Single-particle explosion type fluorescent scintillation carbon dot as well as preparation method and application thereof

By adding nitrogen source dopant to the heating and oxidation reaction between carbon structure materials and oxidant, a single-particle burst fluorescent scintillation carbon dot with uniform particle size and short fluorescence scintillation period was prepared, and the carbon dot particle size distribution in the prior art was solved. The problems of unevenness and irregular flickering have realized the application of quantitative analysis of super-resolution fluorescence imaging.

CN118895124AInactive Publication Date: 2024-11-05XI'AN PETROLEUM UNIVERSITY
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410895943.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-11-05
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the prior art, the uneven distribution of carbon dot particle size, long fluorescence scintillation period and irregular scintillation results in the fluorescent markers being easily bleached and have poor stability, making it difficult to achieve super-resolution quantitative analysis.

Method used

The carbon structure material and oxidizing agent are used to heat and oxidize in water, and nitrogen source dopants are added for high-temperature treatment. Through multiple filtration and drying, a single-particle burst fluorescent scintillation carbon dot with uniform particle size is obtained, which is used for receptor proteins on the cell membrane. Quantitative analysis of aggregation of super-resolution fluorescence imaging.

Benefits of technology

The particle size distribution of single-particle burst fluorescent scintillation carbon dots is achieved, with a short and regular fluorescent scintillation cycle, and has burst scintillation characteristics. It can be used for super-resolution fluorescence imaging quantitative analysis of receptor protein aggregation on cell membranes to obtain receptor aggregation. Information on the size, distribution density and proportion of the body.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895124A_ABST
    Figure CN118895124A_ABST
Patent Text Reader

Abstract

The invention discloses a single-particle explosion type fluorescent scintillation carbon dot and a preparation method and application thereof, and relates to the field of fluorescence imaging, and the preparation method comprises the following steps: dissolving a carbon material and an oxidant in water, and carrying out a heating oxidation reaction to obtain a carbon nanoparticle mixed solution; adding a nitrogen source dopant into the carbon nanoparticle mixed solution, carrying out a reaction to obtain a nitrogen-doped solution, and carrying out a high-temperature heating reaction to obtain a mixed solution after amination treatment; cooling, centrifuging and drying the aminated mixed solution, performing rotary evaporation concentration on an intermediate product, performing freeze drying, and collecting a carbon nanoparticle product; respectively filtering, washing and centrifuging dispersion liquid formed by dissolving the carbon nanoparticle product in water in filtering equipment with the molecular weight cut-off of 30kDa and 5kDa, and then collecting the single-particle explosive fluorescent scintillation carbon dots. According to the preparation method provided by the invention, the prepared single-particle explosive fluorescent scintillation carbon dots are uniform in particle size distribution, short in fluorescent scintillation period and regular in scintillation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a plurality of technical fields such as nanotechnology, fluorescence imaging, biomedical engineering and material preparation, and in particular to a single-particle burst-type fluorescent scintillation carbon dot and a preparation method and application thereof. Background Art

[0002] In modern biological imaging technology, super-resolution fluorescence imaging has become one of the key technologies for studying the fine structures inside biological molecules and cells because it can break through the optical diffraction limit. However, to achieve super-resolution fluorescence imaging, the key lies in the development of fluorescent nanoprobes with excellent fluorescence blinking properties. Traditional fluorescent probes such as organic dyes and fluorescent proteins are often difficult to meet the needs of high-resolution imaging in time and space due to the easy bleaching, instability and limitations of fluorescence intensity.

[0003] Carbon dots are a type of carbon-based fluorescent nanomaterial with a size of less than 10 nm. Their fluorescence flickering behavior originates from the rich energy levels and defect structures on the surface of carbon dots. When irradiated by an excitation light source, the electrons inside the carbon dots will transition and transfer between different energy levels, resulting in fluorescence flickering. This flickering behavior enables carbon dots to emit strong fluorescence signals in a very short time, thereby achieving high-precision positioning and imaging of biological molecules. Therefore, it has shown great application potential in the field of super-resolution fluorescence imaging. However, it is not easy to prepare single-particle flickering carbon dots with excellent fluorescence flickering properties. Although traditional preparation methods such as arc discharge and laser ablation can produce carbon dots, they often have problems such as uneven particle size distribution, long fluorescence flickering period or irregular flickering.

[0004] Patent CN111334067B discloses a self-scintillating fluorescent dye that can be used for super-resolution fluorescence imaging and its synthesis and application. The dye has the characteristics of high quantum yield and high stability by introducing azetidine at the 4,5-position of silicon rhodamine to inhibit intramolecular rotation. At the same time, the fluorescent and non-fluorescent forms of the probe can be mutually converted through intramolecular action under normal physiological conditions, so that it can be applied to super-resolution imaging of living cells. The dye can be combined with antibodies to specifically label and image tubulin in cells. The dye can be widely used in the fields of protein labeling and super-resolution fluorescence imaging. However, in the actual application process, the self-scintillating fluorescent dye will undergo rapid photobleaching under the irradiation of strong lasers, and because the labeling ratio between it and the protein cannot be determined, it is even more impossible to realize the distribution and quantitative research of membrane proteins such as G-protein coupled receptors and epidermal growth factor receptors on the cell membrane, such as the size of receptor aggregates, distribution density, the number of receptor proteins in the aggregates, and the proportion of aggregated receptor molecules.

[0005] Therefore, developing a new preparation method to obtain carbon dots with high brightness, high stability and short blinking period is of great significance for promoting the development of super-resolution fluorescence imaging technology. Summary of the invention

[0006] The present invention provides a single-particle burst-type fluorescent scintillation carbon dot and its preparation method and application, so as to overcome the problems of uneven carbon dot particle size distribution, long fluorescent scintillation period and irregular scintillation in the prior art, as well as technical problems such as easy bleaching of fluorescent markers, poor stability and limitations in super-resolution quantitative analysis applications.

[0007] In order to achieve the above object, the technical solution of the embodiment of the present invention is:

[0008] The first aspect of the present invention provides a method for preparing single-particle burst-type fluorescent scintillating carbon dots, comprising:

[0009] Dissolving the carbon material and the oxidant in water, and performing a heating oxidation reaction to obtain a carbon nanoparticle mixed solution;

[0010] Adding a nitrogen source dopant to the carbon nanoparticle mixed solution, performing a high temperature reaction to obtain a nitrogen-doped solution, and performing a high temperature heating reaction on the nitrogen-doped solution to obtain an amination-treated mixed solution;

[0011] The mixed solution after the amination treatment is cooled, centrifuged and dried, and the intermediate product is concentrated by rotary evaporation and freeze-dried to collect the carbon nanoparticle product;

[0012] The dispersion formed by dissolving the carbon nanoparticle product in water is filtered, washed and centrifuged in filter devices with a molecular weight cutoff of 30 kDa and 5 kDa, respectively, to collect single-particle burst-type fluorescent flashing carbon dots.

[0013] In combination with the first aspect, preferably, the carbon structural material is one or more of carbon black, graphite, graphene and carbon nanotubes;

[0014] And / or, the added amount of the carbon structural material is 0.1-1.0 g / L.

[0015] In combination with the first aspect, preferably, the oxidant is one or more of nitric acid and sulfuric acid.

[0016] In combination with the first aspect, preferably, the added amount of the oxidant is 30-100 mL.

[0017] In combination with the first aspect, preferably, when the heating oxidation reaction is carried out, the reaction temperature is 120-200° C. and the reaction time is 4-24 h.

[0018] In combination with the first aspect, preferably, the nitrogen source dopant is one or more of ethylenediamine, urea, geranylamine, cyanamide, oleylamine, dimethylpyridylamine, trimethylamine borane, and thiazole-5-amine.

[0019] In combination with the first aspect, preferably, the added amount of the nitrogen source dopant is 0.5 g.

[0020] In combination with the first aspect, preferably, when the high temperature heating reaction is carried out, the high temperature is 170° C. and the reaction time is 2-6 hours.

[0021] The second aspect of the present invention provides a single-particle burst-type fluorescent scintillating carbon dot prepared as described in the first aspect.

[0022] The third aspect of the present invention provides an application of the single-particle burst-type fluorescent scintillating carbon dots prepared in the first aspect or the single-particle burst-type fluorescent scintillating carbon dots described in the second aspect in super-resolution fluorescent imaging quantitative analysis of receptor protein aggregation on cell membranes.

[0023] Compared with the prior art, the advantages or beneficial effects of the embodiments of the present invention include at least:

[0024] The preparation method provided by the present invention uses carbon structural material as carbon precursor, water as solvent, nitric acid or sulfuric acid or diacid combination as oxidant, cuts the carbon material of macromolecular structure into nano-scale carbon dots by oxidation cutting, filters, adds nitrogen source dopant and then heats at high temperature to obtain a solution after amino; then cools, centrifuges, dries, rotary evaporates and concentrates, freeze-dries to obtain carbon dot products with larger particle size; performs multiple ultrafiltration in a filter device with a molecular weight cutoff of 30kDa and 5kDa to obtain single-particle burst-type fluorescent flashing carbon dots with a size of 5nm. In this way, the preparation method provided by the present application can, on the one hand, make the prepared single-particle burst-type fluorescent flashing carbon dots have uniform particle size distribution, short fluorescent flashing period and flashing regularity; on the other hand, make the prepared single-particle burst-type fluorescent flashing carbon dots have the characteristics of burst-type flashing; thirdly, it can also be used to realize super-resolution fluorescence imaging quantitative analysis of receptor protein aggregation on cell membrane, and can obtain information such as the size, distribution density, number of receptor proteins in the aggregates and proportion of aggregated receptor molecules of receptor aggregates. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a total internal reflection single-particle fluorescence imaging image of a single-particle burst-type fluorescent scintillating carbon dot prepared in Example 1;

[0026] Figure 2 The flashing trajectory diagram of the single-particle burst-type fluorescent flashing carbon dots prepared in Example 2;

[0027] Figure 3(a) is a super-resolution fluorescence imaging image of CXCR4 protein on the Hela cell membrane, (b) is a super-resolution fluorescence imaging rendering of chemokine receptor protein on the Hela cell membrane, and (c) is a super-resolution fluorescence imaging quantitative analysis result of the aggregation state of chemokine receptor protein on the Hela cell membrane;

[0028] Figure 4 This is a total internal reflection single-particle fluorescence imaging image of a single-particle burst-type fluorescent scintillating carbon dot prepared in Example 2;

[0029] Figure 5 This is a flashing trajectory diagram of a single-particle burst-type nano fluorescent carbon dot prepared in Example 3;

[0030] Figure 6 This is a transmission electron microscope image of a single-particle burst-type fluorescent flashing carbon dot prepared in Example 5. DETAILED DESCRIPTION

[0031] In order to make the purpose, technical solutions and advantages of the present invention clearer, the present invention will be further described in detail below in conjunction with the accompanying drawings. The described embodiments should not be regarded as limiting the present invention. All other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention.

[0032] In the following description, reference is made to "some embodiments", which describe a subset of all possible embodiments, but it is understood that "some embodiments" may be the same subset or different subsets of all possible embodiments, and may be combined with each other without conflict. Unless otherwise defined, all technical and scientific terms used in the embodiments of the present invention have the same meaning as those commonly understood by those skilled in the art to which the embodiments of the present invention pertain. The terms used in the embodiments of the present invention are only for the purpose of describing the embodiments of the present invention and are not intended to limit the present invention.

[0033] In the following description of this embodiment, the terms "include", "comprising", "having" and "containing" are all open terms, meaning including but not limited to.

[0034] It should be noted that all raw materials / reagents in the embodiments of the present invention can be purchased on the market or prepared according to conventional methods well known to those skilled in the art; the term "and / or" in the embodiments of the present invention is only used to describe the association relationship between associated objects, indicating that three relationships may exist, for example, A and / or B means the existence of A alone, B alone, and A and B at the same time, wherein A and B can be singular or plural, and the character " / " generally indicates that the associated objects before and after are in an "or" relationship.

[0035] In the following description of this embodiment, the term "at least one" refers to one or more, and "plurality" refers to two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b or c", or "at least one of a, b and c", can all represent: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.

[0036] Those skilled in the art should understand that in the following description of the embodiments of the present invention, the order of serial numbers does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present invention.

[0037] The terms used in the embodiments of the present invention are only for the purpose of describing specific embodiments, and are not intended to limit the present invention. The singular forms "a", "an" and "the" used in the embodiments of the present invention and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.

[0038] It will be appreciated by those skilled in the art that the numerical ranges in the embodiments of the present invention are to be understood as also specifically disclosing each intermediate value between the upper and lower limits of the range. Each smaller range between the intermediate values ​​in any stated value and stated range and any other stated value or intermediate value in the range is also included in the present invention. The upper and lower limits of these smaller ranges may be independently included or excluded in the range.

[0039] Unless otherwise specified, the technical / scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention only describes preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the embodiments or test cases of the present invention. All documents mentioned in this specification are generally incorporated by reference to disclose and describe methods and / or materials related to the documents. In the event of a conflict with any incorporated document, the content of the present invention shall prevail.

[0040] It should be noted that all raw materials and / or reagents in the examples of the present invention are purchased on the market or prepared according to conventional methods well known to those skilled in the art.

[0041] In a first aspect, an embodiment of the present invention provides a method for preparing a single-particle burst-type fluorescent scintillating carbon dot, the preparation method comprising:

[0042] S10: dissolving the carbon material and the oxidant in water, and performing a heating oxidation reaction to obtain a carbon nanoparticle mixed solution;

[0043] S20: adding a nitrogen source dopant to the carbon nanoparticle mixed solution, reacting to obtain a nitrogen-doped solution, and heating the nitrogen-doped solution at a high temperature to obtain an amination-treated mixed solution;

[0044] S30: cooling, centrifuging and drying the mixed solution after the amination treatment, concentrating the intermediate product by rotary evaporation and freeze drying, and collecting the carbon nanoparticle product;

[0045] S40: The dispersion formed by dissolving the carbon nanoparticle product in water is filtered, washed and centrifuged in filter devices with a molecular weight cutoff of 30 kDa and 5 kDa, and then single-particle burst-type fluorescent flashing carbon dots are collected.

[0046] The preparation method provided by the present invention uses carbon structural material as carbon precursor, water as solvent, nitric acid or sulfuric acid or diacid combination as oxidant, cuts the carbon material of macromolecular structure into nano-scale carbon dots by oxidation cutting, filters, adds nitrogen source dopant and then heats at high temperature to obtain a solution after amino; then cools, centrifuges, dries, rotary evaporates and concentrates, freeze-dries to obtain carbon dot products with larger particle size; performs multiple ultrafiltration in a filter device with a molecular weight cutoff of 30kDa and 5kDa to obtain single-particle burst-type fluorescent flashing carbon dots with a size of 5nm. In this way, the preparation method provided by the present application can, on the one hand, make the prepared single-particle burst-type fluorescent flashing carbon dots have uniform particle size distribution, short fluorescent flashing period and flashing regularity; on the other hand, make the prepared single-particle burst-type fluorescent flashing carbon dots have the characteristics of burst-type flashing; thirdly, it can also be used to realize super-resolution fluorescence imaging quantitative analysis of receptor protein aggregation on cell membrane, and can obtain information such as the size, distribution density, number of receptor proteins in the aggregates and proportion of aggregated receptor molecules of receptor aggregates.

[0047] It should be noted that in the above step S10, carbon black, graphite, graphene, carbon nanotubes and other carbon structural materials are used as carbon precursors, water is used as solvent, nitric acid and sulfuric acid or a combination of the two acids are used as oxidants to oxidize the carbon structural materials, and the reaction is heated at 120-200°C for 4-24h to decompose the large-structure carbon materials into nano-sized carbon dots to obtain a nano-scale carbon nanoparticle mixed solution.

[0048] It should be noted that, in the above step S20, before adding the nitrogen source dopant to the carbon nanoparticle mixed solution, the carbon nanoparticle mixed solution needs to be filtered. In the present invention, a 0.22 μm filter head can be used to filter the carbon nanoparticle mixed solution. Of course, the nanoparticle mixed solution can also be filtered using filter heads of other sizes or filtering methods. In the embodiment of the present invention, the form of the filtering method and the size of the filter head are not specifically limited.

[0049] In the above step S30, the mixed solution after the amination treatment is cooled to room temperature (25°C), collected in a 50mL centrifuge tube, centrifuged to remove the undissolved matter, and the supernatant is added to a round-bottom flask and dried using a heating jacket; it is preferably heated until there is no flowing liquid in the bottle and there is steam at the bottle mouth; the dried sample at the bottom of the bottle is washed out with a small amount of ultrapure water; the carbon dot product is concentrated by rotary evaporation, and then freeze-dried and the sample is collected, i.e., the carbon nanoparticle product.

[0050] In the above step S40, the carbon nanoparticle product is taken, dissolved with ultrapure water, loaded into the upper cavity of an ultrafiltration tube with a molecular weight cutoff of 30kDa, and ultrafiltration centrifuged to obtain a permeated solution; the permeated carbon dot solution is loaded into the upper cavity of an ultrafiltration tube with a molecular weight cutoff of 5kDa, centrifuged and ultrafiltered to obtain an upper solution, and washed once with ultrapure water to obtain the washed upper solution again, thereby obtaining a single-particle burst-type fluorescent flashing carbon dot of 5k-30kDa.

[0051] In a specific embodiment, the carbon structural material in the embodiment of the present invention is preferably one of carbon black, graphite, graphene and carbon nanotubes.

[0052] In a specific embodiment, the added amount of the carbon structural material in the embodiment of the present invention is preferably 0.1-1.0 g / L.

[0053] It should be noted that the addition of an appropriate amount of carbon structural material can ensure that the carbon precursor fully reacts with other components in the reaction system, thereby increasing the yield of carbon dots. Excessive addition may cause the reaction system to become viscous, affecting the uniformity of stirring and mixing, thereby reducing the yield and dispersibility of carbon dots. In addition, the addition amount of carbon precursor can affect the morphology and size of carbon dots. An appropriate amount of addition helps to form a uniform and regular carbon dot morphology. Excessive or insufficient addition may result in irregular carbon dot morphology and uneven size distribution.

[0054] In a specific embodiment, the oxidant in the embodiment of the present invention is preferably one of nitric acid and sulfuric acid or a mixture of these two acids in a ratio of 1:1.

[0055] It should be noted that the oxidant in the embodiment of the present invention plays the role of oxidation cutting, that is, oxidation cutting of the carbon structure material with a macromolecular structure into nano-scale carbon dots.

[0056] It should be noted that the amount of oxidant added has the following effects on carbon dots: 1) Reaction rate: An appropriate amount of oxidant can provide sufficient oxidizing power to promote the rapid cutting and oxidation of macromolecular carbon structural materials, thereby accelerating the formation of carbon dots. When the amount of oxidant added is insufficient, the reaction rate may decrease, resulting in a prolonged reaction time and a reduced yield of carbon dots. However, excessive addition of oxidant may also lead to a too fast reaction rate, or even induce a violent reaction, affecting the quality and morphology of carbon dots. 2) Morphology and size of carbon dots: An appropriate amount of oxidant can make macromolecular carbon structural materials cut uniformly to form carbon dots with a narrow size distribution and regular morphology. When the amount of oxidant added is insufficient, the cutting may be uneven, resulting in a wide size distribution of carbon dots and irregular morphology. On the contrary, too much oxidant may lead to over-cutting, making the carbon dots too small in size, or even forming carbon oxides or other impurities. 3) Carbon dot performance: An appropriate amount of oxidant can ensure that the carbon dots have good electrical conductivity, thermal stability, chemical stability and other properties. Excessive oxidant may introduce too much oxygen, affecting the electrical conductivity and stability of carbon dots. At the same time, excessive oxidants may also produce by-products, such as acidic substances, which have a negative impact on the chemical stability of carbon dots. 4) Nonspecific cleavage: Excessive oxidants may lead to nonspecific cleavage, causing carbon dots to lose their original structure and properties.

[0057] In a specific embodiment, the amount of the oxidant added in the embodiment of the present invention is preferably 30-100 mL.

[0058] In a specific embodiment, when the heating oxidation reaction is carried out in the embodiment of the present invention, the reaction temperature is preferably 120-200° C., and the reaction time is preferably 4-24 hours.

[0059] It should be noted that the effects of reaction temperature on carbon dots are as follows: 1) A higher reaction temperature can enhance the oxidizing ability of nitric acid or sulfuric acid, making the carbon precursor easier to be oxidized and cut, thereby obtaining carbon dots with a higher degree of oxidation. For example, at a higher temperature, the oxidizing ability of nitric acid is higher, and carbon dots with a longer emission wavelength can be formed in a short time. 2) A higher temperature may cause the cutting speed to be too fast, resulting in a smaller size or irregular morphology of the carbon dots. A lower temperature may cause the cutting speed to be too slow, resulting in a larger size or uneven distribution of the carbon dots.

[0060] It should be noted that the effects of reaction time on carbon dots are as follows: 1) Prolonging the reaction time can increase the surface oxidation degree of carbon dots. For example, when oxidatively cutting a carbon precursor in nitric acid or sulfuric acid, prolonging the reaction time can allow the carbon precursor to be more fully oxidatively cut to obtain carbon dots with a higher degree of oxidation. 2) The reaction time will also affect the yield of carbon dots. Appropriate reaction time can ensure that the carbon precursor reacts fully and obtains a higher yield of carbon dots. However, too long a reaction time may cause excessive oxidation or decomposition of the carbon dots, thereby reducing the yield.

[0061] In a specific embodiment, the nitrogen source dopant in the embodiment of the present invention is one of ethylenediamine, urea, geranylamine, cyanamide, oleylamine, dimethylpyridylamine, trimethylamine borane, and thiazole-5-amine.

[0062] It should be noted that the advantages of the nitrogen source dopants selected in the present invention are mainly reflected in the nitrogen source supply capacity, stability, catalytic activity and unique chemical properties. Among them, geranylamine as a nitrogen source dopant has excellent supply capacity and helps to provide a stable nitrogen supply.

[0063] It should be noted that the added amount of the nitrogen source dopant in the embodiment of the present invention is preferably 0.5 g.

[0064] In a specific embodiment, when a high temperature heating reaction is carried out in the embodiment of the present invention, the high temperature is preferably 170° C., and the reaction time is preferably 2-6 hours.

[0065] In a second aspect, an embodiment of the present invention provides a single-particle burst-type fluorescent scintillating carbon dot prepared by the method described in the first aspect.

[0066] In the third aspect, an embodiment of the present invention provides an application of the single-particle burst-type fluorescent flashing carbon dots prepared by the method described in the first aspect or the single-particle burst-type fluorescent flashing carbon dots described in the second aspect in the super-resolution fluorescence imaging quantitative analysis of receptor protein aggregation on the cell membrane.

[0067] The single-particle burst-type fluorescent flashing carbon dots obtained by the preparation method provided by the present invention can be used to realize super-resolution fluorescence imaging quantitative analysis of receptor protein aggregation on the cell membrane, and can obtain information such as the size, distribution density, number of receptor proteins in the aggregates, and proportion of aggregated receptor molecules of the receptor aggregates.

[0068] The present invention provides a method for characterizing the fluorescence scintillation of a single-particle burst-type fluorescence scintillation carbon dot:

[0069] Using a Nikon A1 confocal microscope with high detection sensitivity, total internal reflection and epi-fluorescence imaging systems, under a 100x oil objective (NA=1.49), with appropriate filters (532nm laser, 570nm dichroic mirror, 590nm long-pass emission filter), and with the help of an Andor 897 single-molecule EMCCD, single-particle carbon dots were imaged to investigate the fluorescence properties of single carbon dots, such as fluorescence blinking behavior, photostability and fluorescence brightness.

[0070] The present invention provides a carbon dot super-resolution fluorescence imaging method for quantitatively analyzing the aggregation of G protein-coupled receptors on cell membranes:

[0071] The antibody fragments were obtained by enzymatic hydrolysis, and the antibodies were modified onto the carbon dots by chemical cross-linking based on the carboxyl and amino groups on the surface of the carbon dots under the activation of EDC-NHS. The binding ratio of CDs to antibodies was optimized to obtain a probe with a binding ratio of 1:1, which was used for specific labeling of receptor proteins on cell membranes.

[0072] The ThunderSTORM plug-in of the open software ImageJ was used to locate, fit and superimpose the single particle positions in the continuously collected image sequence to complete the super-resolution reconstruction. The spatial clustering analysis method of single particle positioning, such as Ripley's K and other functions, was used to carry out super-resolution imaging quantitative analysis to obtain information such as receptor distribution and aggregation (aggregate size, distribution and the number of receptor molecules contained in the aggregate).

[0073] In summary, the fluorescent carbon dots prepared in the present invention not only have the characteristic of explosive flashing, but can also be used to realize super-resolution fluorescence imaging quantitative analysis of receptor protein aggregation on cell membranes, and can obtain information such as the size and distribution density of receptor aggregates, the number of receptor proteins in the aggregates, and the proportion of aggregated receptor molecules.

[0074] The technical method of the present invention will be further described below in conjunction with specific embodiments.

[0075] Example 1

[0076] This embodiment provides a method for preparing a single-particle burst-type fluorescent scintillating carbon dot 1, and the specific steps are as follows:

[0077] (1) dissolving the carbon material and the oxidant in water, and performing a heating oxidation reaction to obtain a carbon nanoparticle mixed solution:

[0078] Weigh 0.5 g of carbon black and 50 mL of ultrapure water, add them into a 250 mL round-bottom flask respectively, and mix them by ultrasonic mixing for 20 min; add 50 mL of nitric acid, mix well and wipe off the water on the outside of the round-bottom flask; build a condensation reflux device, put the above round-bottom flask into an oil bath, heat the reaction at 120 ° C for 24 h to obtain a mixed solution of carbon nanoparticles.

[0079] (2) Adding a nitrogen source dopant to the carbon nanoparticle mixed solution, reacting to obtain a nitrogen-doped solution, and heating the nitrogen-doped solution at a high temperature to obtain an amination-treated mixed solution:

[0080] The carbon nanoparticle mixed solution was cooled to room temperature (25°C), filtered with a 0.22 μm filter head, and then 0.5 g of geranylamine was added to obtain a nitrogen-doped solution; the nitrogen-doped solution was heated at high temperature again for 4 hours to obtain an amination-treated mixed solution.

[0081] (3) After cooling, centrifuging and drying the mixed solution after the amination treatment, the intermediate product is concentrated by rotary evaporation and freeze-dried to collect the carbon nanoparticle product:

[0082] The mixed solution after amination treatment was cooled to room temperature (25°C), collected in a 50 mL centrifuge tube, centrifuged to remove undissolved matter, and the supernatant was added to a round-bottom flask and dried using a heating jacket; it was heated until there was no flowing liquid in the bottle and there was steam at the bottle mouth; the dried sample at the bottom of the bottle was washed out with a small amount of ultrapure water; the carbon nanoparticle product was concentrated by rotary evaporation, and then freeze-dried and collected.

[0083] (4) The dispersion formed by dissolving the carbon nanoparticle product in water is filtered, washed and centrifuged in filter devices with a molecular weight cutoff of 30 kDa and 5 kDa, and single-particle burst-type fluorescent flashing carbon dots are collected:

[0084] Take 10 mg of the carbon dot product, dissolve it with ultrapure water, load it into the upper cavity of an ultrafiltration tube with a molecular weight cutoff of 30 kDa, perform ultrafiltration centrifugation, and obtain a permeated solution; load the permeated carbon dot solution into the upper cavity of an ultrafiltration tube with a molecular weight cutoff of 5 kDa, and perform centrifugal ultrafiltration to obtain an upper solution; wash the upper solution once with ultrapure water by centrifugation, and obtain the washed upper solution again to obtain a single-particle burst-type fluorescent flashing carbon dot 1 of 5-30 kDa.

[0085] Using a Nikon A1 confocal microscope with high detection sensitivity, total internal reflection and epifluorescence imaging system, under a 100x oil objective (NA = 1.49), with appropriate filters (532nm laser, 570nm dichroic mirror, 590nm long-pass emission filter), and with the help of an Andor 897 single-molecule EMCCD, single-particle carbon dots were imaged. Thus, a fluorescence imaging image of a single-particle burst-type fluorescent flashing carbon dot 1 was obtained, as shown in FIG. Figure 1 As shown in the figure, the fluorescence signal intensity of the single-particle burst-type fluorescent flashing carbon dots changes with time, that is, the flashing trajectory of the single-particle burst-type fluorescent flashing carbon dots is shown in Figure 2 shown.

[0086] In the present invention, the obtained single-particle burst-type fluorescent flashing carbon dots are combined with the enzymatically hydrolyzed CXCR4 antibody fragment in a ratio of 1:1, and used for specific labeling of CXCR4 chemokine receptors on the cell membrane and quantification of CXCR4 aggregation and distribution, and the size and distribution of aggregates and the number of receptor molecules contained in the aggregates are obtained. Figure 3 As shown, the results showed that the CXCR4 receptor protein was distributed in clusters on the cell membrane, and the clusters included 87% monomers, 12% dimers, about 1% trimers and tetramers, and 0 pentamers.

[0087] Example 2

[0088] This embodiment provides a method for preparing a single-particle burst-type fluorescent scintillating carbon dot 2, and the specific steps are as follows:

[0089] (1) dissolving the carbon material and the oxidant in water, and performing a heating oxidation reaction to obtain a carbon nanoparticle mixed solution:

[0090] Weigh 0.5 g of graphite and 50 mL of ultrapure water, add them into a 250 mL round-bottom flask respectively, and mix them by ultrasonic mixing for 20 min; add 80 mL of sulfuric acid, mix well, and wipe off the moisture on the outside of the round-bottom flask; build a condensation reflux device, put the above round-bottom flask into an oil bath, and heat the reaction at 160 ° C for 20 h to obtain a mixed solution of carbon nanoparticles.

[0091] (2) Adding a nitrogen source dopant to the carbon nanoparticle mixed solution, reacting to obtain a nitrogen-doped solution, and heating the nitrogen-doped solution at a high temperature to obtain an amination-treated mixed solution:

[0092] The carbon dot solution was cooled to room temperature (25°C), filtered with a 0.22 μm filter head, and then 0.5 g of cyanamide was added to obtain a nitrogen-doped solution; the nitrogen-doped solution was heated at high temperature again for 6 hours to obtain a mixed solution after amino treatment.

[0093] (3) After cooling, centrifuging and drying the mixed solution after the amination treatment, the intermediate product is concentrated by rotary evaporation and freeze-dried to collect the carbon nanoparticle product:

[0094] The mixed solution after amination treatment was cooled to room temperature (25°C), collected in a 50 mL centrifuge tube, centrifuged to remove undissolved matter, and the supernatant was added to a round-bottom flask and dried using a heating jacket; it was heated until there was no flowing liquid in the bottle and there was steam at the bottle mouth; the dried sample at the bottom of the bottle was washed out with a small amount of ultrapure water; the carbon dot product was concentrated by rotary evaporation, and then freeze-dried and the carbon nanoparticle product was collected.

[0095] (4) The dispersion formed by dissolving the carbon nanoparticle product in water is filtered, washed and centrifuged in filter devices with a molecular weight cutoff of 30 kDa and 5 kDa, and single-particle burst-type fluorescent flashing carbon dots are collected:

[0096] Take 10 mg of the carbon nanoparticle product, dissolve it with ultrapure water, load it into the upper cavity of an ultrafiltration tube with a molecular weight cutoff of 30 kDa, perform ultrafiltration centrifugation, and obtain a permeated solution; load the permeated carbon dot solution into the upper cavity of an ultrafiltration tube with a molecular weight cutoff of 5 kDa, and perform centrifugal ultrafiltration to obtain an upper solution; wash the upper solution once with ultrapure water by centrifugation, and obtain the washed upper solution again to obtain a single-particle burst-type fluorescent flashing carbon dot 2 of 5-30 kDa.

[0097] According to the test method described in Example 1, the fluorescence imaging image of the single-particle burst-type fluorescent scintillation carbon dot 2 is obtained, as shown in FIG. Figure 4 As shown, the curve of the change of the fluorescence signal intensity of the single-particle burst-type fluorescent flashing carbon dot over time, that is, the flashing trajectory of the single-particle burst-type fluorescent flashing carbon dot, is statistically calculated.

[0098] In the present invention, the obtained single-particle burst-type fluorescent flashing carbon dots 2 are combined with the enzymatically hydrolyzed CCR3 antibody fragment in a ratio of 1:1, and are used for specific labeling of CCR3 chemokine receptors on the cell membrane and quantification of CCR3 aggregation and distribution, so as to obtain the aggregate size, distribution and the number of receptor molecules contained in the aggregate.

[0099] Example 3

[0100] This embodiment provides a method for preparing a single-particle burst-type fluorescent scintillating carbon dot 3, and the specific steps are as follows:

[0101] (1) dissolving the carbon material and the oxidant in water, and performing a heating oxidation reaction to obtain a carbon nanoparticle mixed solution:

[0102] Weigh 0.5 g of carbon nanotubes and 50 mL of ultrapure water, add them into a 250 mL round-bottom flask respectively, and mix them by ultrasonic mixing for 20 min; add 40 mL of sulfuric acid and nitric acid respectively, mix well, and wipe off the water on the outside of the round-bottom flask; build a condensation reflux device, put the above round-bottom flask into an oil bath, and heat the reaction at 160 ° C for 22 h to obtain a mixed solution of carbon nanoparticles.

[0103] (2) Adding a nitrogen source dopant to the carbon nanoparticle mixed solution, reacting to obtain a nitrogen-doped solution, and heating the nitrogen-doped solution at a high temperature to obtain an amination-treated mixed solution:

[0104] The carbon dot solution was cooled to room temperature (25°C), filtered with a 0.22 μm filter head, and then 0.5 g of dimethylpyridinium amine was added to obtain a nitrogen-doped solution; the nitrogen-doped solution was heated at high temperature again for 5 h to obtain a mixed solution after amino treatment.

[0105] (3) Cooling, centrifuging and drying the mixed solution after the amination treatment, concentrating the intermediate product by rotary evaporation and freeze drying, and collecting the carbon nanoparticle product:

[0106] The mixed solution after amination treatment was cooled to room temperature (25°C), collected in a 50 mL centrifuge tube, centrifuged to remove undissolved matter, and the supernatant was added to a round-bottom flask and dried using a heating jacket; it was heated until there was no flowing liquid in the bottle and there was steam at the bottle mouth; the dried sample at the bottom of the bottle was washed out with a small amount of ultrapure water; the carbon dot product was concentrated by rotary evaporation, and then freeze-dried and the carbon nanoparticle product was collected.

[0107] (4) Dissolving the carbon dot product in water to form a dispersion, filtering, washing, and centrifuging in filter devices with a molecular weight cutoff of 30 kDa and 5 kDa, respectively, to collect single-particle burst-type fluorescent flashing carbon dots:

[0108] Take 10 mg of the carbon nanoparticle product, dissolve it with ultrapure water, load it into the upper cavity of an ultrafiltration tube with a molecular weight cutoff of 30 kDa, perform ultrafiltration centrifugation, and obtain a permeated solution; load the permeated carbon dot solution into the upper cavity of an ultrafiltration tube with a molecular weight cutoff of 5 kDa, and perform centrifugal ultrafiltration to obtain an upper solution; wash the upper solution once with ultrapure water by centrifugation, and obtain the washed upper solution again to obtain a single-particle burst-type fluorescent flashing carbon dot 3 of 5-30 kDa.

[0109] Using a Nikon A1 confocal microscope with high detection sensitivity, a total internal reflection and epifluorescence imaging system, under a 100x oil immersion objective (NA = 1.49), with appropriate filters (532nm laser, 570nm dichroic mirror, 590nm long-pass emission filter), the single-particle burst-type fluorescent flashing carbon dots were imaged with the help of an Andor 897 single-molecule EMCCD. Thus, the flashing image of the single-particle burst-type fluorescent flashing carbon dots 3 was obtained, and the flashing trajectory of the single-particle burst-type fluorescent flashing carbon dots was statistically calculated, as shown in FIG. Figure 5 shown.

[0110] according to Figure 5 It can be seen that the single-particle burst-type fluorescent scintillation carbon dots prepared in the above embodiments all exhibit burst-type scintillation characteristics with extremely low scintillation period.

[0111] The obtained single-particle burst fluorescent flashing carbon dots 3 were combined with the enzymatically hydrolyzed β2AR antibody fragment in a 1:1 ratio and used for specific labeling of β2AR chemokine receptors on the cell membrane and quantification of β2AR aggregation and distribution to obtain the aggregate size, distribution and the number of receptor molecules contained in the aggregate.

[0112] Example 4

[0113] This embodiment provides a method for preparing a single-particle burst-type fluorescent scintillating carbon dot 4, and the specific steps are as follows:

[0114] (1) dissolving the carbon material and the oxidant in water, and performing a heating oxidation reaction to obtain a carbon nanoparticle mixed solution:

[0115] Weigh 0.5 g of graphene and 50 mL of ultrapure water, add them into a 250 mL round-bottom flask respectively, and mix them by ultrasonic mixing for 20 min; add 50 mL of sulfuric acid and nitric acid, mix well and wipe off the water on the outside of the round-bottom flask; build a condensation reflux device, put the above round-bottom flask into an oil bath, heat the reaction at 180 ° C for 24 h to obtain a mixed solution of carbon nanoparticles.

[0116] (2) Adding a nitrogen source dopant to the carbon nanoparticle mixed solution, reacting to obtain a nitrogen-doped solution, and heating the nitrogen-doped solution at a high temperature to obtain an amination-treated mixed solution:

[0117] The carbon nanoparticle mixed solution was cooled to room temperature (25°C), filtered with a 0.22 μm filter head, and then 0.5 g of trimethylamine borane was added to obtain a nitrogen-doped solution; the nitrogen-doped solution was heated at high temperature again for 6 hours to obtain an amination-treated mixed solution.

[0118] (3) After cooling, centrifuging and drying the mixed solution after the amination treatment, the intermediate product is concentrated by rotary evaporation and freeze-dried to collect the carbon nanoparticle product:

[0119] The mixed solution after amination treatment was cooled to room temperature (25°C), collected in a 50 mL centrifuge tube, centrifuged to remove undissolved matter, and the supernatant was added to a round-bottom flask and dried using a heating jacket; it was heated until there was no flowing liquid in the bottle and there was steam at the bottle mouth; the dried sample at the bottom of the bottle was washed out with a small amount of ultrapure water; the carbon dot product was concentrated by rotary evaporation, and then freeze-dried and the carbon nanoparticle product was collected.

[0120] (4) The dispersion formed by dissolving the carbon nanoparticle product in water is filtered, washed and centrifuged in filter devices with a molecular weight cutoff of 30 kDa and 5 kDa, and single-particle burst-type fluorescent flashing carbon dots are collected:

[0121] Take 10 mg of the carbon nanoparticle product, dissolve it in ultrapure water, load it into the upper cavity of an ultrafiltration tube with a molecular weight cutoff of 30 kDa, perform ultrafiltration centrifugation, and obtain a permeated solution; load the permeated carbon dot solution into the upper cavity of an ultrafiltration tube with a molecular weight cutoff of 5 kDa, and perform centrifugal ultrafiltration to obtain an upper solution; wash the upper solution once with ultrapure water by centrifugation, and obtain the washed upper solution again to obtain a single-particle burst-type fluorescent flashing carbon dot 4 of 5-30 kDa.

[0122] Using a Nikon A1 confocal microscope with high detection sensitivity, total internal reflection and epifluorescence imaging system, under a 100x oil immersion lens (NA = 1.49), with appropriate filters (532nm laser, 570nm dichroic mirror, 590nm long-pass emission filter), and with the help of an Andor 897 single-molecule EMCCD, single-particle carbon dots were imaged. Thus, the flashing image of single-particle burst-type fluorescent flashing carbon dots 4 was obtained, and the flashing trajectory of the carbon dots was counted.

[0123] The obtained single-particle burst-type fluorescent flashing carbon dots 4 were combined with the enzymatically hydrolyzed EGFR (epidermal growth factor receptor) antibody fragment in a 1:1 ratio and used for specific labeling of EGFR receptors on the cell membrane and quantification of EGFR aggregation and distribution to obtain the aggregate size, distribution and number of receptor molecules contained in the aggregate.

[0124] Example 5

[0125] This embodiment provides a method for preparing a single-particle burst-type fluorescent scintillating carbon dot 5, and the specific steps are as follows:

[0126] (1) dissolving the carbon material and the oxidant in water, and performing a heating oxidation reaction to obtain a carbon nanoparticle mixed solution:

[0127] Weigh 0.5 g of carbon black and 50 mL of ultrapure water, add them into a 250 mL round-bottom flask respectively, and mix them by ultrasonic mixing for 20 min; add 30 mL of sulfuric acid and nitric acid, mix well, and wipe off the water on the outside of the round-bottom flask; build a condensation reflux device, put the above round-bottom flask into an oil bath, and heat the reaction at 170 ° C for 24 h to obtain a mixed solution of carbon nanoparticles.

[0128] (2) Adding a nitrogen source dopant to the carbon nanoparticle mixed solution, reacting to obtain a nitrogen-doped solution, and heating the nitrogen-doped solution at a high temperature to obtain an amination-treated mixed solution:

[0129] The carbon dot solution was cooled to room temperature (25°C), filtered with a 0.22 μm filter head, and then 0.5 g of thiazole-5-amine was added to obtain a nitrogen-doped solution; the nitrogen-doped solution was heated at high temperature again for 4 hours to obtain a mixed solution after amino treatment.

[0130] (3) After cooling, centrifuging and drying the mixed solution after the amination treatment, the intermediate product is concentrated by rotary evaporation and freeze-dried to collect the carbon nanoparticle product:

[0131] The mixed solution after amination treatment was cooled to room temperature (25°C), collected in a 50 mL centrifuge tube, centrifuged to remove undissolved matter, and the supernatant was added to a round-bottom flask and dried using a heating jacket; it was heated until there was no flowing liquid in the bottle and there was steam at the bottle mouth; the dried sample at the bottom of the bottle was washed out with a small amount of ultrapure water; the carbon dot product was concentrated by rotary evaporation, and then freeze-dried and the carbon nanoparticle product was collected.

[0132] (4) The dispersion formed by dissolving the carbon nanoparticle product in water is filtered, washed and centrifuged in filter devices with a molecular weight cutoff of 30 kDa and 5 kDa, and single-particle burst-type fluorescent flashing carbon dots are collected:

[0133] Take 10 mg of the carbon nanoparticle product, dissolve it with ultrapure water, load it into the upper cavity of an ultrafiltration tube with a molecular weight cutoff of 30 kDa, perform ultrafiltration centrifugation, and obtain a permeated solution; load the permeated carbon dot solution into the upper cavity of an ultrafiltration tube with a molecular weight cutoff of 5 kDa, and perform centrifugal ultrafiltration to obtain an upper solution; wash the upper solution once with ultrapure water by centrifugation, and obtain the washed upper solution again to obtain a single-particle burst-type fluorescent flashing carbon dot 5 of 5-30 kDa.

[0134] Figure 6 This is a transmission electron microscope image of a single-particle burst-type fluorescent flashing carbon dot prepared in Example 5.

[0135] Using a Nikon A1 confocal microscope with high detection sensitivity, total internal reflection and epifluorescence imaging system, under a 100x oil immersion lens (NA = 1.49), with appropriate filters (532nm laser, 570nm dichroic mirror, 590nm long-pass emission filter), and with the help of an Andor 897 single-molecule EMCCD, single-particle carbon dots were imaged. Thus, the blinking image of single-particle burst-type nanocarbon dots was obtained, and the blinking trajectory of single-particle burst-type fluorescent blinking carbon dots was statistically calculated.

[0136] The obtained single-particle burst fluorescent flashing carbon dots 5 were combined with the enzymatically hydrolyzed CXCR5 chemokine receptor antibody fragment in a 1:1 ratio and used for specific labeling of CXCR5 receptors on the cell membrane and quantification of CXCR5 aggregation and distribution to obtain the aggregate size, distribution and the number of receptor molecules contained in the aggregate.

[0137] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A method for preparing single-particle burst-type fluorescent scintillating carbon dots, characterized in that: include: Dissolving the carbon material and the oxidant in water, and performing a heating oxidation reaction to obtain a carbon nanoparticle mixed solution; Adding a nitrogen source dopant to the carbon nanoparticle mixed solution to react to obtain a nitrogen-doped solution, and heating the nitrogen-doped solution at a high temperature to react to obtain an amination-treated mixed solution; The mixed solution after the amination treatment is cooled, centrifuged and dried, and the intermediate product is concentrated by rotary evaporation and freeze-dried to collect the carbon nanoparticle product; The dispersion formed by dissolving the carbon nanoparticle product in water is filtered, washed and centrifuged in filter devices with a molecular weight cutoff of 30 kDa and 5 kDa, respectively, to collect single-particle burst-type fluorescent flashing carbon dots.

2. The method for preparing single-particle burst-type fluorescent scintillation carbon dots according to claim 1, characterized in that: The carbon structural material is one or more of carbon black, graphite, graphene and carbon nanotubes; And / or, the added amount of the carbon structural material is 0.1-1.0 g / L.

3. The method for preparing single-particle burst-type fluorescent scintillating carbon dots according to claim 1, characterized in that: The oxidant is one or more of nitric acid and sulfuric acid.

4. The method for preparing single-particle burst-type fluorescent scintillating carbon dots according to claim 1, characterized in that: The added amount of the oxidant is 30-100 mL.

5. The method for preparing single-particle burst-type fluorescent scintillating carbon dots according to claim 1, characterized in that: When the heating oxidation reaction is carried out, the reaction temperature is 120-200° C. and the reaction time is 4-24 hours.

6. The method for preparing single-particle burst-type fluorescent scintillating carbon dots according to claim 1, characterized in that: The nitrogen source dopant is one or more of ethylenediamine, urea, geranylamine, cyanamide, oleylamine, dimethylpyridiniumamine, trimethylamine borane, and thiazole-5-amine.

7. The method for preparing single-particle burst-type fluorescent carbon dots according to claim 1, characterized in that: The added amount of the nitrogen source dopant is 0.5 g.

8. The method for preparing single-particle burst-type fluorescent scintillating carbon dots according to claim 1, characterized in that: When the high temperature heating reaction is carried out, the high temperature is 170° C. and the reaction time is 2-6 hours.

9. A single-particle burst-type fluorescent carbon dot prepared by any method of claims 1-8.

10. Use of a single-particle burst-type fluorescent carbon dot prepared by the method of any one of claims 1 to 8 or a single-particle burst-type fluorescent carbon dot according to claim 9 in super-resolution fluorescence imaging quantitative analysis of receptor protein aggregation on cell membranes.

Citation Information

Patent Citations

  • Method for extracting carbon quantum dots from activated carbon

    CN101973541A

  • Method for preparing fluorescent carbon point by virtue of chemical oxidation method, fluorescent carbon point and application of fluorescent carbon point

    CN104071769A

  • Environmentally-friendly method for preparing fluorescent carbon quantum dots with activated carbon

    CN106566541A

  • Preparation method and application of cellulose-based nitrogen-doped fluorescent carbon quantum dots

    CN108485660A

  • Preparation method of water-soluble carbon quantum dots

    CN108975311A