Epoxy-based adhesive with self-healing and shape memory functions and preparation method of epoxy-based adhesive
Through the combination of polyurethane, bisphenol A type epoxy resin and disulfide bond aromatic amine curing agent, a cross-linking network is constructed, which solves the problems of poor mechanical brittleness and toughness of epoxy resin, and achieves enhanced mechanical properties and shape memory Ability to be suitable for excellent bonding and remodelable reuse of a variety of substrates.
Patent Information
- Application Number
- CN202410958406.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-07-17
AI Technical Summary
Due to its highly crosslinked and rigid molecular chain structure, traditional epoxy resin materials have problems of poor mechanical brittleness and toughness, which limits their potential for application in multiple fields and is difficult to remodel or reuse through conventional methods, resulting in waste of resources. and environmental pollution.
Polyurethane prepolymer is used to combine with bisphenol A type epoxy resin and bisulphur bond-containing aromatic amine curing agent to build a dense structure through a chemical crosslinking network, increase the flexibility and impact resistance of the material, and pass the low-temperature high-temperature curing step Epoxy-based adhesives with self-healing, shape memory and excellent bonding properties are prepared.
The toughness and remodelability of epoxy resin are achieved, and the mechanical properties and shape memory of the material are improved. It can show excellent bonding properties on a variety of substrates and maintain strength after multiple cycles. , reduces the glass transition temperature to improve flexibility.
Smart Images

Figure CN118895096A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of epoxy-based structural adhesives, in particular to the field of IPCC09J163, and more specifically to an epoxy-based adhesive with self-healing, shape memory and excellent bonding properties and a preparation method thereof. Background Art
[0002] Thermosetting polymers play an indispensable role in modern society and are widely used in many fields due to their excellent physical and chemical stability. Epoxy resin, as an important branch of thermosetting materials, is known for its unique permanent cross-linked structure. This structure gives epoxy resin excellent chemical stability, electrical insulation properties, mechanical strength and bonding strength, making it the material of choice in many industries such as construction, electronic packaging and military. However, it is this permanent cross-linked structure that also brings challenges to the processing and recycling of epoxy resin. Traditional thermosetting polymers are difficult to reshape or reuse by conventional methods, which not only leads to a great waste of resources, but also imposes a burden on the environment that cannot be ignored. In addition, due to its highly cross-linked and rigid molecular chain structure, epoxy resin often exhibits low flexibility in practical applications and is prone to brittle fracture when subjected to impact or stress, limiting its potential for application in a wider range of fields. In order to overcome these limitations, researchers have been exploring innovative methods to improve the processability, reshaping and toughness of epoxy resin, thereby expanding its application range and reducing its impact on the environment. The emergence of adaptive covalent networks (CANs) provides a promising approach for the sustainable development of thermosetting polymers. Although there are many works that have achieved the reprocessability and even degradability of epoxy resins through dynamic covalent bonds, adaptive dynamic networks are often accompanied by mechanical brittleness and poor toughness.
[0003] CN114195984B discloses a bisphenol A type epoxy curing agent containing dynamic enamine bonds and a degradable epoxy resin and a preparation, remodeling, and degradation method thereof, wherein the preparation method comprises: heating and stirring the acetoacetic acid epoxy monomer and the amine curing agent at 30-130°C to obtain; the preparation method of the degradable epoxy resin comprises: mixing the epoxy curing agent with the bisphenol A type epoxy monomer and heating and curing at 60-150°C to obtain; the remodeling method comprises: hot pressing the degradable epoxy resin at 160-220°C to obtain; the degradation method comprises: placing the degradable epoxy resin in an acid solution and stirring at 25-180°C for 0.5-48h, and then completing the degradation after neutralization, solid-liquid separation, washing, and drying in sequence. Compared with the prior art, the epoxy resin material containing dynamic amide bonds in the present invention has the advantages of being degradable, recyclable, and recyclable, which is conducive to promoting the industrial application of dynamic epoxy resins. However, it does not solve the problem that the adaptive dynamic network is often accompanied by mechanical brittleness and poor toughness. Summary of the invention
[0004] The first aspect of the present invention provides an epoxy-based adhesive with self-healing, shape memory and excellent bonding properties. The raw materials for preparing the adhesive include: a polyurethane prepolymer, a bisphenol A epoxy resin, a disulfide bond-containing aromatic amine curing agent and an epoxy accelerator.
[0005] The raw materials for preparing the polyurethane prepolymer include: polyether polyol, diisocyanate and a catalyst.
[0006] The isocyanate includes at least one of toluene diisocyanate, 4-methoxy-1,3-phenylene diisocyanate, 4-isopropyl-1,3-phenylene diisocyanate, 1,4-tetramethylene diisocyanate, 1,6-hexamethylene diisocyanate, 1,10-decamethylene diisocyanate, 1,4-cyclohexylene diisocyanate, xylene diisocyanate, 4,4-methylenebis(cyclohexyl isocyanate), 1,5-tetrahydronaphthalene diisocyanate, and isophorone diisocyanate.
[0007] The catalyst includes one or more of dibutyltin dilaurate, stannous octoate, dibutyltin didodecylsulfide, dibutyltin diacetate, dialkyltin dimaleate, and alkyltin dithiolate.
[0008] The molar ratio of the polyether polyol to the diisocyanate is 1:(2-3).
[0009] The polyether polyol comprises a first polyether polyol and a second polyether polyol, wherein the hydroxyl value of the first polyether polyol is 120-250 mgKOH / g, and the hydroxyl value of the second polyether polyol is 30-100 mgKOH / g.
[0010] Preferably, the hydroxyl value of the first polyether polyol is 180-220 mgKOH / g, and the hydroxyl value of the second polyether polyol is 40-60 mgKOH / g.
[0011] The molar ratio of the first polyether polyol to the second polyether polyol is (1-3):1.
[0012] The molar ratio of the polyurethane prepolymer to the bisphenol A epoxy resin is 1:(1.5-4).
[0013] Preferably, the molar ratio of the polyurethane prepolymer to the bisphenol A epoxy resin is 1:(1.5-3).
[0014] More preferably, the molar ratio of the polyurethane prepolymer to the bisphenol A epoxy resin is 1:(2-3).
[0015] Preferably, the molar ratio of the bisphenol A epoxy resin to the disulfide bond-containing aromatic amine curing agent is 1:(1-2).
[0016] The disulfide bond-containing aromatic amine curing agent includes at least one of 4,4'-dithiodiphenylamine, bis(3-fluoro-4-aminophenyl) disulfide, 2-[(2-amino-5-isopropylphenyl) dithio]-4-isopropylaniline, bis(2-aminophenyl) disulfide, [2-(2-amino-5-methoxy-phenyl) dithio-4-methoxy-phenyl] amine, 2-[(2-amino-5-methylphenyl) dithio]-4-methylaniline, 2-[(2-amino-5-ethylphenyl) dithio]-4-ethylaniline, 5,5'-disulfanediylbis(2-chloroaniline), bis(2-amino-4-methylphenyl) disulfide, 2,2'-dithiodi(1-naphthylamine), and 6,6-disulfidediylbis(2-methylaniline).
[0017] Preferably, the disulfide bond-containing aromatic amine curing agent includes bis(2-aminophenyl) disulfide.
[0018] The epoxy accelerator includes at least one of DMP-30 (2,4,6-tris(dimethylaminomethyl)phenol), imidazole, triethanolamine and resorcinol.
[0019] Preferably, the epoxy accelerator includes DMP-30.
[0020] The second aspect of the present invention provides a method for preparing an epoxy-based adhesive with self-healing, shape memory and excellent bonding properties, comprising the following steps: mixing a polyurethane prepolymer, a bisphenol A epoxy resin, a disulfide bond-containing aromatic amine curing agent and an epoxy accelerator, and stirring them evenly in a vacuum defoaming mixer, and curing to obtain the adhesive.
[0021] The curing is performed in sequence of low temperature curing and high temperature curing; the conditions of the low temperature curing are: curing at 60-90° C. for 10-15 hours; the conditions of the high temperature curing are: curing at 110-130° C. for 4-7 hours.
[0022] Preferably, the curing is performed sequentially by low-temperature curing and high-temperature curing; the conditions for the low-temperature curing are: curing at 70-90°C for 10-12h; the conditions for the high-temperature curing are: curing at 110-120°C for 5-7h.
[0023] Traditional epoxy resin has a relatively low mechanical strength despite its high crosslink density and rigidity. This phenomenon is attributed to the lack of toughness, which results in the inability to effectively dissipate energy when subjected to external force, thereby causing the failure of the entire structure within a relatively short displacement. The applicant has found that by using aromatic amine curing agents as curing agents, polyurethane can be combined with epoxy resin, and the bisphenol A structure with rigid characteristics and the diamine structure are linearly connected, and the chemical crosslinking network is constructed by flexible polyurethane resin. It may be that polyurethane can form microscopic phase separation in epoxy resin due to its highly branched structure, and this structure can serve as a barrier for crack propagation, improve the toughness of the material, and thus toughen epoxy resin. Active functional groups (such as hydroxyl or amino) in polyurethane can react chemically with epoxy groups in epoxy resin to form covalent bonds, which helps to enhance interfacial bonding and improve overall mechanical properties. At the same time, polyurethane has flexible molecular chains, and these segments can provide additional flexibility in the epoxy resin matrix, which helps to absorb impact energy, thereby improving the impact resistance of the material. At the same time, the introduction of polyurethane can increase the free volume of epoxy resin and lower the glass transition temperature (Tg) of the resin, so that the material can maintain good flexibility at lower temperatures, and can more effectively absorb and disperse stress and avoid stress concentration.
[0024] Further research found that the molar ratio of the polyurethane prepolymer to the bisphenol A epoxy resin is 1: (1.5-4), which can make the adhesive achieve an efficient balance between mechanical strength, toughness and reshaping and reprocessing. With the increase of polyurethane content, the modulus of the material at room temperature gradually decreases (becomes softer), which is because the flexible segment characteristics of polyurethane enhance the flexibility of the material, reduce the overall rigidity, and make the material less likely to break when impacted. At the same time, the increase in polyurethane content is also accompanied by a decrease in glass transition temperature. The contribution of polyether soft segments to Tg is relatively low relative to the rigidity of high benzene rings in epoxy resin. However, the decrease in glass transition temperature also gives the material shape memory ability at room temperature. When polyurethane toughens epoxy resin, a special phase separation structure is formed, in which polyurethane is used as a dispersed phase and epoxy resin is used as a continuous phase. When this structure is impacted, the polyurethane phase can act as a stress concentration area, thereby improving the overall mechanical properties. With the increase of polyurethane content, the degree of phase separation gradually increases, and the phases become more continuous. The appropriate degree of phase separation helps to achieve a balance between the toughness and strength of the material, thanks to the dissociation and association of multi-level hydrogen bonds and dynamic covalent disulfide bonds.
[0025] Beneficial Effects
[0026] 1. By using disulfide bond-containing aromatic amine curing agent as a curing agent, polyurethane and epoxy resin can be combined to construct a dense cross-linked network structure with a shear strength of up to 11.9MPa.
[0027] 2. The molar ratio of the polyurethane prepolymer to the bisphenol A epoxy resin is 1:(1.5-4), which enables the adhesive to achieve an efficient balance between mechanical strength, toughness and reshaping and reprocessing.
[0028] 3. The adhesive prepared in this application obtains a continuous shape memory cycle through a stress control mode.
[0029] 4. After 6 cycles of bonding, the strength of the adhesive prepared in this application can still be maintained at 9.6 MPa.
[0030] 5. The adhesive prepared in this application can bond a variety of substrates, including steel-titanium, steel-iron, steel-zinc, steel-aluminum, and steel-magnesium.
[0031] 6. The adhesive prepared in this application has excellent bonding properties at 0-55°C. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 This is the NMR spectrum of Example 1.
[0033] Figure 2 The infrared spectra of Examples 1-5 are shown below.
[0034] Figure 3 This is the DSC curve of Example 1-5.
[0035] Figure 4 These are stress-strain curves for Examples 1-5.
[0036] Figure 5 Microscope images of the incision repaired at 120°C for different times using the adhesive of Example 3.
[0037] Figure 6 This is the engineering diagram of the adhesive shape memory recovery of Example 3. DETAILED DESCRIPTION
[0038] Examples 1-5
[0039] An epoxy-based adhesive with self-healing, shape memory and excellent bonding properties, the raw materials for preparation are: polyurethane prepolymer, bisphenol A epoxy resin (epoxy resin NPEL128 (E51), purchased from Nanya Electronic Materials Co., Ltd.), disulfide bond-containing aromatic amine curing agent and epoxy accelerator, and the raw material components are shown in Table 1.
[0040] The disulfide bond-containing aromatic amine curing agent is bis(2-aminophenyl) disulfide, and the epoxy accelerator is DMP-30, both of which are brands: Adamas.
[0041] The added amount of DMP-30 is 0.2 wt %.
[0042] The raw materials for preparing the polyurethane prepolymer are: polyether polyol, diisocyanate and catalyst.
[0043] The isocyanate is isophorone diisocyanate; the catalyst is dibutyltin dilaurate; the hydroxyl value of the first polyether polyol is 180-207 mgKOH / g, model: PPG600, brand: Adamas; the hydroxyl value of the second polyether polyol is 56 mgKOH / g, model: C3050A, brand: INOVOL.
[0044] The preparation method of the polyurethane prepolymer is as follows: PPG600 (6 g, 10 mmol) and C3050A (15 g, 5 mmol) are placed in a four-necked flask and vacuum dehydrated at 110° C. for 2 hours. The temperature is then lowered to 80° C., isophorone diisocyanate (7.78 g, 35 mmol) is added and stirred for 1 hour. Subsequently, a catalyst dibutyltin dilaurate (0.01 wt %) is added and prepolymerized for 3 hours.
[0045] A method for preparing an epoxy-based adhesive with self-healing, shape memory and excellent bonding properties comprises the following steps: mixing a polyurethane prepolymer, a bisphenol A epoxy resin, a disulfide bond-containing aromatic amine curing agent and an epoxy accelerator, stirring for 120 seconds at a speed of 2000 rpm in a vacuum defoaming mixer, curing at 80°C for 12 hours, and then curing at 120°C for 6 hours to obtain the adhesive.
[0046] The adhesives prepared in Examples 1-5 were named PDA-20, PDA-25, PDA-30, PDA-35 and PDA-40, respectively.
[0047] Table 1
[0048] Example Polyurethane prepolymer Bisphenol A epoxy resin Bis(2-aminophenyl) disulfide Example 1 (PDA-20) 17.5mmol 70.0mmol 87.5mmol Example 2 (PDA-25) 17.5mmol 52.5mmol 70.0mmol Example 3 (PDA-30) 17.5mmol 40.9mmol 58.4mmol Example 4 (PDA-35) 17.5mmol 32.5mmol 50.0mmol Example 5 (PDA-40) 17.5mmol 26.3mmol 43.8mmol
[0049] Performance testing methods and data
[0050] 1. Gel permeation chromatography (GPC) was used to test the molecular weight and molecular weight distribution of Examples 1-5. GPC was performed using Agilent LC1200, with DMF as the mobile phase, at 25°C, a flow rate of 1 mL / min, and a sample concentration of 1 mg / mL. The test data are listed in Table 2.
[0051] 2. Nuclear magnetic resonance characterization, Example 1: Nuclear magnetic resonance hydrogen spectrum (1HNMR) was obtained using a Bruker Avance 400 MHz NMR instrument from Germany with tetramethylsilane (TMS) as the internal standard. About 10 mg of the sample was dissolved in 0.50 mL of deuterated dimethyl sulfoxide (DMSO-d6) and scanned at 25°C. The test data are listed in Figure 1 middle.
[0052] 3. Infrared characterization, Examples 1-5: Infrared spectroscopy (FTIR) tests were performed using a German Bruker ALPHAII Fourier transform infrared spectrometer. The dissociation process of the samples was monitored using a variable temperature Fourier transform infrared spectrometer ranging from 30°C to 150°C, with a detection interval of 10°C and a heating rate of 5°C / min. The test data are listed in Figure 2 middle.
[0053] 4. Thermal analysis, Examples 1-5: DSC tests were performed using DSCQ2000 (TA, USA) under nitrogen with a heating rate of 10°C / min. The test data are listed in Figure 3 middle.
[0054] 5. Uniaxial tensile and tensile shear strength test, where the lap shear test and tensile test were carried out at a speed of 100 mm / min, referring to ASTM D5045 / E399. The test data are listed in Table 3, and the stress-strain curve is shown in Figure 4 shown.
[0055] 6. Example 3, shear strength test at different temperatures, the test data are listed in Table 4.
[0056] 7. Example 3, shear strength test under different cycle numbers, the test data are listed in Table 5, where the cycle scheme is as follows: initially, it rises to 70°C at 5°C / min, holds for 5 minutes, and balances at 0.1MPa for 5 minutes. Then it drops to 0°C at 4°C / min to release the force, and then heats to 70°C at 5°C / min and holds for a certain time to ensure complete shape recovery.
[0057] 8. Example 3, shear strength test under different bonding substrates, the test data are listed in Table 6.
[0058] 9. Repair performance test: The adhesive of Example 3 was cut from the middle of the sample at room temperature, and then the sections were spliced together. The repaired sample was repaired in a 120°C oven for different times. The microscope images of the cuts repaired at 120°C for different times are as follows: Figure 5 shown.
[0059] 10. Shape memory test: Figure 6As shown, the adhesive of Example 3 was raised to 70°C at 5°C / min, held for 5 minutes, and balanced at 0.1 MPa for 5 minutes, then dropped to 0°C at 4°C / min to release the force, and then heated to 70°C at 5°C / min and held for a certain time to fully recover the shape.
[0060] Table 2
[0061] Example Mn(g / mol) Mw(g / mol) PDI (polydispersity index) Example 1 (PDA-20) 20288 52457 2.5856 Example 2 (PDA-25) 21926 54545 3.0550 Example 3 (PDA-30) 23415 69778 2.9801 Example 4 (PDA-35) 30171 198889 6.5921 Example 5 (PDA-40) 29678 158849 5.3524
[0062] Table 3
[0063]
[0064] Table 4
[0065] Temperature(℃) Shear strength(MPa) 0 7.143 25 11.909 35 10.413 45 7.201 55 5.617
[0066] Table 5
[0067]
[0068]
[0069] Table 6
[0070] Bonding substrate Shear strength(MPa) Steel-Titanium 10.977 Steel-Iron 9.941 Steel-Zinc 9.665 Steel-Aluminum 7.673 Steel-Magnesium 6.091
Claims
1. An epoxy-based adhesive with self-healing, shape memory and excellent bonding properties, It is characterized in that The preparation raw materials include: polyurethane prepolymer, bisphenol A type epoxy resin, disulfide bond-containing aromatic amine curing agent and epoxy accelerator.
2. The epoxy-based adhesive having self-healing, shape memory and excellent bonding properties according to claim 1, It is characterized in that The raw materials for preparing the polyurethane prepolymer include: polyether polyol, diisocyanate and a catalyst.
3. The epoxy-based adhesive having self-healing, shape memory and excellent bonding properties according to claim 2, It is characterized in that The molar ratio of the polyether polyol to the diisocyanate is 1:(2-3).
4. The epoxy-based adhesive having self-healing, shape memory and excellent bonding properties according to claim 2 or 3, It is characterized in that The polyether polyol comprises a first polyether polyol and a second polyether polyol, wherein the hydroxyl value of the first polyether polyol is 120-250 mgKOH / g, and the hydroxyl value of the second polyether polyol is 30-100 mgKOH / g.
5. The epoxy-based adhesive having self-healing, shape memory and excellent bonding properties according to claim 4, It is characterized in that The molar ratio of the first polyether polyol to the second polyether polyol is (1-3):
1.
6. The epoxy-based adhesive having self-healing, shape memory and excellent bonding properties according to claim 1 or 5, It is characterized in that The molar ratio of the polyurethane prepolymer to the bisphenol A epoxy resin is 1:(1. 5-4)。 7. The epoxy-based adhesive having self-healing, shape memory and excellent bonding properties according to claim 6, It is characterized in that The disulfide bond-containing aromatic amine curing agent includes at least one of 4,4'-dithiodiphenylamine, bis(3-fluoro-4-aminophenyl) disulfide, 2-[(2-amino-5-isopropylphenyl) dithio]-4-isopropylaniline, bis(2-aminophenyl) disulfide, [2-(2-amino-5-methoxy-phenyl) dithio-4-methoxy-phenyl] amine, 2-[(2-amino-5-methylphenyl) dithio]-4-methylaniline, 2-[(2-amino-5-ethylphenyl) dithio]-4-ethylaniline, 5,5'-disulfanediylbis(2-chloroaniline), bis(2-amino-4-methylphenyl) disulfide, 2,2'-dithiodi(1-naphthylamine), and 6,6-disulfidediylbis(2-methylaniline).
8. The epoxy-based adhesive having self-healing, shape memory and excellent bonding properties according to claim 7, It is characterized in that The epoxy accelerator includes at least one of DMP-30, imidazole, triethanolamine and resorcinol.
9. A method for preparing an epoxy-based adhesive having self-healing, shape memory and excellent bonding properties according to any one of claims 1 to 8, It is characterized in that The method comprises the following steps: mixing polyurethane prepolymer, bisphenol A epoxy resin, disulfide bond-containing aromatic amine curing agent and epoxy accelerator, stirring evenly in a vacuum defoaming mixer, and curing to obtain the product.
10. The method for preparing the epoxy-based adhesive having self-healing, shape memory and excellent bonding properties according to claim 9, It is characterized in that The curing is performed in sequence of low temperature curing and high temperature curing; the conditions of the low temperature curing are: curing at 60-90°C for 10-15h; the conditions of the high temperature curing are: curing at 110-130°C for 4-7h.
Citation Information
Patent Citations
High temperature resistant, high strength modified epoxy resin adhesive and preparation thereof
CN101407708A
Process for preparing normal temp solidification polyurethane toughened epoxy resin adhesive
CN1143661A
Waterproof leaking stoppage polyurethane as well as preparation method and application thereof
CN117024704A
Modified epoxy resin and curable resin composition
JP2007246648A
Toughened two component epoxy structural adhesive
WO2023239857A1
Cited By
Long-acting durable waterproof coating with self-repairing function and synthesis method thereof
CN120665495A