Super-hydrophobic fly ash-based photothermal conversion composite phase change heat storage material as well as preparation method and application thereof

The preparation of fly ash-based photothermal conversion composite phase-changing heat storage material through alkaline hydrothermal method has solved the problem of ice covering in the transmission line, and achieved efficient and low-cost anti-icing and frost-resistant effect, which is suitable for large-scale promotion.

CN118895081AActive Publication Date: 2024-11-05NORTHEAST DIANLI UNIVERSITY

Patent Information

Application Number
CN202410925533.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-05
Estimated Expiration
2044-07-11

AI Technical Summary

Technical Problem

The existing technology cannot effectively solve the ice-covering disaster of high-voltage transmission lines. The traditional mechanical deicing method is inefficient and costly. The existing photothermal conversion materials are large in size and heavy in weight, which cannot meet the lightweight requirements, and are high in cost and are not suitable for large-scale scale. Promotion.

Method used

The alkaline hydrothermal method is used to prepare fly ash alkali leaching liquid and calcium-based oxygen-containing compounds, and the carbon source is added to improve the thermal conductivity and photothermal conversion efficiency of the composite phase-change heat storage material, and is mixed and filled by vacuum impregnation or normal pressure heating. Spectral adjustment materials and phase change substances form superhydrophobic fly ash-based photothermal conversion composite phase change heat storage material.

Benefits of technology

It achieves high thermal conductivity, excellent hydrophobic performance and efficient photothermal conversion performance, is low in cost, is suitable for large-scale promotion and use, can effectively prevent transmission lines from icing and reduce the risk of damage to the power system.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895081A_ABST
    Figure CN118895081A_ABST
Patent Text Reader

Abstract

The invention discloses a super-hydrophobic fly ash-based photothermal conversion composite phase change heat storage material and a preparation method and application thereof, and belongs to the field of solid waste-based phase change energy storage materials.The preparation method comprises the steps that raw materials are weighed according to mass parts, and a carbon self-growth modified fly ash-based porous material, a spectrum adjusting material and a phase change substance are mixed through a vacuum impregnation method or normal-pressure heating; and mixing the carbon self-growth modified fly ash-based photothermal conversion composite phase change heat storage material with a hydrophobic material, stirring, and drying, so as to obtain the super-hydrophobic fly ash-based photothermal conversion composite phase change heat storage material. The defects that the composite phase change heat storage supporting material is high in preparation cost, the coal ash-based porous material is difficult to prepare, and the coal ash-based composite phase change heat storage material is low in heat conductivity are overcome.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of solid waste-based phase change energy storage materials, and in particular relates to a super-hydrophobic fly ash-based photothermal conversion composite phase change heat storage material and a preparation method and application thereof. Background Art

[0002] Icing disasters on high-voltage transmission lines seriously affect the safe and stable transportation of electricity, and are an important cause of accidents such as line breaks, tower collapses, and power grid decoupling. The currently commonly used mechanical deicing methods are labor-intensive and inefficient, and mechanical vibrations can easily cause transmission lines to break, leading to damage to the power system. Therefore, in order to improve the ability of power grids to resist ice disasters, it is urgent to develop an efficient, convenient, and economical means of preventing transmission line icing disasters. Studies have shown that hydrophobic coatings can prevent the occurrence of line icing by promoting the rapid rolling of water droplets, delaying ice nucleation, and reducing ice adhesion. However, relying solely on the hydrophobicity of the coating cannot completely prevent the formation and growth of the ice layer, and it is impossible to take effective measures on cables that have been iced.

[0003] Phase change heat storage materials, as a material that can store ambient heat and release heat when needed, have been used in anti-icing and anti-freezing. For photothermal conversion phase change heat storage materials, it can absorb solar energy and convert it into latent heat for storage; when the ambient temperature is low, it releases heat through a reversible phase change process to ensure that the temperature of the object is maintained at an appropriate level. Therefore, the development of composite phase change materials with both hydrophobicity and photothermal conversion heat storage functions for power grid transmission lines can replace traditional mechanical ice melting methods, which can effectively solve the problem of icing on transmission lines and help the power system operate safely and stably.

[0004] CN116278277A discloses a photothermal conversion bionic anti-icing / deicing functional surface, which is mainly formed by stacking an intelligent deformation layer, a photothermal conversion layer and an energy storage layer. The main principle is that the photothermal conversion layer absorbs solar heat to cause temperature changes, thereby deforming the intelligent deformation layer to achieve the ice removal effect. However, the minimum thickness of the material still reaches 2.52mm, and the maximum thickness reaches 6.1mm. Limited by factors such as the excessive volume and weight of the material, it cannot meet the requirements of lightweight transmission lines to reduce the load on transmission towers.

[0005] CN113462363A discloses a photothermal phase change energy storage super-hydrophobic antifreeze particle, which mainly improves the antifreeze effect by adding silver particles to the energy storage material to increase the thermal conductivity of the phase change material. However, silver particles are expensive and the cost of antifreeze particles is high, which is not conducive to the large-scale promotion and implementation of power grid lines.

[0006] CN116333519A discloses a fly ash-based hydrophobic coating prepared by mixing polyethylene wax with fly ash, which mainly needs to select fly ash with a particle size of 7-9 μm and polyethylene wax particles with a particle size of less than 60 meshes. After fly ash, polyethylene wax and water are mixed in proportion to prepare the hydrophobic coating, a super hydrophobic coating is prepared through the steps of mixing, drying, thermal curing, polishing, etc. The preparation method has many steps and the operation process is not easy to control. In addition, the coating is only applicable to the ice prevention stage, and the ice melting process cannot be achieved after ice formation.

[0007] As a composite phase change material suitable for power transmission lines that has both hydrophobicity and photothermal conversion and heat storage functions to prevent icing disasters, it is necessary to consider comprehensive factors such as cheap and available raw materials, simple preparation, and suitability for large-scale promotion and use in power grid lines while ensuring strong hydrophobicity, high photothermal conversion efficiency and energy storage density. Summary of the invention

[0008] The purpose of the present invention is to provide a super-hydrophobic fly ash-based photothermal conversion composite phase change heat storage material and its preparation method and application, so as to solve the problems existing in the above-mentioned prior art. The present invention uses fly ash alkali leachate and calcium-based oxygen-containing compounds as raw materials, adopts alkaline hydrothermal method to prepare the supporting skeleton of the composite phase change heat storage material, and adds carbon source in the hydrothermal process to improve the thermal conductivity and photothermal conversion efficiency of the composite material. The spectrum adjustment material and the phase change material are filled into the fly ash-based porous skeleton of carbon self-growth by vacuum impregnation or normal pressure heating and mixing, and blended with a hydrophobic material to prepare a super-hydrophobic fly ash-based photothermal conversion composite phase change heat storage material with high-efficiency spectral selectivity, photothermal conversion performance and hydrophobic performance.

[0009] One of the technical solutions provided by the present invention:

[0010] A super-hydrophobic fly ash-based photothermal conversion composite phase-change heat storage material comprises the following raw materials in parts by weight: 65-80 parts of a phase-change material, 10-32 parts of a fly ash-based porous material modified by carbon self-growth, 2-5 parts of a spectrum adjustment material and 10-15 parts of a hydrophobic material.

[0011] Preferably, the phase change material is one or more of polyethylene glycol, tetradecane, pentadecane, octanoic acid, lauric acid, stearic acid, decanoic acid, myristic acid and methyl laurate; the spectrum adjustment material is one or more of nano zinc oxide, nano titanium nitride, nano titanium dioxide, vanadium dioxide, tungsten dioxide and indium tin oxide; the hydrophobic material is one or more of polydimethylsiloxane, hexamethyldisilazane, dodecyltriethoxysilane and methyl hydrogen silicone oil.

[0012] The second technical solution provided by the present invention is:

[0013] A method for preparing a super-hydrophobic fly ash-based photothermal conversion composite phase change heat storage material comprises weighing raw materials according to parts by mass, mixing a carbon self-growth modified fly ash-based porous material, a spectrum adjustment material and a phase change material through a vacuum impregnation method or a normal pressure heating method to obtain a carbon self-growth modified fly ash-based photothermal conversion composite phase change heat storage material, and mixing, stirring and drying the carbon self-growth modified fly ash-based photothermal conversion composite phase change heat storage material and a hydrophobic material to obtain a super-hydrophobic fly ash-based photothermal conversion composite phase change heat storage material.

[0014] Preferably, the mixing temperature of the vacuum impregnation method is 60-100°C, the vacuum degree is -0.1 MPa, and the holding time is 0.5-2h; the temperature of the normal pressure heating mixing method is 60-100°C, and the holding time is 0.5-2h.

[0015] Preferably, the preparation method of the carbon self-growth modified fly ash-based porous material is: adding a calcium-based oxygen-containing compound and a carbon source to the fly ash alkaline leaching solution, mixing, obtaining a hydrothermal ligand solution, hydrothermal treatment, centrifugation, filtering, obtaining a carbon self-growth modified fly ash-based precursor solid product, and carbonization treatment to obtain a carbon self-growth modified fly ash-based porous material.

[0016] More preferably, the calcium-based oxygen-containing compound is one or more of calcium oxide, calcium hydroxide, calcium nitrate, calcium carbonate, calcium sulfate, calcium acetate, calcium phosphate and calcium dihydrogen phosphate; and the carbon source is one or more of furfural, glucose, cellulose, polyacrylonitrile, lignin and hemicellulose.

[0017] More preferably, the mass ratio of the fly ash to the calcium-based oxygen-containing compound is (15:1)-(30:1).

[0018] When too much calcium-based oxygen-containing compound is added, the calcium-based oxygen-containing compound cannot react completely, resulting in pore blockage and affecting the pores. When too little calcium-based oxygen-containing compound is added, the yield will be low.

[0019] More preferably, the mass ratio of the calcium-based oxygen-containing compound to the carbon source is (1:10)-(1:20).

[0020] More preferably, the temperature of the hydrothermal treatment is 150-250° C. and the time is 8-20 h.

[0021] More preferably, the carbonization treatment is: carbonization treatment at 600-800° C. for 10-60 min in an inert mixed atmosphere.

[0022] The inert mixed atmosphere is a mixture of nitrogen and argon in a ratio of (1:1)-(3:1), and the gas flow rate is 70-100 mL / min.

[0023] More preferably, the fly ash alkali leaching solution is prepared by adding fly ash to a pre-prepared alkali composite solution, mixing and stirring, alkali washing, centrifugal filtration, and obtaining a supernatant liquid, which is the fly ash alkali leaching solution.

[0024] The prior art still stays at modifying the surface of the fly ash microstructure to improve the pore structure of its surface, and then adsorbing the phase change material, but this method has a poor effect on improving the pores, resulting in a low adsorption amount of the phase change material, and the content of the components with high thermal conductivity in the fly ash is low, so the thermal conductivity of the composite material formed is poor. The present invention forms silicate ions by reacting the alkali composite solution with the silicon-containing components in the fly ash, and the silicate ions further react with the calcium-based oxygen-containing compound under hydrothermal conditions, and the products continue to accumulate and grow in different directions, and finally form a porous material with a three-dimensional interconnected network structure, which provides sufficient space for the filling of the phase change material, and the carbon precursor provided by the carbon source grows on the surface and inside of the porous structure during the hydrothermal process. After carbonization treatment, a carbon self-growing modified fly ash-based porous material is formed, which can enhance the thermal conductivity of the composite material. In addition, the present invention also affects its porosity by controlling the hydrothermal time and hydrothermal temperature.

[0025] The specific preparation method of the carbon self-growth modified fly ash-based porous material is as follows: placing fly ash in a pre-prepared alkali composite solution, mixing and stirring it thoroughly, washing it with alkali, and centrifuging and filtering it to obtain the upper clear liquid, which is the fly ash alkali leaching solution; adding calcium-based oxygen-containing compounds and carbon sources to the fly ash alkali leaching solution, stirring, and mixing them thoroughly to obtain a hydrothermal ligand solution; charging the hydrothermal ligand solution into a hydrothermal reactor, performing hydrothermal treatment, and after the hydrothermal treatment is completed, centrifuging and filtering it to obtain a carbon self-growth modified fly ash-based precursor solid product; and carbonizing the solid product under an inert mixed atmosphere to obtain a carbon self-growth modified fly ash-based porous material.

[0026] More preferably, the alkaline composite solution is one or more of sodium hydroxide, potassium hydroxide, lithium hydroxide, ammonia water, sodium carbonate and sodium bicarbonate solution; the concentration of the alkaline composite solution is 1-5 mol / L, the temperature of alkaline washing is 60-150°C, and the time is 30-120 min.

[0027] The third technical solution provided by the present invention is:

[0028] An application of the above-mentioned super-hydrophobic fly ash-based photothermal conversion composite phase change heat storage material in preventing power transmission lines from icing disasters.

[0029] Technical principle of the present invention:

[0030] The present invention reconstructs the structure of fly ash by using an alkaline hydrothermal method, and the porous fly ash obtained has a higher porosity. A carbon source is added during the hydrothermal process so that hydrothermal carbon with high thermal conductivity is attached to the surface of the hydrothermally generated porous material, thereby improving the energy storage efficiency of the composite phase change thermal storage material. The added spectrum adjustment material has a higher absorptivity in the solar spectrum range, further improving the photothermal conversion efficiency of the composite phase change thermal storage material; the phase change material in the composite phase change thermal storage material has a higher mass fraction and has an adjustable enthalpy value.

[0031] Beneficial effects of the present invention:

[0032] The super-hydrophobic fly ash-based photothermal conversion composite phase-change heat storage material provided by the present invention has the advantages of high thermal conductivity, high visible light absorptivity, high stability, etc., wherein the high pore capacity and high thermal conductivity of the carbon self-grown modified fly ash porous material make the phase change latent heat of the composite phase-change heat storage material reach 65-80% of the theoretical latent heat of the phase change material, and the thermal conductivity of the obtained composite phase-change heat storage material is increased to 2-5 times the thermal conductivity of the phase change material; the composite phase-change heat storage material has excellent thermal stability and cycle stability, and no leakage occurs after 1000 cycles, and the shape stability is still maintained when the phase change material is heated for a long time or even overheated. The surface contact angle of the coating formed by the composite phase-change heat storage material is greater than 150°, and the rolling angle is less than 10°, which has excellent super-hydrophobic properties.

[0033] The fly ash raw material used in the super-hydrophobic fly ash-based photothermal conversion composite phase change heat storage material disclosed in the present invention has the advantages of being environmentally friendly, abundant raw materials, low price, and suitable for mass production. The carbon self-growth modified fly ash-based porous material prepared by the present invention has the advantage of high thermal conductivity due to the addition of hydrothermal carbon, overcoming the problem of low thermal conductivity of phase change materials and ordinary fly ash.

[0034] The present invention makes up for the defects of high preparation cost of composite phase change heat storage support materials, difficulty in preparing fly ash-based porous materials, and low thermal conductivity of fly ash-based composite phase change heat storage materials. The composite phase change heat storage material has the advantages of low cost, low leakage, high thermal conductivity, and good light-heat conversion performance. It provides an effective method for realizing the high-value utilization of fly ash solid waste in the field of thermal energy storage and efficient solar energy conversion. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0036] Figure 1 This is a SEM image of the fly ash-based porous material modified by carbon self-growth obtained in Example 1;

[0037] Figure 2 This is an SEM image of the super-hydrophobic fly ash-based photothermal conversion composite phase change heat storage material prepared in Example 1. DETAILED DESCRIPTION

[0038] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0039] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0040] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0041] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present application description and examples are exemplary only.

[0042] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0043] The room temperature in the present invention refers to 25±2° C., and the normal pressure refers to 0.1013 MPa.

[0044] In the embodiments of the present invention, “parts” refer to “parts by mass” unless otherwise specified.

[0045] An embodiment of the present invention provides a super-hydrophobic fly ash-based photothermal conversion composite phase change heat storage material, which includes the following raw materials, measured by mass: 65-80 parts of phase change material, 10-32 parts of carbon self-growth modified fly ash-based porous material, 2-5 parts of spectrum adjustment material and 10-15 parts of hydrophobic material.

[0046] The embodiment of the present invention also provides a method for preparing a super-hydrophobic fly ash-based photothermal conversion composite phase change heat storage material: the carbon self-growth modified fly ash-based porous material uses fly ash alkali leaching solution as raw material, and the porous material prepared by alkaline hydrothermal chemical synthesis and high-temperature carbonization process has high porosity and participates in the preparation as a supporting skeleton. The phase change material and the spectrum adjustment material are uniformly filled in the pores of the carbon self-growth modified fly ash-based porous material by vacuum impregnation or normal pressure heating and mixing, and the hydrophobic material is uniformly dispersed on the surface of the composite material by blending. The carbon self-growth modified fly ash-based porous material as a supporting skeleton provides a large number of pores for the phase change material to attach stably, the high thermal conductivity of hydrothermal carbon and the light absorption characteristics of the spectrum adjustment material provide the composite phase change heat storage material with good thermal conductivity and photothermal conversion efficiency, the selective spectrum absorption function of the spectrum adjustment material enhances the absorption capacity of the target wavelength, and the hydrophobic material improves the overall hydrophobic performance of the composite phase change heat storage material.

[0047] Example 1

[0048] A method for preparing a super-hydrophobic fly ash-based photothermal conversion composite phase change heat storage material

[0049] 1) Add 20 g of fly ash to 100 mL of sodium hydroxide solution (3 mol / L), heat and stir at 80°C for 0.5 h, filter the resulting mixed solution, take the filtrate as fly ash alkali leaching solution, add 0.8 g of calcium oxide and 13 g of furfural, stir and mix, and hydrothermally react at 180°C for 12 h; centrifuge and filter the solution after the hydrothermal reaction to obtain a carbon self-growth modified fly ash-based precursor solid product; heat the obtained solid product from room temperature to 600°C for 0.5 h in a nitrogen and argon atmosphere with a mixed volume ratio of 1:1 to prepare a carbon self-growth modified fly ash-based porous material, and the specific surface area of ​​the prepared porous material is 68.5 m 2 / g, much higher than the 2.7m / g of ordinary fly ash 2 / g, Figure 1 The SEM image of the fly ash-based porous material modified by carbon self-growth obtained in this embodiment. Figure 1 It can be seen that the obtained porous material has relatively developed pores, which provides sufficient space for the adsorption of a large amount of phase change substances.

[0050] 2) Grind and mix 0.15g of the porous material prepared in step 1), 0.04g of vanadium dioxide and 0.7g of polyethylene glycol, put them into a vacuum heating container, use a vacuum pump to evacuate to -0.1MPa, wait for the vacuum container temperature to reach 80°C and keep it warm for 0.5h, cool the vacuum container, take out the carbon self-growth modified fly ash-based composite phase change heat storage material, mix the obtained composite phase change heat storage material with 0.11g of polydimethylsiloxane, stir and disperse evenly, and then dry (70°C, 12h) to obtain a super-hydrophobic fly ash-based photothermal conversion composite phase change heat storage material. Figure 2 The SEM image of the composite phase change heat storage material prepared in this embodiment is Figure 2 It can be seen that the pores of the porous material can be completely filled and the composite effect is good.

[0051] The phase change latent heat of the obtained super-hydrophobic fly ash-based photothermal conversion composite phase change thermal storage material is 68% of that of pure polyethylene glycol, and the thermal conductivity is 0.8W / m·K, which is 4 times that of pure polyethylene glycol (0.2W / m·K). The photothermal conversion efficiency of the composite phase change thermal storage material prepared in this embodiment reaches 80.3% within the solar spectrum range.

[0052] Example 2

[0053] A method for preparing a super-hydrophobic fly ash-based photothermal conversion phase change heat storage composite phase change material

[0054] 1) Add 20g of fly ash to 100mL of sodium hydroxide solution (4mol / L), heat at 90℃ and stir for 0.5h, filter the resulting mixture, take the filtrate as fly ash alkaline leaching solution, add 0.7g of calcium hydroxide and 10g of glucose, stir and mix, and hydrothermally react at 180℃ for 12h; centrifuge and filter the solution after the hydrothermal reaction to obtain a carbon self-growth modified fly ash-based precursor solid product; heat the obtained solid product from room temperature to 700℃ in a nitrogen and argon atmosphere with a mixing ratio of 2:1 for 0.5h to obtain a carbon self-growth modified fly ash-based porous material. The specific surface area of ​​the prepared porous material is 65.3m 2 / g;

[0055] 2) Grind and mix 0.1g of the porous material prepared in step 1), 0.05g of tungsten dioxide and 0.75g of stearic acid, put them into a vacuum heating container, use a vacuum pump to evacuate to -0.1MPa, wait for the vacuum container temperature to reach 90°C and keep it warm for 0.5h, cool the vacuum container, take out the carbon self-growth modified fly ash-based composite phase change heat storage material; mix the obtained composite phase change heat storage material with 0.1g of hexamethyldisilazane, stir and disperse evenly, and then dry (60°C, 15h) to obtain a super-hydrophobic fly ash-based photothermal conversion composite phase change heat storage material.

[0056] The phase change latent heat of the obtained super-hydrophobic fly ash-based photothermal conversion composite phase change thermal storage material is 73% of that of pure stearic acid, and the thermal conductivity is 0.7W / m·K, which is 2.3 times that of pure stearic acid (0.3W / m·K). The photothermal conversion efficiency of the composite phase change thermal storage material prepared in this embodiment reaches 82.6% within the solar spectrum range.

[0057] Example 3

[0058] A method for preparing a super-hydrophobic fly ash-based photothermal conversion phase change heat storage composite phase change material

[0059] 1) Add 20 g of fly ash to 200 mL of potassium hydroxide solution (1 mol / L), heat and stir at 120° C. for 1.5 h, filter the resulting mixed solution, take the filtrate as fly ash alkali leaching solution, add 1 g of calcium oxide powder and 12 g of furfural, stir and mix, and hydrothermally react at 165° C. for 10 h; centrifuge and filter the solution after the hydrothermal reaction to obtain a carbon self-growth modified fly ash-based precursor solid product; heat the obtained solid product from room temperature to 700° C. for 1 h in a nitrogen and argon atmosphere with a mixing ratio of 3:1 to prepare a carbon self-growth modified fly ash-based porous material, and the specific surface area of ​​the prepared porous material is 64.7 m 2 / g;

[0060] 2) Grind and mix 0.15g of the porous material prepared in step 1), 0.05g of nano zinc oxide and 0.7g of lauric acid, put them into a vacuum heating container, use a vacuum pump to evacuate to -0.1MPa, wait for the vacuum container temperature to reach 70°C and then keep it warm for 0.5h; cool the vacuum container, take out the carbon self-growth modified fly ash-based composite phase change heat storage material, mix the obtained composite phase change heat storage material with 0.1g of dodecyltriethoxysilane, stir and disperse evenly, and then dry to obtain a super hydrophobic fly ash-based photothermal conversion composite phase change heat storage material.

[0061] The phase change latent heat of the obtained super-hydrophobic fly ash-based photothermal conversion composite phase change heat storage material is 67% of that of pure lauric acid, and the thermal conductivity is 0.8 W / m·K, which is 4 times that of pure lauric acid (0.2 W / m·K). The composite phase change heat storage material prepared in this embodiment has a photothermal conversion efficiency of 85.1% within the solar spectrum range.

[0062] Example 4

[0063] A method for preparing a super-hydrophobic fly ash-based photothermal conversion phase change heat storage composite phase change material

[0064] 1) Add 20 g of fly ash to 100 mL of potassium hydroxide solution (2 mol / L), heat and stir at 90 ° C for 1 h, filter the resulting mixed solution, take the filtrate as fly ash alkali leaching solution, add 1.2 g of calcium oxide powder and 15 g of polyacrylonitrile, stir and mix, and hydrothermally react at 220 ° C for 12 h; centrifuge and filter the solution after the hydrothermal reaction to obtain a carbon self-growth modified fly ash-based precursor solid product; heat the obtained solid product from room temperature to 800 ° C for 1 h in a nitrogen and argon atmosphere with a mixing ratio of 1:1 to prepare a carbon self-growth modified fly ash-based porous material, and the specific surface area of ​​the prepared porous material is 65.8 m 2 / g;

[0065] 2) Grind and mix 0.18g of the porous material prepared in step 1), 0.03g of tungsten dioxide and 0.67g of lauric acid, put them into a vacuum heating container, use a vacuum pump to evacuate to -0.1MPa, wait for the vacuum container temperature to reach 70°C and keep it warm for 0.5h; cool the vacuum container, take out the carbon self-growth modified fly ash-based composite phase change heat storage material, mix the obtained composite phase change heat storage material with 0.12g of methyl hydrogen silicone oil, stir and disperse evenly, and then dry (80°C, 10h) to obtain a super hydrophobic fly ash-based photothermal conversion composite phase change heat storage material.

[0066] The phase change latent heat of the obtained super-hydrophobic fly ash-based photothermal conversion composite phase change heat storage material is 66% of that of pure lauric acid, and the thermal conductivity is 0.8 W / m·K, which is 4 times that of pure lauric acid (0.2 W / m·K). The composite phase change heat storage material prepared in this embodiment has a photothermal conversion efficiency of 79.2% within the solar spectrum range.

[0067] Example 5

[0068] A method for preparing a super-hydrophobic fly ash-based photothermal conversion composite phase change heat storage material

[0069] 1) Add 20 g of fly ash to 100 mL of lithium hydroxide solution (5 mol / L), heat and stir at 60°C for 0.5 h, filter the resulting mixed solution, take the filtrate as fly ash alkali leaching solution, add 0.9 g of calcium nitrate powder and 10 g of cellulose, stir and mix, and hydrothermally react at 220°C for 12 h; centrifuge and filter the solution after the hydrothermal reaction to obtain a carbon self-growth modified fly ash-based precursor solid product; heat the obtained solid product from room temperature to 600°C for 1 h in a nitrogen and argon atmosphere with a mixing ratio of 3:1 to prepare a carbon self-growth modified fly ash-based porous material, and the specific surface area of ​​the prepared porous material is 66.7 m 2 / g;

[0070] 2) Grind and mix 0.12g of the porous material prepared in step 1), 0.02g of nano-titanium dioxide and 0.75g of polyethylene glycol, put them into a vacuum heating container, use a vacuum pump to evacuate to -0.1MPa, wait for the vacuum container temperature to reach 90°C and keep it warm for 0.5h, cool the vacuum container, take out the carbon self-growth modified fly ash-based composite phase change heat storage material, mix the obtained composite phase change heat storage material with 0.11g of polydimethylsiloxane, stir and disperse evenly, and then dry (70°C, 12h) to obtain a super hydrophobic fly ash-based photothermal conversion composite phase change heat storage material.

[0071] The phase change latent heat of the obtained super-hydrophobic fly ash-based photothermal conversion composite phase change heat storage material is 75% of that of pure polyethylene glycol, and the thermal conductivity is 0.7 W / m·K, which is 3.5 times that of pure polyethylene glycol (0.2 W / m·K). The composite phase change heat storage material prepared in this embodiment has a photothermal conversion efficiency of 75.9% within the solar spectrum range.

[0072] Comparative Example 1

[0073] 1) Add 20g of fly ash to 100mL of sodium hydroxide solution (2mol / L), heat at 60°C and stir for 0.5h, filter the resulting mixed solution, take the filtrate as fly ash alkali leaching solution, add 0.7g of calcium oxide powder, stir and mix, hydrothermally react at 180°C for 12h, filter the solution after the hydrothermal reaction to separate the solid and the liquid, dry the solid part at 85°C for 15h, and the dried solid powder is the modified fly ash porous material;

[0074] 2) Grind and mix 0.3 g of the porous material prepared in step 1) with 0.65 g of polyethylene glycol, put them into a vacuum heating container, use a vacuum pump to evacuate to -0.1 MPa, wait for the vacuum container temperature to reach 80°C and keep it warm for 0.5 h, cool the vacuum container, take out the modified fly ash-based composite phase change material, mix the obtained composite phase change material with 0.05 g of polydimethylsiloxane, stir and disperse evenly, and then dry (100°C, 5 h) to obtain a hydrophobic fly ash-based composite phase change heat storage material.

[0075] The phase change latent heat of the obtained hydrophobic fly ash-based composite phase change heat storage material is 61% of that of pure polyethylene glycol, and the thermal conductivity is 1.1 times that of pure polyethylene glycol. The composite phase change material prepared in this comparative example has a light-to-heat conversion efficiency of 35.6% within the solar spectrum.

[0076] Comparative Example 2

[0077] 1) Add 10g of fly ash to 100mL of potassium hydroxide solution (3mol / L), heat and stir at 30°C for 0.5h, filter the resulting mixed solution, take the filtrate as fly ash alkali leaching solution, add 0.5g of calcium hydroxide powder, stir and mix, hydrothermally react at 130°C for 5h, filter the solution after the hydrothermal reaction to separate the solid and the liquid, dry the solid part at 80°C for 15h, and the dried solid powder is the modified fly ash porous material;

[0078] 2) Grind and mix 0.35 g of the porous material prepared in step 1) with 0.59 g of stearic acid, put them into a vacuum heating container, use a vacuum pump to evacuate to -0.1 MPa, wait for the vacuum container temperature to reach 50°C and keep it warm for 0.5 h, cool the vacuum container, take out the modified fly ash-based composite phase change material, mix the obtained composite phase change material with 0.06 g of dodecyltriethoxysilane, stir and disperse evenly, and then dry (70°C, 12 h) to obtain a hydrophobic fly ash-based composite phase change heat storage material.

[0079] The phase change latent heat of the obtained hydrophobic fly ash-based composite phase change heat storage material is 57% of that of pure stearic acid, and the thermal conductivity is 1.3 times that of pure stearic acid. The composite phase change material prepared in this comparative example has a light-to-heat conversion efficiency of 33.5% within the solar spectrum.

[0080] Comparative Example 3

[0081] 1) Slowly add 10g of fly ash into 100mL of potassium hydroxide solution (4mol / L), heat at 50℃ and stir for 0.5h, filter the resulting mixed solution, take the filtrate as fly ash alkali leaching solution, add 0.6g of calcium hydroxide powder, stir and mix, react at 90℃ for 6h, filter the reaction product to separate the solid and liquid, dry the solid part at 60℃ for 24h, and the dried solid powder is the modified fly ash porous material.

[0082] 2) Grind and mix 0.23 g of the porous material prepared in step 1) with 0.7 g of lauric acid, put them into a vacuum heating container, use a vacuum pump to evacuate to -0.1 MPa, wait for the temperature of the vacuum container to reach 30°C, cool the vacuum container, take out the modified fly ash-based composite phase change material, mix the obtained composite phase change material with 0.07 g of hexamethyldisilazane, stir and disperse evenly, and then dry (80°C, 12h) to obtain a hydrophobic fly ash-based composite phase change heat storage material.

[0083] The phase change latent heat of the obtained hydrophobic fly ash-based composite phase change heat storage material is 57% of that of pure lauric acid, and the thermal conductivity is 1.3 times that of pure lauric acid. The composite phase change material prepared in this comparative example has a light-to-heat conversion efficiency of 36.1% within the solar spectrum.

[0084] Comparative Example 4

[0085] Same as Example 1, except that furfural is not added in step 1).

[0086] The phase change latent heat of the obtained super hydrophobic fly ash-based photothermal conversion composite phase change thermal storage material is 63% of that of pure polyethylene glycol, and the thermal conductivity is 1.3 times that of pure polyethylene glycol. The composite phase change material prepared in this comparative example has a photothermal conversion efficiency of 70.6% within the solar spectrum.

[0087] Comparative Example 5

[0088] Same as Example 1, except that vanadium dioxide is not added in step 2).

[0089] The phase change latent heat of the obtained super-hydrophobic fly ash-based photothermal conversion composite phase change thermal storage material is 67% of that of pure polyethylene glycol, and the thermal conductivity is 0.7W / m·K, which is 3.5 times that of pure polyethylene glycol (0.2W / m·K). The composite phase change material prepared in this comparative example has a photothermal conversion efficiency of 51.3% within the solar spectrum.

[0090] Comparative Example 6

[0091] 1) Add 20 g of fly ash to 100 mL of sodium hydroxide solution (3 mol / L), heat and stir at 80°C for 0.5 h, filter the resulting mixed solution, take the filtrate as fly ash alkali leaching solution, add 1.5 g of calcium oxide and 15 g of furfural, stir and mix, and hydrothermally react at 180°C for 12 h; centrifuge and filter the solution after the hydrothermal reaction to obtain a carbon self-growth modified fly ash-based precursor solid product; heat the obtained solid product from room temperature to 600°C for 0.5 h in a nitrogen and argon atmosphere with a mixing ratio of 1:1 to prepare a carbon self-growth modified fly ash-based porous material, and the specific surface area of ​​the prepared porous material is 39.7 m 2 / g;

[0092] Step 2) is the same as in Example 1.

[0093] The phase change latent heat of the obtained super-hydrophobic fly ash-based photothermal conversion composite phase change thermal storage material is 37% of that of pure polyethylene glycol, and the thermal conductivity is 0.8W / m·K, which is 4 times that of pure polyethylene glycol (0.2W / m·K). The composite phase change material prepared in this comparative example has a photothermal conversion efficiency of 76% within the solar spectrum.

[0094] Comparative Example 7

[0095] 1) Add 20 g of fly ash to 100 mL of sodium hydroxide solution (3 mol / L), heat at 80°C and stir for 0.5 h, filter the resulting mixed solution, take the filtrate as fly ash alkali leaching solution, add 0.4 g of calcium oxide and 8 g of furfural, stir and mix, and hydrothermally react at 180°C for 12 h; centrifuge and filter the solution after the hydrothermal reaction to obtain a carbon self-growth modified fly ash-based precursor solid product; heat the obtained solid product from room temperature to 600°C in a nitrogen and argon atmosphere with a mixing ratio of 1:1 for 0.5 h to prepare a carbon self-growth modified fly ash-based porous material, and the specific surface area of ​​the prepared porous material is 60.7 m 2 / g, the yield of porous materials decreased by about 50%;

[0096] Step 2) is the same as in Example 1.

[0097] The phase change latent heat of the obtained super-hydrophobic fly ash-based photothermal conversion composite phase change thermal storage material is 63% of that of pure polyethylene glycol, and the thermal conductivity is 0.7W / m·K, which is 3.5 times that of pure polyethylene glycol (0.2W / m·K). The composite phase change material prepared in this comparative example has a photothermal conversion efficiency of 79.6% within the solar spectrum.

[0098] Application Example 1

[0099] Composite coatings were prepared using the composite phase change materials prepared in Examples 1-5 and Comparative Examples 1-7, and the hydrophobic properties of the coatings were verified through simulation experiments.

[0100] The specific determination method is: take 1g of each of the composite phase change materials prepared in Examples 1-5 and Comparative Examples 1-7, disperse them in 20mL of ethyl acetate solvent, stir at room temperature to form a mixed solution, spray the mixed solution on the surface of the copper sheet with a spray gun, and form a composite coating after drying. The surface contact angle and rolling angle of the obtained composite coating are tested, and the experimental results are shown in Tables 1 and 2.

[0101] Table 1

[0102]

[0103] Table 2

[0104]

[0105] It can be seen from Tables 1 and 2 that the composite coating formed by the composite phase change heat storage material prepared by Examples 1-5 has a higher surface contact angle and a lower rolling angle, indicating that the super-hydrophobic fly ash-based photothermal conversion phase change heat storage composite phase change material prepared by the alkaline hydrothermal method of the present invention has great potential in suppressing ice disasters, etc. However, the amount of hydrophobic material in Comparative Examples 1, 2, and 3 is relatively small, so the hydrophobic effect is relatively poor.

[0106] Cyclic stability test: The cyclic stability of Examples 1-5 and Comparative Examples 1-7 was verified by simulation experiments. The specific test method is: 5 g of the composite phase change materials prepared in Examples 1-5 and Comparative Examples 1-7 were taken, and pressed into thin sheets using a circular mold with a diameter of 50 mm and a pressure of 14 MPa for 3 minutes. The thin sheets were placed in a high and low temperature test box and heated from -10°C to 80°C at a rate of 5°C / min, and then cooled from 80°C to -10°C at a rate of 5°C / min. The temperature was raised and lowered for 1000 cycles, and the leakage of the samples during the cycle was tested. The experimental results are shown in Tables 3 and 4.

[0107] Table 3

[0108]

[0109] Table 4

[0110]

[0111] Thermal stability test: The thermal stability of Examples 1-5 and Comparative Examples 1-7 was verified by simulation experiments. The specific test method is: 5 g of the composite phase change materials prepared in Examples 1-5 and Comparative Examples 1-7 were taken, and pressed into thin sheets using a circular mold with a diameter of 50 mm and a pressure of 14 MPa for 3 minutes. The thin sheets were placed in a high temperature environment of 150°C for 6 hours, and the stability of the samples under high temperature conditions was tested. The experimental results are shown in Tables 5 and 6.

[0112] Table 5

[0113]

[0114] Table 6

[0115]

[0116] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A super-hydrophobic fly ash-based photothermal conversion composite phase change heat storage material, characterized in that: The raw materials include the following by mass: 65-80 parts of phase change material, 10-32 parts of fly ash-based porous material modified by carbon self-growth, 2-5 parts of spectrum adjustment material and 10-15 parts of hydrophobic material.

2. A method for preparing the super-hydrophobic fly ash-based photothermal conversion composite phase change thermal storage material according to claim 1, characterized in that: The raw materials are weighed by mass, and the carbon self-growth modified fly ash-based porous material, the spectrum adjustment material and the phase change material are mixed by vacuum impregnation method or normal pressure heating method to obtain the carbon self-growth modified fly ash-based photothermal conversion composite phase change heat storage material; the carbon self-growth modified fly ash-based photothermal conversion composite phase change heat storage material and the hydrophobic material are mixed, stirred and dried to obtain the super-hydrophobic fly ash-based photothermal conversion composite phase change heat storage material.

3. The preparation method according to claim 2, characterized in that: The preparation method of the carbon self-growth modified fly ash-based porous material is as follows: adding a calcium-based oxygen-containing compound and a carbon source into fly ash alkaline leaching solution, mixing to obtain a hydrothermal ligand solution, hydrothermally treating, centrifuging, filtering to obtain a carbon self-growth modified fly ash-based precursor solid product, and carbonizing to obtain a carbon self-growth modified fly ash-based porous material.

4. The preparation method according to claim 3, characterized in that: The mass ratio of the fly ash to the calcium-based oxygen-containing compound is (15:1)-(30:1).

5. The preparation method according to claim 3, characterized in that: The mass ratio of the calcium-based oxygen-containing compound to the carbon source is (1:10)-(1:20).

6. The preparation method according to claim 3, characterized in that: The temperature of the hydrothermal treatment is 150-250° C. and the time is 8-20 hours.

7. The preparation method according to claim 3, characterized in that: The carbonization treatment is: in an inert mixed atmosphere, at 600-800° C., for 10-60 minutes.

8. The preparation method according to claim 3, characterized in that: The preparation method of the fly ash alkali leaching solution is as follows: adding fly ash into a pre-prepared alkali composite solution, mixing and stirring, centrifuging and filtering to obtain a supernatant liquid, which is the fly ash alkali leaching solution.

9. An application of the super-hydrophobic fly ash-based photothermal conversion composite phase change heat storage material according to claim 1 in preventing icing disasters on power transmission lines.

Citation Information

Patent Citations

  • Preparation method of phase-change energy-storage material

    CN103773318A

  • Preparation method and application of fly ash CO2 trapping agent

    CN112707746A

  • Bamboo-like phase change heat storage material and preparation method thereof

    CN114292628A

  • Multifunctional biochar-based phase change composite material and preparation method thereof

    CN115160991A

  • Heat storage material prepared from solid wastes such as fly ash and slag

    CN115872768A

Cited By

  • Desert sand-based low-cost composite heat storage material as well as preparation method and application thereof

    CN121801545A