Fluorine conjugated structure nano-modified pressure-resistant reinforced epoxy glass fiber composite material
The composite of nanoepoxy resin and glass fiber cloth through fluorine conjugated structure is solved, and the defect rate and electrical performance of traditional insulating pull rod materials are significantly improved, which is suitable for the material's AC breakdown field strength and dielectric strength. Advanced gas insulated switch cabinet.
Patent Information
- Application Number
- CN202410995286.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-05
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The insulated pull rods of traditional glass fiber epoxy composites have high defect rate and failure rate in terms of mechanical strength and electrical properties, especially the agglomeration of nanofillers and the poor compatibility of glass fiber cloth with epoxy substrates, resulting in dielectric properties. decline.
Nanoepoxy resin modified with fluorine-conjugated structure and glass fiber cloth composite material is enhanced by nano-inorganic powder surface modification and ultrasonic dispersion technology, combining silane coupling agent and fluorine-conjugated modifier to enhance the dispersion and compatibility of the material. , a pressure-reinforced epoxy glass fiber composite material with nanomodified fluorine conjugated structure was prepared.
It significantly improves the AC breakdown field strength and dielectric strength of the material, reduces the defect rate and failure rate, improves the mechanical and electrical performance of the insulated pull rod, and is suitable for higher grade gas insulated switch cabinets.
Smart Images

Figure HDA0004959982300000011
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electrical components and relates to a fluorine conjugated structure nano-modified pressure-resistant reinforced epoxy glass fiber composite material and a preparation method thereof. Background Art
[0002] Sulfur hexafluoride (SF6) circuit breakers are key components in power transmission and transformation equipment, and high-performance insulating rods are the core components. Glass fiber insulating rods are widely used in gas insulated switchgear (GIS) with voltage levels of 110kV and above. Their design features are slenderness, frequent breaking operations, and great mechanical force and impact vibration. Therefore, they are required to have excellent electrical properties and mechanical strength. Insulating rods made of traditional glass fiber epoxy composites have certain defect rates and failure rates in production and actual operation, and the product qualification rate and operation reliability need to be improved. In order to improve the thermal conductivity and dielectric properties of epoxy composites, adding inorganic fillers to the epoxy resin matrix of insulating rods is a common method. Compared with traditional micron-filled epoxy resin composites, nano-epoxy composites are more superior in electrical properties. However, due to the large specific surface area and high surface activity of nano-fillers, they are prone to agglomeration during the material preparation process, which directly affects the breakdown performance and dielectric properties of insulating rods. On the other hand, the poor compatibility of glass fiber cloth with epoxy matrix exacerbates the decrease in the overall dielectric strength of the material. Summary of the invention
[0003] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a fluorine-conjugated structure nano-modified pressure-resistant reinforced epoxy glass fiber composite material to solve the problems of defect rate and failure rate, poor electrical comprehensive performance, etc. of traditional insulating pull rod materials.
[0004] In order to solve the above technical problems, the present invention adopts the following technical solutions to achieve the above problems:
[0005] A fluorine conjugated structure nano-modified pressure-resistant reinforced epoxy glass fiber composite material, the composite material is made of glass fiber cloth and a fluorine conjugated structure modified nano-epoxy resin composite material, the fluorine conjugated structure modified nano-epoxy resin composite material comprises the following raw materials: epoxy resin, curing agent, accelerator, toughening agent, nano inorganic powder, fluorine conjugated modifier, initiator, silane coupling agent.
[0006] The present invention also includes the following technical features:
[0007] Specifically, the fluorine conjugated structure modified nano epoxy resin composite material includes the following raw materials in parts by weight: 100 parts of epoxy resin, 85 parts of curing agent, 10 parts of accelerator, 0.5 parts of toughening agent, 0.5-10 parts of nano inorganic powder, 0.01-10 parts of fluorine conjugated modifier, 0.01-1 parts of initiator, and 0.1-1 parts of silane coupling agent.
[0008] Specifically, the glass fiber cloth has a density of 10 to 20 strands / cm in the warp direction and 10 to 20 strands / cm in the weft direction, and its surface is modified by a silane coupling agent.
[0009] Specifically, the epoxy resin is a bisphenol A type glycidyl ether epoxy resin with an epoxy equivalent of 185 to 192q / eq; the curing agent is methyltetrahydrophthalic anhydride; the accelerator is dimethylbenzylamine; the toughening agent is nitrile rubber; the initiator is selected from dibenzoyl peroxide and azobisisobutyronitrile; and the silane coupling agent is γ-aminopropyltriethoxysilane.
[0010] Specifically, the nano inorganic powder is selected from silicon oxide, aluminum oxide, titanium oxide, cerium oxide, zirconium oxide, samarium oxide, antimony oxide, tin oxide, aluminum cerium oxide, and indium tin oxide;
[0011] The fluorine conjugated modifier is selected from styrene, 4-fluorostyrene, 1-fluoro-4-(isopropenyl)benzene, 2,4-difluoro-1-vinylbenzene, 2-fluorostyrene, 3-fluorostyrene, 4-fluorostyrene, 3,4-difluorostyrene, 1,3-difluoro-2-vinylbenzene, 2,4-difluoro-1-vinylbenzene, 2,3,4-trifluorostyrene, 3,4,5-trifluorostyrene, 1-vinylnaphthalene, 2-vinylnaphthalene, 2-isopropylphenylnaphthalene, and vinylanthracene.
[0012] The method for preparing the fluorine-conjugated structure nano-modified pressure-resistant reinforced epoxy glass fiber composite material comprises the following steps:
[0013] Step 1, preparation of fluorine conjugated structure modified nanopowder: fully mix nano inorganic powder and silane coupling agent, and disperse nano particles by high energy ultrasound to obtain nano inorganic filler with preliminary surface modification of coupling agent, and heat it to 60-80° C. in a solvent environment, add initiator and fluorine conjugated modifier, then remove the solvent, and place in a vacuum oven to dry to obtain fluorine conjugated structure modified nano powder;
[0014] Step 2, prefabrication of fluorine conjugated structure modified nanopowder and epoxy resin composite material: epoxy resin, curing agent, accelerator, toughening agent and fluorine conjugated structure modified nanopowder are fully mixed;
[0015] Step 3, dispersion of fluorine conjugated structure modified nanopowder in epoxy resin: stirring and dispersing the pre-prepared epoxy resin composite material containing fluorine conjugated structure modified nanopowder obtained in step 2 uniformly, and then ultrasonicating, and obtaining a suspension after sufficient ultrasonication, and placing the obtained suspension in a vacuum drying oven for vacuum degassing;
[0016] Step 4, preparation of glass fiber reinforced epoxy nanocomposite sheet: cutting glass fiber cloth and removing moisture therein in a drying oven, applying a layer of epoxy resin composite material obtained in step 3 on the flat substrate, stacking the glass fiber cloth in a manner of applying a layer of epoxy resin composite material for each layer of glass fiber cloth, and then applying a layer of epoxy resin composite material on the surface of the top glass fiber cloth, placing the obtained multilayer structure in an oven for pre-curing, and then placing it in a hot press for curing and post-curing, and finally obtaining a fluorine-conjugated structure nano-modified pressure-resistant reinforced epoxy glass fiber composite material.
[0017] Specifically, in the step 1, the nano inorganic powder is dried at 70° C. for 6 to 24 hours before use; the ultrasonic power in step 1 is 350 to 400 W, the ultrasonic time for each time is 1 to 2 seconds, the ultrasonic interval is 1 to 2 seconds, and the cumulative time of the entire ultrasonic process is 90 to 120 minutes; the vacuum oven is maintained at a vacuum degree of 0.1 atmosphere at room temperature for 6 to 24 hours.
[0018] Specifically, in step 3, the temperature during vacuum degassing is 60° C., the vacuum degree is increased step by step, the maximum stable vacuum degree is 0.1 atmosphere, and the stable bubble-free time is 10 minutes.
[0019] Specifically, in step 4, the thickness of the glass fiber cloth is 0.16-0.20 mm; the moisture of the glass fiber cloth is removed in a drying oven, the drying temperature is 60-80° C., and the drying time is 6-24 hours.
[0020] Specifically, in step 4, the pre-curing temperature is 60-100°C, and the pre-curing time is 1-6 hours; the curing is carried out under a pressure of 10 MPa, the curing temperature is 80°C-150°C, and the curing time is 1-24 hours; the post-curing is carried out under a pressure of 10 MPa, the curing temperature is 130°C-200°C, and the post-curing time is 0.5-4 hours.
[0021] Compared with the prior art, the present invention has the following technical effects:
[0022] The fluorine-conjugated structure nano-modified pressure-resistant reinforced epoxy glass fiber composite material provided by the present invention can reduce the defect rate and failure rate of traditional glass fiber epoxy insulating rods caused by electrical breakdown. The epoxy glass fiber composite material with surface fluorine-conjugated structure grafted and modified nano inorganic powder prepared by this method has significantly improved AC breakdown field strength compared with traditional epoxy glass fiber composite materials for insulating rods.
[0023] The invention provides a method for preparing a pressure-resistant reinforced epoxy glass fiber composite material modified with a fluorine conjugated structure nanometer. The method comprises adding a certain mass ratio of surface fluorine conjugated structure grafted modified nanometer inorganic powder into an epoxy matrix of the glass fiber epoxy composite material, thereby enhancing the fusion of the glass fiber and the epoxy resin, strengthening the dispersibility of the nanometer inorganic particles in the epoxy resin, and finally improving the dielectric strength of the material. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 Weibull distribution diagram of AC breakdown field strength of composite insulation material. DETAILED DESCRIPTION
[0025] The present invention provides a fluorine conjugated structure nano-modified pressure-resistant reinforced epoxy glass fiber composite material, wherein an inorganic nano filler is grafted and modified with a surface fluorine conjugated structure and introduced into a glass fiber-reinforced epoxy composite material, and the strong electrophilicity of the fluorine conjugated structure is utilized to improve the breakdown strength and dielectric properties of the insulating pull rod of a high-voltage switch; the material can be applied to higher-level gas-insulated switchgear to promote the miniaturization and integration of the switchgear, and has broad economic and social value.
[0026] By grafting fluorine conjugated groups on the surface of the filler, the compatibility between the filler, the resin matrix and the glass fiber cloth can be effectively regulated, thereby significantly improving the compressive strength. This surface modification can not only improve the dispersion of the filler in the matrix, but also enhance the overall performance of the composite material. Therefore, the fluorine conjugated grafting modification of nanofillers and the glass fiber toughened epoxy composite materials and their preparation methods have become a hot topic.
[0027] The fluorine conjugated structure nano-modified pressure-resistant reinforced epoxy glass fiber composite material of the present invention is made of glass fiber cloth and fluorine conjugated structure modified nano-epoxy resin composite material, and the fluorine conjugated structure modified nano-epoxy resin composite material includes the following raw materials: epoxy resin, curing agent, accelerator, toughening agent, nano inorganic powder, fluorine conjugated modifier, initiator, and silane coupling agent. The fluorine conjugated structure modified nano-epoxy resin composite material, by weight, includes the following raw materials: 100 parts of epoxy resin, 85 parts of curing agent, 10 parts of accelerator, 0.5 parts of toughening agent, 0.5-10 parts of nano inorganic powder, 0.01-10 parts of fluorine conjugated modifier, 0.01-1 parts of initiator, and 0.1-1 parts of silane coupling agent.
[0028] The density of the glass fiber cloth in the warp direction is 10 to 20 strands / cm, the density in the weft direction is 10 to 20 strands / cm, and the surface is modified by a silane coupling agent.
[0029] The epoxy resin is a bisphenol A type glycidyl ether epoxy resin with an epoxy equivalent of 185 to 192 q / eq.
[0030] The curing agent is methyltetrahydrophthalic anhydride, with a boiling point of 115-155° C., a viscosity of 40-80 mPa·s at 25° C., anhydride content of ≥40%, and can be dissolved in acetone, ethanol and toluene solvents.
[0031] The accelerator is dimethylbenzylamine, a colorless to slightly yellow transparent liquid with a viscosity of 90 mPa·s at 25°C and a density of 0.897 g / cm at 25°C. 3 , boiling range 178 ~ 184 ℃ or 70 ~ 72 ℃ / kPa, soluble in ethanol, ether and other solvents.
[0032] The toughening agent is nitrile rubber.
[0033] The initiator is selected from dibenzoyl peroxide and azobisisobutyronitrile.
[0034] The silane coupling agent is γ-aminopropyltriethoxysilane (brand number KH550).
[0035] The nano inorganic powder is selected from silicon oxide, aluminum oxide (α-type nano Al2O3), titanium oxide, cerium oxide, zirconium oxide, samarium oxide, antimony oxide, tin oxide, aluminum cerium oxide, indium tin oxide, with a particle size of 5nm to 500nm and a purity of 95% to 99.9%.
[0036] The fluorine conjugated modifier is selected from styrene, 4-fluorostyrene, 1-fluoro-4-(isopropenyl)benzene, 2,4-difluoro-1-vinylbenzene, 2-fluorostyrene, 3-fluorostyrene, 4-fluorostyrene, 3,4-difluorostyrene, 1,3-difluoro-2-vinylbenzene, 2,4-difluoro-1-vinylbenzene, 2,3,4-trifluorostyrene, 3,4,5-trifluorostyrene, 1-vinylnaphthalene, 2-vinylnaphthalene, 2-isopropylphenylnaphthalene, and vinylanthracene.
[0037] The method for preparing the fluorine-conjugated structure nano-modified pressure-resistant reinforced epoxy glass fiber composite material of the present invention comprises the following steps:
[0038] Step 1, preparation of fluorine conjugated structure modified nano powder: fully mix nano inorganic powder and silane coupling agent, and disperse nano particles by high energy ultrasound to obtain nano inorganic filler with preliminary surface modification of coupling agent, and heat it to 60-80℃ in solvent (butanone, etc.), add initiator and fluorine conjugated modifier, remove solvent, and dry in vacuum oven to obtain fluorine conjugated structure modified nano powder. Nano inorganic powder is dried at 70℃ for 6-24h before use; ultrasonic power is 350-400W, ultrasonic time is 1-2s each time, ultrasonic interval is 1-2s, and the total time of the whole ultrasonic process is 90-120min; vacuum oven is kept at 0.1 atmosphere at room temperature for 6-24h.
[0039] Step 2, prefabrication of fluorine-conjugated structure modified nanopowder and epoxy resin composite material: epoxy resin, curing agent, accelerator, toughening agent and fluorine-conjugated structure modified nanopowder are fully mixed.
[0040] Step 3, dispersion of fluorine conjugated structure modified nanopowder in epoxy resin: the pre-prepared epoxy resin composite material containing fluorine conjugated structure modified nanopowder obtained in step 2 is stirred and dispersed uniformly, and then ultrasonicated, and a suspension is obtained after sufficient ultrasonication, and the obtained suspension is placed in a vacuum drying oven for vacuum degassing. The temperature during vacuum degassing is 60°C, and the vacuum degree is gradually increased, the maximum stable vacuum degree is 0.1 atmosphere, and the stable bubble-free time is 10 minutes.
[0041] Step 4, preparation of glass fiber toughened epoxy nanocomposite sheet: cutting glass fiber cloth and removing moisture from it in a drying oven, applying a layer of epoxy resin composite material obtained in step 3 on the flat substrate, stacking glass fiber cloth in a manner of coating a layer of epoxy resin composite material for each layer of glass fiber cloth, and then coating a layer of epoxy resin composite material on the surface of the top glass fiber cloth, placing the obtained multilayer structure in an oven for pre-curing, and then placing it in a hot press for curing and post-curing, and finally obtaining a fluorine conjugated structure nano-modified pressure-resistant reinforced epoxy glass fiber composite material. The thickness of the glass fiber cloth is 0.16 to 0.20 mm; the moisture of the glass fiber cloth is removed in a drying oven, the drying temperature is 60 to 80°C, and the drying time is 6 to 24 hours. The pre-curing temperature is 60-100°C, and the pre-curing time is 1-6h; the curing is carried out under a pressure of 10MPa, the curing temperature is 80°C-150°C, and the curing time is 1-24h; the post-curing is carried out under a pressure of 10MPa, the curing temperature is 130°C-200°C, and the post-curing time is 0.5-4h.
[0042] Specific embodiments of the present invention are given below. It should be noted that the present invention is not limited to the following specific embodiments, and all equivalent changes made on the basis of the technical solution of this application fall within the protection scope of the present invention.
[0043] Embodiment 1:
[0044] This embodiment provides a fluorine-conjugated structure nano-modified pressure-resistant reinforced epoxy glass fiber composite material, and the preparation method thereof comprises the following steps:
[0045] 1.955g of α-type nano-Al2O3 particles and 0.0391g of silane coupling agent were stirred and dispersed uniformly in 20ml of anhydrous ethanol environment solution at 60°C. The obtained mixed solution was ultrasonically dispersed, and the total time of ultrasonic dispersion was 120min, wherein each ultrasonic wave lasted for 1s, the ultrasonic interval was 2s, and the ultrasonic power was 400W. After that, the precipitate was washed with ethanol several times, and then soaked in anhydrous ethanol for 24h and vacuum dried in a vacuum drying oven for 24h. The dry powder was placed in a solvent of 20ml of butanone, mixed and heated to 60-80°C, and 50mg of azobisisobutyronitrile and 1.955mg of styrene were added and reacted for 3h. After the reaction, the butanone was removed and the powder was dried in a vacuum oven to obtain a fluorine-conjugated structure-modified nanopowder.
[0046] 100 g of bisphenol A glycidyl ether epoxy resin, 85 g of anhydride curing agent methyltetrahydrophthalic anhydride (MeTHPA), 10 g of accelerator dimethylbenzylamine and 0.5 g of toughening agent nitrile rubber were added to the obtained nano powder.
[0047] The mixture was fully mixed at 60°C and stirred evenly. The obtained mixed solution was subjected to ultrasonic dispersion, and the total time of ultrasonic dispersion was 120 minutes, wherein each ultrasonic wave lasted for 1 second, the ultrasonic interval was 2 seconds, and the ultrasonic power was 400W. The suspension obtained after sufficient ultrasonic treatment was placed in a vacuum drying oven, the oven temperature was 60°C, and the vacuum degree in the vacuum drying oven was gradually increased from 1 standard atmospheric pressure until the air pressure in the drying oven dropped to 0.1 atmospheric pressure, and the pressure was maintained at this pressure for 10 minutes without bubbles, to obtain an epoxy resin preform containing 1wt% nano-alumina powder.
[0048] The epoxy resin preform was pre-cured at a temperature of 80°C for 4 hours, then cured at a pressure of 10 MPa and 120°C for 12 hours, and finally post-cured at a pressure of 10 MPa and 160°C for 1 hour.
[0049] Embodiment 2:
[0050] This embodiment provides a fluorine-conjugated structure nano-modified pressure-resistant reinforced epoxy glass fiber composite material, and the preparation method thereof comprises the following steps:
[0051] 1.955g of α-type nano-Al2O3 particles and 0.0391g of silane coupling agent were stirred and dispersed uniformly in 20ml of anhydrous ethanol environment solution at 60°C. The obtained mixed solution was ultrasonically dispersed, and the total time of ultrasonic dispersion was 120min, wherein each ultrasonic wave lasted for 1s, the ultrasonic interval was 2s, and the ultrasonic power was 400W. After that, the precipitate was washed with ethanol several times, and then soaked in anhydrous ethanol for 24h and vacuum dried in a vacuum drying oven for 24h. The dry powder was placed in a solvent of 20ml of butanone, mixed and heated to 60-80°C, and 50mg of azobisisobutyronitrile and 2.293mg of 4-fluorostyrene were added and reacted for 3h. After the reaction, the butanone was removed and the powder was dried in a vacuum oven to obtain a fluorine-conjugated structure-modified nanopowder.
[0052] 100 g of bisphenol A glycidyl ether epoxy resin, 85 g of anhydride curing agent methyltetrahydrophthalic anhydride (MeTHPA), 10 g of accelerator dimethylbenzylamine and 0.5 g of toughening agent nitrile rubber were added to the obtained nano powder.
[0053] The mixture was fully mixed at 60°C and stirred evenly. The obtained mixed solution was subjected to ultrasonic dispersion, and the total time of ultrasonic dispersion was 120 minutes, wherein each ultrasonic wave lasted for 1 second, the ultrasonic interval was 2 seconds, and the ultrasonic power was 400W. The suspension obtained after sufficient ultrasonic treatment was placed in a vacuum drying oven, the oven temperature was 60°C, and the vacuum degree in the vacuum drying oven was gradually increased from 1 standard atmospheric pressure until the air pressure in the drying oven dropped to 0.1 atmospheric pressure, and the pressure was maintained at this pressure for 10 minutes without bubbles, to obtain an epoxy resin preform containing 1wt% nano-alumina powder.
[0054] The epoxy resin preform was pre-cured at a temperature of 80°C for 4 hours, then cured at a pressure of 10 MPa and 120°C for 12 hours, and finally post-cured at a pressure of 10 MPa and 160°C for 1 hour.
[0055] Embodiment 3:
[0056] This embodiment provides a fluorine-conjugated structure nano-modified pressure-resistant reinforced epoxy glass fiber composite material, and the preparation method thereof comprises the following steps:
[0057] 9.775g of α-type nano-Al2O3 particles and 0.1955g of silane coupling agent were stirred and dispersed uniformly in 100ml of anhydrous ethanol environment solution at 60°C. The obtained mixed solution was ultrasonically dispersed, and the total time of ultrasonic dispersion was 120min, wherein each ultrasonic wave lasted for 1s, the ultrasonic interval was 2s, and the ultrasonic power was 400W. After that, the precipitate was washed with ethanol several times, and then soaked in anhydrous ethanol for 24h and vacuum dried in a vacuum drying oven for 24h. The dry powder was placed in a solvent of 100ml of butanone and mixed and heated to 60-80°C, and 250mg of azobisisobutyronitrile and 11.465mg of 4-fluorostyrene were added and reacted for 3h. After the reaction, the butanone was removed and the fluorine-conjugated structure-modified nanopowder was obtained by drying in a vacuum oven.
[0058] 100 g of bisphenol A glycidyl ether epoxy resin, 85 g of anhydride curing agent methyltetrahydrophthalic anhydride (MeTHPA), 10 g of accelerator dimethylbenzylamine and 0.5 g of toughening agent nitrile rubber were added to the obtained nano powder.
[0059] The mixture was fully mixed at 60°C and stirred evenly. The obtained mixed solution was subjected to ultrasonic dispersion, and the total time of ultrasonic dispersion was 120 minutes, wherein each ultrasonic wave lasted for 1 second, the ultrasonic interval was 2 seconds, and the ultrasonic power was 400W. The suspension obtained after sufficient ultrasonic treatment was placed in a vacuum drying oven, the oven temperature was 60°C, and the vacuum degree in the vacuum drying oven was gradually increased from 1 standard atmospheric pressure until the air pressure in the drying oven dropped to 0.1 atmospheric pressure, and the pressure was maintained at this pressure for 10 minutes without bubbles, to obtain an epoxy resin preform containing 1wt% nano-alumina powder.
[0060] The epoxy resin preform was pre-cured at a temperature of 80°C for 4 hours, then cured at a pressure of 10 MPa and 120°C for 12 hours, and finally post-cured at a pressure of 10 MPa and 160°C for 1 hour.
[0061] Comparative Example:
[0062] The preparation process of the composite material in this comparative example includes: adding 85g of anhydride curing agent methyltetrahydrophthalic anhydride, 10g of accelerator dimethylbenzylamine and 0.5g of toughening agent nitrile rubber to 100g of bisphenol A glycidyl ether epoxy resin. Fully mix and stir evenly at 60°C. Add 1.955g of α-type nano-Al2O3 particles and 0.0391g of silane coupling agent to the obtained prefabricated material, stir and disperse evenly at 60°C. The obtained mixed solution is ultrasonically dispersed, and the total time of ultrasonic dispersion is 120min, wherein each ultrasonic wave is 1s, the ultrasonic interval is 2s, and the ultrasonic power is 400W. The suspension obtained after sufficient ultrasonic wave is placed in a vacuum drying oven, the oven temperature is 60°C, and the vacuum degree in the vacuum drying oven is gradually increased from 1 standard atmospheric pressure until the air pressure in the drying oven drops to 0.1 atmospheric pressure, and it is kept at this pressure for 10min without bubbles to obtain an epoxy resin prefabricated material containing 1wt% nano-alumina powder. The epoxy resin preform was pre-cured at a temperature of 80°C for 4 hours, then cured at a pressure of 10 MPa and 120°C for 12 hours, and finally post-cured at a pressure of 10 MPa and 160°C for 1 hour.
[0063] Figure 1 The Weibull distribution diagram of the power frequency AC breakdown strength of the epoxy composite material. From the Weibull distribution diagram of the breakdown field strength, it can be seen that the relationship between the breakdown field strengths of the various epoxy composite insulation materials is: Comparative Example - Sample 1 < Example 2 - Sample 3 < Example 1 - Sample 2 < Example 3 - Sample 4. Figure 1 It can be seen that when 1% of the mass fraction of nanofillers is added to the epoxy composite material, the ability of the samples modified with styrene on the surface of the nanoparticles (Sample 2 of Example 1) and fluorostyrene (Sample 3 of Example 2) to withstand AC electric fields is higher than that of the sample modified with only silane coupling agent (Comparative Example Sample 1). For the epoxy composite material modified with fluorine conjugated structure nanoparticles, when the filler density is increased from 1% mass fraction (Sample 3 of Example 2) to 5% mass fraction (Sample 4 of Example 3), the ability of the material to withstand AC electric fields is further increased. The AC breakdown field strength (calculated according to the characteristic failure field strength of 63.2% of the Weibull distribution) of the epoxy composite material modified with 5% mass fraction of fluorostyrene (Sample 4 of Example 3) is increased by 20% compared with the epoxy composite material modified with only silane coupling agent (Comparative Example Sample 1).
Claims
1. A fluorine-conjugated nanostructured pressure-resistant reinforced epoxy glass fiber composite material, characterized in that: The composite material is made of glass fiber cloth and fluorine conjugated structure modified nano epoxy resin composite material. The fluorine conjugated structure modified nano epoxy resin composite material includes the following raw materials: epoxy resin, curing agent, accelerator, toughening agent, nano inorganic powder, fluorine conjugated modifier, initiator, and silane coupling agent.
2. The fluorine-conjugated structure nano-modified pressure-resistant reinforced epoxy glass fiber composite material according to claim 1, characterized in that: The fluorine conjugated structure modified nano epoxy resin composite material comprises the following raw materials in parts by weight: 100 parts of epoxy resin, 85 parts of curing agent, 10 parts of accelerator, 0.5 parts of toughening agent, 0.5-10 parts of nano inorganic powder, 0.01-10 parts of fluorine conjugated modifier, 0.01-1 parts of initiator and 0.1-1 parts of silane coupling agent.
3. The fluorine-conjugated structure nano-modified pressure-resistant reinforced epoxy glass fiber composite material according to claim 1, characterized in that: The glass fiber cloth has a density of 10 to 20 strands / cm in the warp direction and 10 to 20 strands / cm in the weft direction, and its surface is modified by a silane coupling agent.
4. The fluorine-conjugated structure nano-modified pressure-resistant reinforced epoxy glass fiber composite material according to claim 1, characterized in that: The epoxy resin is a bisphenol A type glycidyl ether epoxy resin with an epoxy equivalent of 185 to 192q / eq; the curing agent is methyltetrahydrophthalic anhydride; the accelerator is dimethylbenzylamine; the toughening agent is nitrile rubber; the initiator is selected from dibenzoyl peroxide and azobisisobutyronitrile; and the silane coupling agent is γ-aminopropyltriethoxysilane.
5. The fluorine-conjugated structure nano-modified pressure-resistant reinforced epoxy glass fiber composite material according to claim 1, characterized in that: The nano inorganic powder is selected from silicon oxide, aluminum oxide, titanium oxide, cerium oxide, zirconium oxide, samarium oxide, antimony oxide, tin oxide, aluminum cerium oxide, and indium tin oxide; The fluorine conjugated modifier is selected from styrene, 4-fluorostyrene, 1-fluoro-4-(isopropenyl)benzene, 2,4-difluoro-1-vinylbenzene, 2-fluorostyrene, 3-fluorostyrene, 4-fluorostyrene, 3,4-difluorostyrene, 1,3-difluoro-2-vinylbenzene, 2,4-difluoro-1-vinylbenzene, 2,3,4-trifluorostyrene, 3,4,5-trifluorostyrene, 1-vinylnaphthalene, 2-vinylnaphthalene, 2-isopropylphenylnaphthalene, and vinylanthracene.
6. The method for preparing the fluorine-conjugated structure nano-modified pressure-resistant reinforced epoxy glass fiber composite material according to claim 1, characterized in that: The following steps are involved: Step 1, preparation of fluorine conjugated structure modified nanopowder: fully mix nano inorganic powder and silane coupling agent, and disperse nano particles by high energy ultrasound to obtain nano inorganic filler with preliminary surface modification of coupling agent, and heat it to 60-80° C. in a solvent environment, add initiator and fluorine conjugated modifier, then remove the solvent, and place in a vacuum oven to dry to obtain fluorine conjugated structure modified nano powder; Step 2, prefabrication of fluorine conjugated structure modified nanopowder and epoxy resin composite material: epoxy resin, curing agent, accelerator, toughening agent and fluorine conjugated structure modified nanopowder are fully mixed; Step 3, dispersion of fluorine conjugated structure modified nanopowder in epoxy resin: stirring and dispersing the pre-prepared epoxy resin composite material containing fluorine conjugated structure modified nanopowder obtained in step 2 uniformly, and then ultrasonicating, and obtaining a suspension after sufficient ultrasonication, and placing the obtained suspension in a vacuum drying oven for vacuum degassing; Step 4, preparation of glass fiber reinforced epoxy nanocomposite sheet: cutting glass fiber cloth and removing moisture therein in a drying oven, applying a layer of epoxy resin composite material obtained in step 3 on the flat substrate, stacking the glass fiber cloth in a manner of applying a layer of epoxy resin composite material for each layer of glass fiber cloth, and then applying a layer of epoxy resin composite material on the surface of the top glass fiber cloth, placing the obtained multilayer structure in an oven for pre-curing, and then placing it in a hot press for curing and post-curing, and finally obtaining a fluorine-conjugated structure nano-modified pressure-resistant reinforced epoxy glass fiber composite material.
7. The method for preparing the fluorine-conjugated structure nano-modified pressure-resistant reinforced epoxy glass fiber composite material according to claim 6, characterized in that: In the step 1, the nano inorganic powder is dried at 70° C. for 6 to 24 hours before use; the ultrasonic power in step 1 is 350 to 400 W, the ultrasonic time for each time is 1 to 2 seconds, the ultrasonic interval is 1 to 2 seconds, and the cumulative time of the entire ultrasonic process is 90 to 120 minutes; the vacuum oven is maintained at a vacuum degree of 0.1 atmosphere at room temperature for 6 to 24 hours.
8. The method for preparing the fluorine-conjugated structure nano-modified pressure-resistant reinforced epoxy glass fiber composite material according to claim 6, characterized in that: In step 3, the temperature during vacuum degassing is 60° C., and the vacuum degree is gradually increased until the maximum stable vacuum degree is 0.1 atmosphere, and the stable bubble-free time is 10 minutes.
9. The method for preparing the fluorine-conjugated structure nano-modified pressure-resistant reinforced epoxy glass fiber composite material according to claim 6, characterized in that: In the step 4, the thickness of the glass fiber cloth is 0.16-0.20 mm; the moisture of the glass fiber cloth is removed in a drying oven, the drying temperature is 60-80° C., and the drying time is 6-24 hours.
10. The method for preparing the fluorine-conjugated structure nano-modified pressure-resistant reinforced epoxy glass fiber composite material according to claim 6, characterized in that: In step 4, the pre-curing temperature is 60-100°C, and the pre-curing time is 1-6 hours; the curing is carried out under a pressure of 10 MPa, the curing temperature is 80-150°C, and the curing time is 1-24 hours; the post-curing is carried out under a pressure of 10 MPa, the curing temperature is 130-200°C, and the post-curing time is 0.5-4 hours.