Epoxy-polyvinyl alcohol-epoxy iodine polarizer and preparation method thereof

By using the preparation method of epoxy-polyvinyl alcohol-epoxy iodine polarizer in electronic display, the problem of PVA polarizer is easily deformed and has low intensity in humid and heat environments, and high mechanical properties and moisture barrier properties are achieved. Reduces production costs and is suitable for industrial applications.

CN118895007APending Publication Date: 2024-11-05HUAQIAO UNIVERSITY +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410935889.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The existing polarizers are prone to deform and shrink in humid and hot environments. The PVA polarizer has a low intensity and is easily broken, which makes it difficult to use in electronic displays. The process cost of alternative materials is high, making it difficult to meet the requirements of mechanical strength and optical performance.

Method used

Using the preparation method of epoxy-polyvinyl alcohol-epoxy iodine polarizer, the epoxy resin is mixed with a cationic initiator and cured in an ultraviolet curing box to form a three-way network structure coating, which is directly compounded in PVA On the polarizing film, avoid high temperature and high pressure conditions, and improve mechanical properties and moisture barrier properties.

Benefits of technology

It realizes the formation of a polarizer with high mechanical properties under normal temperature and pressure, has good light transmittance and humidity resistance, reduces production costs, and is suitable for industrial mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895007A_ABST
    Figure CN118895007A_ABST
Patent Text Reader

Abstract

The invention discloses an epoxy-polyvinyl alcohol-epoxy iodine system polaroid and a preparation method of the epoxy-polyvinyl alcohol-epoxy iodine system polaroid. The preparation method comprises the following steps: (1) stirring and mixing epoxy resin and a cationic initiator in a mass ratio of 100: (1-5), and removing bubbles to obtain a mixed solution; (2) coating one surface of an iodine polarizing film with the mixed solution, carrying out ultraviolet curing in an ultraviolet curing box, then coating the other surface of the iodine polarizing film with the mixed solution, and carrying out ultraviolet curing to obtain an epoxy-polyvinyl alcohol-epoxy iodine polarizer; wherein the power of the ultraviolet light in the ultraviolet light curing is 1000 to 4000 W, and the illumination time is 30 to 90 seconds. The first epoxy resin coating and the second epoxy resin coating serve as protection and supporting films of the PVA polarizing film, the hydrophobic performance of the polaroid can be greatly improved, the epoxy resin has good light transmittance, and the light transmittance of the prepared polaroid is excellent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electronic display, and in particular relates to an epoxy-polyvinyl alcohol-epoxy iodine polarizer and a preparation method thereof. Background Art

[0002] Polarizer is a key material in the electronic display industry, mainly composed of PVA polarizing film, TAC film, pressure-sensitive adhesive, release film and protective film. The manufacturing technology of TAC film, which accounts for more than half of the cost of polarizer, is mainly from Japanese manufacturers. The technical barriers of each film layer of polarizer are high and difficult to break. Iodine-based polarizer is the most widely used polarizer. Since PVA film is easy to absorb water, it will quickly deform, shrink and relax in a hot and humid environment after stretching. When the temperature and humidity are slightly high, iodine is easy to volatilize, causing the PVA polarizing film to fade and the polarization performance to decline. In addition, the strength of PVA polarizing film is very low, and it is brittle and easy to break, which is not convenient for subsequent use and processing.

[0003] In order to solve the above problems, the existing technology usually uses other materials to replace TAC film, but materials that meet the corresponding mechanical strength and optical properties often require additional production lines, which increases a lot of cost investment. In addition, in terms of technology, the replacement materials are often combined with PVA polarizing film and optical compensation film to prepare polarizer base film materials by melting materials or pressure-sensitive adhesives combined with lamination. The required high temperature and high pressure conditions will damage the PVA polarizing film. Therefore, how to select suitable alternative materials and processes to solve the problem of deformation and shrinkage of polarizing films, and ensure that polarizers have good moisture barrier properties, moisture and heat resistance, and mechanical strength is the key to related industries. Summary of the invention

[0004] The purpose of the present invention is to overcome the deficiencies of the prior art and provide an epoxy-polyvinyl alcohol-epoxy iodine based polarizer and a preparation method thereof, thereby solving the problems in the above-mentioned background technology.

[0005] One of the technical solutions adopted by the present invention to solve the technical problem is: a method for preparing an epoxy-polyvinyl alcohol-epoxy iodine polarizer is provided, comprising the following steps:

[0006] (1) mixing epoxy resin and cationic initiator at a mass ratio of 100:1 to 5, and removing bubbles to obtain a mixed solution;

[0007] (2) coating the mixed solution on one side of an iodine-based polarizing film, and curing the film by ultraviolet light in an ultraviolet curing box, and then coating the mixed solution on the other side of the iodine-based polarizing film, and curing the film by ultraviolet light to obtain an epoxy-polyvinyl alcohol-epoxy iodine-based polarizing film; wherein the power of the ultraviolet light in the ultraviolet light curing is 1000 to 4000 W, and the illumination time is 30 to 90 seconds.

[0008] In a preferred embodiment of the present invention, the epoxy resin includes bisphenol A epoxy resin, glycerol epoxy resin or aliphatic epoxy resin.

[0009] In a preferred embodiment of the present invention, the cationic initiator includes 6976 initiator, 6990 initiator or 250 initiator.

[0010] In a preferred embodiment of the present invention, the coating method is spin coating, spray coating, scraper coating, brush coating, dip coating, roller coating or slit coating.

[0011] In a preferred embodiment of the present invention, the debubbling method is static debubbling, heating debubbling, vacuum debubbling or solder paste agitator debubbling.

[0012] In a preferred embodiment of the present invention, the iodine-based polarizing film includes a PVA film on which iodine molecules are adsorbed.

[0013] The second technical solution adopted by the present invention to solve the technical problem is: providing an epoxy-polyvinyl alcohol-epoxy iodine based polarizer, which is prepared by the above method.

[0014] In a preferred embodiment of the present invention, the first epoxy resin coating, the iodine-based polarizing film, and the second epoxy resin coating are arranged in order from top to bottom.

[0015] In a preferred embodiment of the present invention, the first epoxy resin coating and the second epoxy resin coating have a three-dimensional network structure.

[0016] In a preferred embodiment of the present invention, the thickness of the first epoxy resin coating is 5-100 μm, and the thickness of the second epoxy resin coating is 5-100 μm.

[0017] In a preferred embodiment of the present invention, the thickness of the iodine-based polarizing film is 5-50 μm.

[0018] Compared with the background technology, this technical solution has the following advantages:

[0019] 1. The epoxy resin used in the present invention has two production methods: liquid and solid. Under the action of a cationic photoinitiator, the epoxy resin can undergo a cross-linking reaction at room temperature to form an insoluble, infusible polymer with a three-dimensional network structure. The epoxy resin has good adhesion and flexibility. The epoxy resin can be directly compounded on the PVA polarizing film by light curing at room temperature and pressure, thereby replacing the application of TAC film and pressure-sensitive adhesive in polarizers. The required curing time is short and the preparation method is simple, effectively avoiding damage to the PVA polarizing film under high temperature and high pressure conditions;

[0020] 2. The epoxy-polyvinyl alcohol-epoxy iodine polarizer of the present invention comprises a three-layer structure from top to bottom. The three-dimensional mesh structure inside the epoxy resin coating on the upper and lower surfaces ensures its mechanical properties as a supporting film. The upper and lower coating methods also provide sufficient protection for the iodine-based polarizer. The overall polarizer has good mechanical properties, moisture barrier properties and moisture and heat resistance while ensuring good light transmittance: The water vapor permeability of the epoxy-polyvinyl alcohol-epoxy iodine polarizer provided by the present invention is 16.21-44.03 g / (m 2 24h), light transmittance is higher than 42%;

[0021] 3. The raw materials of the present invention are cheap, the preparation method is simple, the cost is low, and it is easy to realize industrial mass production, and it has good application prospects in the field of electronic display. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a comparison chart of the film structure of traditional iodine-based polarizers and epoxy-polyvinyl alcohol-epoxy-iodine-based polarizers;

[0023] Figure 2 The figure is a flow chart for preparing epoxy-polyvinyl alcohol-epoxy iodine based polarizer;

[0024] Figure 3 is the water vapor transmission of the polarizers of Examples 1 to 3 and Comparative Example 1;

[0025] Figure 4 It is the light transmittance of the polarizers of Examples 1 to 3 and Comparative Example 1. DETAILED DESCRIPTION

[0026] In the following embodiments, the source of the PVA polarizing film is commercially available, and the thickness of the PVA polarizing film is preferably 20 to 50 μm, and more preferably 25 to 40 μm. The PVA polarizing film is pretreated before the mixed solution is coated, and the pretreatment is preferably: wiping the surface of the PVA polarizing film with anhydrous ethanol. The coating is preferably one or more of spin coating, spray coating, scraper coating, brush coating, dip coating, roller coating and slit coating. The power of ultraviolet light in photocuring is 1000 to 4000 W, and more preferably 3000 to 4000 W; the illumination time is 30 to 90 s, and more preferably 30 to 60 s.

[0027] It should be noted that the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance.

[0028] The epoxy-polyvinyl alcohol-epoxy iodine polarizer and the preparation method thereof provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0029] Example 1

[0030] The present embodiment provides a method for preparing an epoxy-polyvinyl alcohol-epoxy iodine based polarizer, comprising the following steps:

[0031] (1) 6002 bisphenol A epoxy resin and cationic photoinitiator 6979 (Shanghai Yinchang New Materials Co., Ltd.) were mixed and stirred at a mass ratio of 100:5 to remove bubbles in the resin;

[0032] (2) Wipe the surface of the PVA polarizing film (25 μm, Xiang Fuxing Technology Co., Ltd.) with anhydrous ethanol and dry it;

[0033] The epoxy resin was coated on one side of the PVA polarizing film, and was irradiated in a UV curing box for 30 seconds for UV curing. Then, the mixed solution was coated on the other side of the PVA polarizing film, and the same light curing steps were performed to obtain an epoxy-polyvinyl alcohol-epoxy iodine polarizer.

[0034] The epoxy-polyvinyl alcohol-epoxy iodine polarizer prepared in this embodiment is arranged from top to bottom as a first epoxy resin coating, a PVA polarizing film, and a second epoxy resin coating, wherein the first and second epoxy resin coatings have a three-dimensional mesh structure, so that they have good mechanical support performance. The thickness of the first and second epoxy resin coatings is measured by a thickness gauge to be 10 μm. The water vapor permeability of the epoxy-polyvinyl alcohol-epoxy iodine polarizer is measured by a water vapor permeability tester (38° C., 90% RH) to be 16.21 g / (m 2 ·24h).

[0035] Example 2

[0036] The difference between this embodiment and embodiment 1 is that:

[0037] (1) 6002 bisphenol A epoxy resin and cationic photoinitiator 6979 (Shanghai Yinchang New Materials Co., Ltd.) were mixed and stirred at a mass ratio of 100:3 to remove bubbles in the resin;

[0038] (2) Wipe the surface of the PVA polarizing film (25 μm, Xiang Fuxing Technology Co., Ltd.) with anhydrous ethanol and dry it;

[0039] The epoxy resin was coated on one side of the PVA polarizing film, and was irradiated in a UV curing box for 40 seconds for UV curing. Then, the mixed solution was coated on the other side of the PVA polarizing film, and the same light curing steps were performed to obtain an epoxy-polyvinyl alcohol-epoxy iodine polarizer.

[0040] The thickness of the epoxy resin coating was measured by a thickness gauge to be 30 μm, and the water vapor permeability of the epoxy-polyvinyl alcohol-epoxy iodine polarizer was measured by a water vapor permeability tester (38°C, 90% RH) to be 20.41 g / (m 2 ·24h).

[0041] Example 3

[0042] The difference between this embodiment and embodiment 1 is that:

[0043] (1) 6002 bisphenol A epoxy resin and cationic photoinitiator 6979 (Shanghai Yinchang New Materials Co., Ltd.) were mixed and stirred at a mass ratio of 100:1 to remove bubbles in the resin;

[0044] (2) Wipe the surface of the PVA polarizing film (25 μm, Xiang Fuxing Technology Co., Ltd.) with anhydrous ethanol and dry it;

[0045] The epoxy resin was coated on one side of the PVA polarizing film, and was irradiated in a UV curing box for 60 seconds for UV curing. Then, the mixed solution was coated on the other side of the PVA polarizing film, and the same light curing steps were performed to obtain an epoxy-polyvinyl alcohol-epoxy iodine polarizer.

[0046] The thickness of the epoxy resin coating was measured by a thickness gauge to be 60 μm, and the water vapor permeability of the epoxy-polyvinyl alcohol-epoxy iodine polarizer was measured by a water vapor permeability tester (38°C, 90% RH) to be 44.03 g / (m 2 ·24h).

[0047] Comparative Example 1

[0048] This comparative example uses a commercially available iodine-based polarizer (25 μm, Xiang Fuxing Technology Co., Ltd.), wipes the surface with anhydrous ethanol and air-dries it, and measures the water vapor permeability of the commercially available polarizer using a water vapor permeability tester (38°C, 90% RH) to be 72.55 g / (m 2 ·24h).

[0049] The water vapor transmission rates of the polarizers of Examples 1 to 3 and Comparative Example 1 are as follows: Figure 3 As shown, the transmittance is Figure 4 As shown, the transmittance is tested by UV-visible spectrophotometer. Figure 3 and Figure 4 It can be seen that the light transmittance of the epoxy-polyvinyl alcohol-epoxy iodine based polarizer provided by the present invention is almost the same as that of commercially available polarizers, the water vapor permeability is lower than that of commercially available polarizers, and the water-proof performance is more excellent.

[0050] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some or all of the technical features thereof may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing an epoxy-polyvinyl alcohol-epoxy iodine polarizer, characterized in that: The steps include: (1) mixing epoxy resin and cationic initiator at a mass ratio of 100:1 to 5, and removing bubbles to obtain a mixed solution; (2) coating the mixed solution on one side of an iodine-based polarizing film, and curing the film by ultraviolet light in an ultraviolet curing box, and then coating the mixed solution on the other side of the iodine-based polarizing film, and curing the film by ultraviolet light to obtain an epoxy-polyvinyl alcohol-epoxy iodine-based polarizing film; wherein the power of the ultraviolet light in the ultraviolet light curing is 1000 to 4000 W, and the illumination time is 30 to 90 seconds.

2. The method for preparing an epoxy-polyvinyl alcohol-epoxy iodine polarizer according to claim 1, characterized in that: The epoxy resin includes bisphenol A epoxy resin, glycerol epoxy resin or aliphatic epoxy resin.

3. The method for preparing an epoxy-polyvinyl alcohol-epoxy iodine polarizer according to claim 1, characterized in that: The cationic initiator includes 6976 initiator, 6990 initiator or 250 initiator.

4. The method for preparing an epoxy-polyvinyl alcohol-epoxy iodine polarizer according to claim 1, characterized in that: The coating method is spin coating, spray coating, blade coating, brush coating, dip coating, roller coating or slit coating.

5. The method for preparing an epoxy-polyvinyl alcohol-epoxy iodine polarizer according to claim 1, characterized in that: The debubbling method includes static debubbling, heating debubbling, vacuum debubbling or solder paste agitator debubbling.

6. The method for preparing an epoxy-polyvinyl alcohol-epoxy iodine polarizer according to claim 1, characterized in that: The iodine-based polarizing film includes a PVA film on which iodine molecules are adsorbed.

7. An epoxy-polyvinyl alcohol-epoxy iodine polarizer, characterized in that: The method is prepared by the method according to any one of claims 1 to 6.

8. The epoxy-polyvinyl alcohol-epoxy iodine based polarizer according to claim 7, characterized in that: From top to bottom, they are arranged in sequence as follows: a first epoxy resin coating, an iodine-based polarizing film, and a second epoxy resin coating.

9. The epoxy-polyvinyl alcohol-epoxy iodine polarizer according to claim 8, characterized in that: The first epoxy resin coating and the second epoxy resin coating have a three-dimensional network structure.

10. The epoxy-polyvinyl alcohol-epoxy iodine polarizer according to claim 8, characterized in that: The thickness of the first epoxy resin coating is 5 to 100 μm, and the thickness of the second epoxy resin coating is 5 to 100 μm.

11. The epoxy-polyvinyl alcohol-epoxy iodine polarizer according to claim 8, characterized in that: The thickness of the iodine-based polarizing film is 5 to 50 μm.