orthographic projection of the strengthening sublayer 120 on the base sublayer 110 covers the bending area 101. In this way, the bending performance of the cover plate 10 can be further improved.

[0075] In some other embodiments of the present application, the orthographic projection of the strengthening sublayer 120 on the base sublayer 110 may also be located within the bending zone 101. In this way, the bending performance of the cover plate 10 may be improved to a certain extent. The present application does not limit this.

[0076] Optionally, the orthographic projection of the strengthening sublayer 120 on the base sublayer 110 is the same as the range of the bending zone 101 in the first direction, and can be located within the range of the bending zone 101 in the second direction, or can exceed the range of the bending zone 101, or can overlap with the range of the bending zone 101, and this application does not limit this. It should be noted that in the embodiments of this application, "same" means the same within a certain tolerance range, and the meaning of "same" appearing in the following text is the same as here, and will not be repeated.

[0077] In the first embodiment of the present application, Figure 1 As shown, the strengthening sublayer 120 can be flush with the portion of the first surface 111 or the second surface 112 located in the non-bending area 102 , thereby forming a flat plane, which is helpful to ensure the flatness of the cover plate 10 .

[0078] In the first embodiment of the present application, Figure 1 As shown, when the ultra-thin glass layer 100 is flattened, the cross-sectional shape of the ultra-thin glass layer 100 along the second direction and the thickness direction of the cover plate 10 is rectangular. The rectangular ultra-thin glass layer 100 is easy to process and helps improve production efficiency.

[0079] In the process of preparing the ultra-thin glass layer 100, a laser strengthening method can be used to form a strengthening sublayer 120. The laser is used to irradiate the outer surface of the ultra-thin glass. The laser instantly melts the surface layer of the ultra-thin glass and quickly cools it. The melted and cooled position forms the strengthening sublayer 120, and a stress difference is formed with the unmelted position. The unmelted part forms the basic sublayer 110, thereby forming the ultra-thin glass layer 100.

[0080] like Figure 3 As shown, Figure 3 Schematic diagram of the laser line path when preparing the ultra-thin glass layer 100 in the embodiment of the present application. By laser strengthening the ultra-thin glass, a strengthening sublayer 120 can be formed. In this process, multiple laser beams can be emitted in sequence, such as Figure 3 As shown, laser line 1 is emitted first, and then a laser emitter (not shown in the figure) is moved along the path of the laser line to emit laser line 2. In order to ensure the integrity of the formed strengthening sublayer 120, the laser line irradiation areas of two adjacent laser lines, such as laser line 1 and laser line 2, should overlap, so that two adjacent laser strengthening sub-areas 11 corresponding to the laser line irradiation areas form an overlapping area 11-2 and a non-overlapping area 11-1. Since the laser line has the characteristics of being strong in the middle area and weak in the areas on both sides, and the internal stress value of the strengthening sublayer 120 is positively correlated with the intensity of the laser line, the internal stress value of the strengthening sublayer 120 along the direction of the laser line path is not exactly the same, and since there are certain differences in the degree of melting and the cooling speed of each part, it will also affect the internal stress of the strengthening sublayer 120. The internal stress value of the strengthening sublayer 120 may be as follows Figure 4 The striped partitions shown.

[0081] In the first embodiment of the present application, Figure 3 and 4 As shown, Figure 4 for Figure 1The partial enlarged schematic diagram at P of FIG. 1 shows that the strengthening sublayer 120 includes at least one first strengthening region 121, a second strengthening region 122 and a third strengthening region 123; the second strengthening region 122 corresponds to the middle region where the laser line is stronger, the first strengthening region 121 corresponds to the two side regions where the laser line is weaker, and the third strengthening region 123 corresponds to the overlapping region 11-2, and the range of the overlapping region 11-2 is smaller than the range of the first strengthening region 121; since the third strengthening region 123 is irradiated by the laser line with a weaker intensity twice, its internal stress value is greater than that of the first strengthening region 121 which is irradiated by the laser line with a weaker intensity only once, but the superposition intensity of the laser line with a weaker intensity twice may still be less than the intensity of the middle region of the laser line, therefore, at least one first strengthening region 121, the second strengthening region 122 and the third strengthening region 123 are arranged in sequence in the manner of the first strengthening region 121, the second strengthening region 122, the first strengthening region 121 and the third strengthening region 123 being arranged in sequence as a period; the internal stresses of the first strengthening region 121, the third strengthening region 123 and the second strengthening region 122 increase in sequence. The first strengthening region 121 , the second strengthening region 122 and the third strengthening region 123 are distributed in stripes and are arranged in a certain period.

[0082] In the first embodiment of the present application, the thickness range of the ultra-thin glass layer 100 is: 30μm-200μm, for example, it can be 30μm, 60μm, 100μm, 150μm, 200μm; the thickness range of the strengthening sublayer 120 is: 0.1μm-40μm, for example, it can be 0.1μm, 1μm, 10μm, 20μm, 30μm, 40μm; the value range of the internal stress of the strengthening sublayer 120 is: 10MPa-1000Mpa, for example, it can be 10MPa, 200MPa, 5 The difference between the internal stress of the strengthening sublayer 120 and the base sublayer 110 is in the range of 400-800 MPa, for example, 400 MPa, 500 MPa, 600 MPa, 700 MPa, 800 MPa; the total thickness of the strengthening sublayer 120 located in the bending zone 101 is less than or equal to two-thirds of the thickness of the ultra-thin glass layer 100 in the bending zone 101, for example, one-quarter, one-third, two-fifths, one-half, two-thirds, etc. Meeting the above numerical range can improve the strain limit of the ultra-thin glass layer 100, thereby improving the impact resistance and bending performance of the cover plate 10.

[0083] like Figure 1As shown, in the first embodiment of the present application, a strengthening sublayer 120 is formed at the positions of the first surface 111 and the second surface 112 corresponding to the bending zone 101; then the sum of the thicknesses of the two strengthening sublayers 120 must be less than or equal to two-thirds of the sum of the thicknesses of the base sublayer 110 and the strengthening sublayer 120 located in the bending zone 101.

[0084] In the first embodiment of the present application, the ultra-thin glass layer 100 is aluminosilicate glass, lithium aluminosilicate glass or microcrystalline glass. Aluminosilicate glass has a high content of Al2O3 and SiO2, and has good chemical stability, electrical insulation, mechanical strength and low thermal expansion coefficient; lithium aluminosilicate glass has high light transmittance, low dispersion and low radiation absorption, and can reach an optical transmittance of more than 98%, ensuring the balance in optical aspects such as transmission, reflection and refraction; microcrystalline glass has the characteristics of both glass and ceramics, and has excellent wear resistance and corrosion resistance.

[0085] like Figure 5 As shown, Figure 5 This is a schematic diagram of the structure of the ultra-thin glass layer 100 of the second embodiment of the present application. The difference between the cover plate 10 of the second embodiment of the present application and the cover plate 10 of the first embodiment of the present application is that the cover plate 10 of the second embodiment of the present application has a strengthening sublayer 120 formed only on one side of the ultra-thin glass layer 100, rather than on both sides.

[0086] In the second embodiment of the present application, Figure 5 As shown, the base sublayer 110 includes a first surface 111 and a second surface 112 disposed opposite to each other; the strengthening sublayer 120 is disposed outside the first surface 111 and at least partially located in the bending zone 101. The strengthening sublayer 120 is disposed in the bending zone 101 to improve the bending performance of the cover plate 10. Figure 5 In the illustrated embodiment, the strengthening sublayer 120 is disposed on the outer side of the first surface 111 . In some other embodiments of the present application, the strengthening sublayer 120 may also be disposed on the outer side of the second surface 112 , which is not limited in the present application.

[0087] Optionally, when the ultra-thin glass layer 100 is in a folded state, the first surface 111 is located on the outside of the second surface 112, and the strengthening sublayer 120 can be arranged only on the outside of the first surface 111. The surface located on the outside is usually subjected to greater tensile stress. The strengthening sublayer 120 is arranged on the outside to better improve the bending performance of the cover plate 10. Of course, in some other embodiments of the present application, the strengthening sublayer 120 can also be arranged only on the second surface 112 located on the inside, which also has a certain effect of improving the bending performance of the cover plate 10, and the present application does not limit this.

[0088] like Figure 6 As shown, Figure 62 is a schematic structural diagram of an ultra-thin glass layer 100 according to a third embodiment of the present application. The difference between the cover plate 10 according to the third embodiment of the present application and the cover plate 10 according to the first embodiment of the present application is that the ultra-thin glass layer 100 in the third embodiment of the present application is provided with a groove 114 in the bending area 101.

[0089] In the third embodiment of the present application, Figure 6 As shown, the first surface 111 and / or the second surface 112 are recessed inward at positions corresponding to the strengthening sublayer 120 to form a groove 114; the strengthening sublayer 120 is formed in the groove 114. The side of the strengthening sublayer 120 away from the base sublayer 110 is lower than the notch of the groove 114 accommodating the strengthening sublayer 120. In this way, the overall thickness of the bending area 101 is thinner, which is conducive to bending, and the overall thickness of the non-bending area 102 is thicker, which is conducive to improving strength.

[0090] In the third embodiment of the present application, Figure 6 As shown, when the first surface 111 and the second surface 112 are flattened, the cross-sectional shape of the ultra-thin glass layer 100 along the second direction and the thickness direction of the cover plate 10 is dumbbell-shaped, and the ultra-thin glass layer 100 is thinned in the bending area 101 .

[0091] It should be noted that the ultra-thin glass layer 100 in the third embodiment of the present application may have a strengthening sub-layer 120 formed on one side or on both sides, and the present application does not limit this.

[0092] like Figure 7 As shown, Figure 7 This is a schematic diagram of the structure of the ultra-thin glass layer 100 of the fourth embodiment of the present application. The difference between the cover plate 10 of the fourth embodiment of the present application and the cover plate 10 of the first embodiment of the present application lies in that the strengthening sublayer 120 of the cover plate 10 of the fourth embodiment of the present application is not only formed on the first surface 111 and the second surface 112, but also formed on the third surface 113.

[0093] In the fourth embodiment of the present application, Figure 7 As shown, the base sublayer 110 further includes a third surface 113; the third surface 113 surrounds the first surface 111 and the second surface 112, and is connected to the edge of the first surface 111 and the edge of the second surface 112 respectively; the strengthening sublayer 120 is arranged on the outside of the third surface 113 and covers the third surface 113. Since the third surface 113 is the side of the cover plate 10 and is easily impacted, the strengthening sublayer 120 covers the third surface 113, which can improve the impact resistance of the cover plate 10.

[0094] It is understandable that in order to improve the impact resistance of the side of the cover plate 10 , in some other embodiments of the present application, the reinforcing sublayer 120 may not be provided in the bending zone 101 , and the reinforcing sublayer 120 may only be provided on the outer side of the third surface 113 .

[0095] like Figure 8 As shown, Figure 8 2 is a schematic structural diagram of an ultra-thin glass layer 100 according to a fifth embodiment of the present application. The difference between the cover plate 10 according to the fifth embodiment of the present application and the cover plate 10 according to the fourth embodiment of the present application is that the shape of the ultra-thin glass layer 100 is different.

[0096] In the fifth embodiment of the present application, Figure 8 As shown, when the first surface 111 and the second surface 112 are flattened, the cross-sectional shape of the ultra-thin glass layer 100 along the second direction and the thickness direction of the cover plate 10 is an octagon, that is, the side edges of the ultra-thin glass layer 100 are chamfered for easy assembly.

[0097] like Fig. 9 As shown, Fig. 9 1 is a schematic structural diagram of an ultra-thin glass layer 100 according to a sixth embodiment of the present application. The difference between the cover plate 10 according to the sixth embodiment of the present application and the cover plate 10 according to the first embodiment of the present application is that the formation range of the strengthening sublayer 120 is different.

[0098] In the sixth embodiment of the present application, Fig. 9 As shown, the outer sides of the first surface 111 and the second surface 112 of the base sublayer 110 in the sixth embodiment of the present application may be provided with a strengthening sublayer 120, and the strengthening sublayer 120 completely covers the first surface 111 and the second surface 112, thereby improving the impact resistance and bending performance of the cover plate 10 as a whole.

[0099] like Fig.10 As shown, Fig.10 : is a schematic diagram of the structure of the cover plate 10 of the embodiment of the present application, the cover plate 10 further includes a protective layer 200; in the thickness direction of the cover plate 10, the protective layer 200 and the ultra-thin glass layer 100 are stacked and cover the ultra-thin glass layer 100. It can be understood that the protective layer 200 can be formed on the display side of the ultra-thin glass layer 100. Optionally, the material of the protective layer 200 can be CPI (transparent polyimide).

[0100] like Figure 11 to Figure 12b As shown, Fig.11 This is a flow chart of a method for preparing a cover plate 10 according to the first embodiment of the present application. Fig.12a This is a process flow chart of preparing the cover plate 10 of the first embodiment of the present application (step 1 and step 2). Figure 12bThe process flow chart of the preparation process of the cover plate 10 of the first embodiment of the present application (step 3 and step 5) is as follows. The embodiment of the second aspect of the present application proposes a method for preparing the cover plate 10, which is used to prepare the cover plate 10 of any embodiment of the first aspect, comprising:

[0101] S1, step of preparing an ultra-thin glass layer 100;

[0102] S2 . Preparing a protective layer 200 on the ultra-thin glass layer 100 .

[0103] The cover plate 10 prepared by the preparation method of the cover plate 10 of the embodiment of the present application includes an ultra-thin glass layer 100, and the ultra-thin glass layer 100 includes a base sublayer 110 and a strengthening sublayer 120; the strengthening sublayer 120 is arranged on the outside of the base sublayer 110; when the cover plate 10 is bent or impacted, the outer surface of the ultra-thin glass layer 100 is impacted first, because the internal stress of the strengthening sublayer 120 is greater than the internal stress of the base sublayer 110, and the strengthening sublayer 120 is arranged on the outside of the base sublayer 110, the strengthening sublayer 120 can resist greater external tensile stress and impact force, thereby improving the strain limit of the ultra-thin glass layer 100, thereby improving the impact resistance and bending performance of the cover plate 10, thereby reducing the occurrence of cracks in the cover plate 10, and thereby improving the performance of the display panel.

[0104] Specifically, S1, the step of preparing the ultra-thin glass layer 100 comprises:

[0105] S11, providing ultra-thin glass 1;

[0106] S12, use of laser (i.e. Fig.12a The laser line 21 in the laser beam irradiates at least one preset area M of the ultra-thin glass 1, so that the ultra-thin glass 1 in the preset area M melts under the action of the laser; the ultra-thin glass 1 after laser irradiation is cooled, so that the ultra-thin glass 1 in the preset area M forms a strengthening sublayer 120; the remaining part of the ultra-thin glass 1 forms a basic sublayer 110, forming an ultra-thin glass layer 100 including the basic sublayer 110 and the strengthening sublayer 120.

[0107] like Fig.12a and Figure 12b As shown, in some embodiments of the present application, S12, using laser to irradiate at least one preset area M of the ultra-thin glass 1, so that the ultra-thin glass 1 in the preset area M melts under the action of the laser; the ultra-thin glass 1 after laser irradiation is cooled, so that the ultra-thin glass 1 in the preset area M forms a strengthening sublayer 120; the remaining part of the ultra-thin glass 1 forms a basic sublayer 110, and the ultra-thin glass layer 100 including the basic sublayer 110 and the strengthening sublayer 120 is formed, including:

[0108] Starting from the first end of the preset area M along the preset moving direction, the laser line 21 is used to sequentially move and irradiate the preset area M until the second end of the preset area M along the preset moving direction; so that after each irradiation and cooling, a laser enhanced sub-area 11 corresponding to the irradiation area of ​​the laser line 21 can be formed in the preset area M, and in the first direction, adjacent laser enhanced sub-areas 11 have overlapping areas 11-2 (refer to Figure 3 ) ; a plurality of laser enhanced sub-regions 11 form an enhanced sub-layer 120 ; and the area not irradiated by the laser is formed as a base sub-layer 110 .

[0109] like Fig.12a and Figure 12b As shown, in some embodiments of the present application, the preset area M may include a bending area 101; S12, using a laser to irradiate at least one preset area M of the ultra-thin glass 1, so that the ultra-thin glass 1 in the preset area M melts under the action of the laser; cooling the ultra-thin glass 1 after the laser irradiation, so that the ultra-thin glass 1 in the preset area M forms a strengthening sublayer 120; the remaining part of the ultra-thin glass 1 forms a basic sublayer 110, and an ultra-thin glass layer 100 including the basic sublayer 110 and the strengthening sublayer 120 is formed, including:

[0110] The bending area 101 of the ultra-thin glass 1 is irradiated with laser, so that the ultra-thin glass 1 in the bending area 101 is melted under the action of the laser; the ultra-thin glass 1 after laser irradiation is cooled, so that the ultra-thin glass 1 in the bending area 101 is formed into a strengthening sub-layer 120; the remaining part of the ultra-thin glass 1 is formed into a basic sub-layer 110, forming an ultra-thin glass layer 100 including the basic sub-layer 110 and the strengthening sub-layer 120.

[0111] like Fig.12a and Figure 12b As shown, the ultra-thin glass 1 includes a fourth surface 12, a fifth surface 13 and a sixth surface 14; the fourth surface 12 and the fifth surface 13 are arranged opposite to each other, and the sixth surface 14 surrounds the fourth surface 12 and the fifth surface 13, and is connected to the fourth surface 12 and the fifth surface 13 respectively. The following is a detailed description of the preparation method of the cover plate 10 of the first embodiment of the present application, including:

[0112] Step 1, providing an ultra-thin glass 1 with a thickness of 30 μm;

[0113] Step 2, using the laser line 21 to irradiate the preset area M of the fourth surface 12 of the ultra-thin glass 1; the laser line 21 irradiates the first end of the preset area M along the preset moving direction, and after the area is melted and cooled, a laser strengthening sub-area 11 corresponding to the irradiation area of ​​the laser line 21 is formed;

[0114] Step 3: The laser line 21 starts from the first end of the preset area M along the preset moving direction, and the laser line 21 is used to sequentially move and irradiate the preset area M until the second end of the preset area M along the preset moving direction; so that after each irradiation and cooling, a laser strengthening sub-area 11 corresponding to the irradiation area of ​​the laser line 21 can be formed in the preset area M, and in the first direction, adjacent laser strengthening sub-areas 11 have overlapping areas 11-2 (refer to Figure 3 ); forming a strengthening sublayer 120 on the fourth surface 12, that is, forming a strengthening sublayer 120 in the bending area 101 outside the first surface 111 of the base sublayer 110;

[0115] That is, the laser line 21 scans and irradiates the preset area M from the first end of the preset area M along the preset moving direction, so that the ultra-thin glass 1 in the preset area M melts and cools to form a strengthening sub-layer 120;

[0116] Step 4, turning over the ultra-thin glass 1 so that the fifth surface 13 is disposed toward the laser emitter 2;

[0117] Step 5, repeating the above steps 2 and 3 to form a strengthening sublayer 120 on the fourth surface 12, that is, forming the strengthening sublayer 120 in the bending area 101 outside the second surface 112 of the base sublayer 110;

[0118] Preparation is complete.

[0119] During the preparation process, the laser can be any form of laser such as carbon dioxide laser, picosecond laser and femtosecond laser. The above types of lasers can be used alone or in combination, and this application does not limit this.

[0120] If there are other parts that need to form the strengthening sub-layer 120, you can refer to steps 4 and 5, first turn the ultra-thin glass 1 over, and then use the laser line 21 to irradiate the preset area M.

[0121] In preparing the second embodiment of this application ( Figure 6 In the process of forming the ultra-thin glass layer 100 in the cover plate 10 of the embodiment shown in the figure, in S12, at least one preset area M of the ultra-thin glass 1 is irradiated with a laser, so that the ultra-thin glass 1 in the preset area M is melted under the action of the laser; the ultra-thin glass 1 after the laser irradiation is cooled, so that the ultra-thin glass 1 in the preset area M is formed into a strengthening sublayer 120; the remaining part of the ultra-thin glass 1 is formed into a basic sublayer 110, and before the ultra-thin glass layer 100 including the basic sublayer 110 and the strengthening sublayer 120 is formed, the method further includes:

[0122] The bending region 101 of the ultra-thin glass 1 is subjected to a patterning process to form a groove 114 ; the strengthening sub-layer 120 is formed in the groove 114 .

[0123] In preparing the third embodiment of this application ( Figure 7 In the process of forming the ultra-thin glass layer 100 in the cover plate 10 of the embodiment shown in the figure, S12, using a laser to irradiate at least one preset area M of the ultra-thin glass 1, so that the ultra-thin glass 1 in the preset area M melts under the action of the laser; cooling the ultra-thin glass 1 after the laser irradiation, so that the ultra-thin glass 1 in the preset area M forms a strengthened sublayer 120; the remaining part of the ultra-thin glass 1 forms a basic sublayer 110, and the ultra-thin glass layer 100 including the basic sublayer 110 and the strengthened sublayer 120 is formed, including: laser strengthening the fourth surface 12, the fifth surface 13 and / or the sixth surface 14 to form the ultra-thin glass layer 100 including the basic sublayer 110 and the strengthened sublayer 120.

[0124] Then, the ultra-thin glass 1 is turned over and the remaining surface is processed.

[0125] It is understandable that laser strengthening can be performed at any time during the forming process of the ultra-thin glass 1. For example, in the process of preparing the ultra-thin glass 1, it is necessary to first prepare a whole large piece of ultra-thin glass, and then cut it to form a plurality of small ultra-thin glasses 1, which can be used to prepare the cover plate 10. The laser strengthening process can be performed before or after cutting; and some small ultra-thin glasses 1 sometimes need to undergo CNC (Computerized Numerical Control) process to form different shapes. The laser strengthening process can be performed before or after the CNC process, and the operation is very flexible.

[0126] In addition, the embodiment of the present application uses laser strengthening to strengthen the ultra-thin glass 1, which is a physical process. Compared with strengthening by chemical strengthening, it greatly simplifies the production process and has higher yield and flexibility.

[0127] The chemical strengthening process involves melting a salt solution, placing the ultra-thin glass 1 in a high-viscosity salt solution, strengthening and maintaining, and then cleaning the surface salt solution. Because chemical strengthening can damage the surface, it is necessary to perform an acid treatment on the glass surface, which is a complicated process. The preparation method of the embodiment of the present application can omit the above steps and only requires the laser treatment step, which greatly simplifies the production process.

[0128] Chemical strengthening requires continuous movement of the ultra-thin glass 1, which is a complicated process, and ion replacement can also damage the ultra-thin glass 1, resulting in a low yield. Laser strengthening only requires one step, which is expected to improve the yield of strengthening.

[0129] Chemical strengthening strengthens the entire outer surface, while laser strengthening can strengthen local areas in a targeted manner, with greater flexibility and efficiency.

[0130] like Fig.13 As shown, Fig.13 The structure diagram of the display panel of the embodiment of the present application is as follows. The embodiment of the third aspect of the present application provides a display panel, comprising the cover plate 10 of any embodiment of the first aspect, and a polarizing layer 20, a light-emitting layer 30 and a supporting layer 40 sequentially arranged in a direction away from the cover plate 10. Specifically, adjacent layers can be connected by an adhesive.

[0131] The display panel of the embodiment of the present application includes the cover plate 10 of any embodiment of the first aspect, the cover plate 10 includes an ultra-thin glass layer 100, and the ultra-thin glass layer 100 includes a base sublayer 110 and a strengthening sublayer 120; the strengthening sublayer 120 is arranged on the outside of the base sublayer 110; when the cover plate 10 is bent or impacted, the first thing to be impacted is the outer surface of the ultra-thin glass layer 100. Since the internal stress of the strengthening sublayer 120 is greater than the internal stress of the base sublayer 110, and the strengthening sublayer 120 is arranged on the outside of the base sublayer 110, the strengthening sublayer 120 can resist greater external tensile stress and impact force, thereby improving the strain limit of the ultra-thin glass layer 100, thereby improving the impact resistance and bending performance of the cover plate 10, thereby reducing the occurrence of cracks in the cover plate 10, and thereby improving the performance of the display panel.

[0132] Optionally, the supporting layer 40 may include SUS (special use stainless steel) (not shown in the figure); the light-emitting layer 30 may include a light-emitting material layer (not shown in the figure), a cathode layer (not shown in the figure), an anode layer (not shown in the figure) and a thin film transistor (not shown in the figure), etc., and the polarizing layer 20 may include a polarizer (not shown in the figure).

[0133] An embodiment of a fourth aspect of the present application provides a display device, comprising a display panel of any embodiment of the third aspect.

[0134] The display device of the embodiment of the present application includes a display panel of any embodiment of the third aspect, and the display panel includes a cover plate 10 of any embodiment of the first aspect, the cover plate 10 includes an ultra-thin glass layer 100, and the ultra-thin glass layer 100 includes a base sublayer 110 and a strengthening sublayer 120; the strengthening sublayer 120 is arranged on the outside of the base sublayer 110; when the cover plate 10 is bent or impacted, the first thing to be impacted is the outer surface of the ultra-thin glass layer 100. Since the internal stress of the strengthening sublayer 120 is greater than the internal stress of the base sublayer 110, and the strengthening sublayer 120 is arranged on the outside of the base sublayer 110, the strengthening sublayer 120 can resist greater external tensile stress and impact force, thereby improving the strain limit of the ultra-thin glass layer 100, thereby improving the impact resistance and bending performance of the cover plate 10, thereby reducing the occurrence of cracks in the cover plate 10, and thereby improving the performance of the display device.

[0135] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.

[0136] Each embodiment in this specification is described in a related manner, and the same or similar parts between the embodiments can be referred to each other, and each embodiment focuses on the differences from other embodiments. In particular, for the system embodiment, since it is basically similar to the method embodiment, the description is relatively simple, and the relevant parts can be referred to the partial description of the method embodiment.

[0137] The above description is only a preferred embodiment of the present invention and is not intended to limit the protection scope of the present invention. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention are included in the protection scope of the present invention.

Claims

1. A cover plate, characterized in that: include: Ultra-thin glass layer; The ultra-thin glass layer includes a base sublayer and a strengthening sublayer; The strengthening sublayer is arranged on the outer side of the base sublayer; and the internal stress of the strengthening sublayer is greater than the internal stress of the base sublayer.

2. The cover plate according to claim 1, characterized in that: The ultra-thin glass layer has a bending area and a non-bending area; the bending area extends along a first direction and is located between two adjacent non-bending areas; At least a portion of the reinforcement sublayer is located in the bending region.

3. The cover plate according to claim 2, characterized in that: The base sublayer comprises a first surface and a second surface arranged opposite to each other; The strengthening sublayer is arranged outside the first surface and / or the second surface, and the orthographic projection of the strengthening sublayer on the base sublayer covers the bending area.

4. The cover plate according to claim 3, characterized in that: The positions of the first surface and / or the second surface corresponding to the strengthening sublayer are recessed inwards to form grooves; The strengthening sublayer is formed in the groove.

5. The cover plate according to claim 4, characterized in that: A side of the strengthening sub-layer away from the basic sub-layer is lower than the notch of the groove accommodating the strengthening sub-layer.

6. The cover plate according to any one of claims 3 to 5, characterized in that: The base sublayer further includes: a third surface; the third surface surrounds the first surface and the second surface and is connected to an edge of the first surface and an edge of the second surface respectively; The strengthening sublayer is arranged on the outer side of the third surface and covers the third surface.

7. The cover plate according to any one of claims 3 to 5, characterized in that: When the ultra-thin glass layer is in a flattened state, the cross-sectional shape of the ultra-thin glass layer along the second direction and the thickness direction of the cover plate is a rectangle, a dumbbell or an octagon; The second direction, the first direction, and a thickness direction of the cover plate are perpendicular to each other.

8. The cover plate according to claim 1, characterized in that: The strengthening sublayer includes: at least a first strengthening region, a second strengthening region and a third strengthening region; At least one of the first strengthening region, the second strengthening region and the third strengthening region is arranged in sequence in a manner that the first strengthening region, the second strengthening region, the first strengthening region and the third strengthening region are arranged in sequence as a period; The internal stresses of the first strengthened region, the third strengthened region and the second strengthened region increase sequentially.

9. The cover plate according to claim 2, characterized in that: The thickness of the ultra-thin glass layer ranges from 30 μm to 200 μm; The thickness of the strengthening sublayer ranges from 0.1 μm to 40 μm; The numerical range of the internal stress of the strengthening sublayer is: 10MPa-1000Mpa; The difference between the internal stress of the strengthening sublayer and the basic sublayer has a numerical range of: 400Mpa-800Mpa; The total thickness of the strengthening sublayer located in the bending zone is less than or equal to two-thirds of the thickness of the ultra-thin glass layer in the bending zone.

10. The cover plate according to claim 1, characterized in that: The cover plate further comprises: a protective layer; In the thickness direction of the cover plate, the protection layer and the ultra-thin glass are stacked and cover the ultra-thin glass layer.

11. A method for preparing a cover plate, characterized in that: Used to prepare the cover plate according to any one of claims 1 to 10, comprising the step of preparing an ultra-thin glass layer; The step of preparing the ultra-thin glass layer comprises: Provide ultra-thin glass; At least one preset area of ​​the ultra-thin glass is irradiated with laser, so that the ultra-thin glass in the preset area is melted under the action of the laser; the ultra-thin glass after laser irradiation is cooled, so that the ultra-thin glass in the preset area is formed into the strengthening sublayer; the remaining part of the ultra-thin glass is formed into the basic sublayer, forming the ultra-thin glass layer including the basic sublayer and the strengthening sublayer.

12. The method for preparing a cover plate according to claim 11, characterized in that: The method further comprises: irradiating at least one preset area of ​​the ultra-thin glass with a laser so that the ultra-thin glass in the preset area is melted under the action of the laser; cooling the ultra-thin glass after the laser irradiation so that the ultra-thin glass in the preset area is formed into the strengthening sublayer; The remaining part of the ultra-thin glass is formed as the base sub-layer, and the ultra-thin glass layer including the base sub-layer and the strengthening sub-layer is formed, including: Starting from a first end of the preset area along a preset moving direction, using a laser line to sequentially move and irradiate the preset area until a second end of the preset area along the preset moving direction; After each irradiation and cooling, a laser strengthening sub-area corresponding to the laser line irradiation area can be formed in the preset area, and in the first direction, adjacent laser strengthening sub-areas have overlapping areas; A plurality of the laser-enhanced sub-regions form the enhanced sub-layer; and the region not irradiated by the laser forms the basic sub-layer.

13. The method for preparing a cover plate according to claim 11, characterized in that: The preset area includes: a bending area; The method comprises: irradiating at least one preset area of ​​the ultra-thin glass with a laser so that the ultra-thin glass in the preset area is melted under the action of the laser; cooling the ultra-thin glass after the laser irradiation so that the ultra-thin glass in the preset area is formed into the strengthening sublayer; and forming the remaining part of the ultra-thin glass into the basic sublayer, thereby forming the ultra-thin glass layer including the basic sublayer and the strengthening sublayer, comprising: Using laser to irradiate the bending area of ​​the ultra-thin glass, so that the ultra-thin glass in the bending area is melted under the action of the laser; cooling the ultra-thin glass after laser irradiation, so that the ultra-thin glass in the bending area is formed into the strengthening sublayer; the remaining part of the ultra-thin glass is formed into the basic sublayer, forming the ultra-thin glass layer including the basic sublayer and the strengthening sublayer; The method of preparing the cover plate further includes: preparing a protective layer on the ultra-thin glass layer.

14. The method for preparing a cover plate according to claim 13, characterized in that: The method further comprises: irradiating at least one preset area of ​​the ultra-thin glass with a laser so that the ultra-thin glass in the preset area is melted under the action of the laser; cooling the ultra-thin glass after the laser irradiation so that the ultra-thin glass in the preset area is formed into the strengthening sublayer; The remaining part of the ultra-thin glass is formed as the base sub-layer, and before the ultra-thin glass layer including the base sub-layer and the strengthening sub-layer is formed, the method further includes: Performing a patterning process on the bending area of ​​the ultra-thin glass to form a groove; The strengthening sublayer is formed in the groove.

15. A display panel, characterized in that: include: The cover plate according to any one of claims 1 to 10, and a polarizing layer, a light-emitting layer and a supporting layer arranged in sequence in a direction away from the cover plate.

16. A display device, characterized in that: Includes the display panel as claimed in claim 15.