Highly homogenized non-quenched and tempered steel and production process thereof

By using MnTe to wrap MnS and Al2O3 nucleation technology in non-tempered steel, combined with electromagnetic stirring and light pressure at solidification ends, the problem of sulfide morphology control is solved, and the production of highly homogenized non-tempered steel is achieved, which has improved its Fatigue properties and surface uniformity.

CN118895459AInactive Publication Date: 2024-11-05NANJING IRON & STEEL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411219971.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-05
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

It is difficult to achieve homogenization of sulfide morphology control during the rolling process of existing non-tempered steels, resulting in reduced fatigue performance and problem with the workpiece surface, especially in extreme cases, which may lead to local failure.

Method used

By adding Te elements to the steel, MnTe is wrapped with MnS, using Al2O3 as a heterogeneous nucleation point to promote sulfide nucleation, and dynamic light pressure is used in the continuous casting process to control the morphology and distribution of sulfides.

Benefits of technology

It effectively inhibits the precipitation of long strip MnS, promotes spherical growth and uniform distribution of sulfides, reduces sulfide aggregation, and improves the homogenization and mechanical properties of non-tempered steels.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895459A_ABST
    Figure CN118895459A_ABST
Patent Text Reader

Abstract

The invention discloses highly homogenized non-quenched and tempered steel, which relates to the technical field of steel production, and comprises the following chemical components in percentage by mass: 0.36-0.42% of C; 0.40% to 0.70% of Si; mn: 1.30 to 1.60%; s is 0.040 to 0.070 percent; 0.0005 to 0.020 percent of Te (Teflon); less than or equal to 0.020% of P; 0.10% to 0.40% of Cr; 0.02 to 0.06 part of V; 0.010% to 0.040% of Ti; 0.005 to 0.040 percent of Al (aluminum); 0.013% to 0.020% of N; b < = 0.0005%; and the balance of Fe and other inevitable impurities. According to the method, the MnTe wraps the surface of the MnS when the molten steel is solidified after Te treatment in the smelting process, precipitation and growth of long-strip-shaped MnS are inhibited, the length-width ratio of MnS is reduced, and MnS is promoted to grow in a spherical shape. The form of the inclusions is changed from a chain shape to a short rod shape and a nearly spherical shape.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of steel production, in particular to a highly homogenized non-quenched and tempered steel and a production process thereof. Background Art

[0002] Non-quenched and tempered steel is an environmentally friendly structural material. The automotive power conversion components made of non-quenched and tempered steel can save the subsequent quenching and tempering heat treatment process, and have the significant advantages of cleanliness, high efficiency, energy saving, material saving, emission reduction and consumption reduction. However, the automotive power conversion components have complex structures and high comprehensive performance requirements, especially lightweight, which puts higher requirements on the performance of raw materials.

[0003] The control technology of non-quenched and tempered steel sulfide morphology is the focus of attention in the industry. In order to improve cutting performance, non-quenched and tempered steel adds S element in the composition design. S combines with Mn in the steel to generate MnS with good ductility. As the rolling process is prolonged, it has a splitting effect on the matrix, which has a great impact on the fatigue performance of the workpiece. At the same time, the segregation of sulfides will cause surface problems of the workpiece, and in extreme cases will cause local failure of the workpiece. Summary of the invention

[0004] The technical problem to be solved by the present invention is to overcome the shortcomings of the prior art and provide a highly homogenized non-quenched and tempered steel and a production process thereof.

[0005] In order to solve the above technical problems, the technical solution of the present invention is as follows: A highly homogenized non-quenched and tempered steel, whose chemical composition and mass percentage are as follows: C: 0.36-0.42%; Si: 0.40-0.70%; Mn: 1.30-1.60%; S: 0.040-0.070%; Te: 0.0005-0.020%; P: ≤0.020%; Cr: 0.10-0.40%; V: 0.02-0.06; Ti: 0.010-0.040%; Al: 0.005-0.040%; N: 0.013-0.020%; B≤0.0005%; the rest are Fe and other inevitable impurities.

[0006] The present invention also provides a production process for highly homogenized non-quenched and tempered steel, which comprises EAF smelting, LF refining, VD refining, continuous casting, heating and rolling in sequence.

[0007] As a preferred solution of the production process of the highly homogenized non-quenched and tempered steel described in the present invention, in the EAF smelting process, the C content at the end of the electric furnace is controlled to be 0.05-0.35%, the P content is ≤0.010%, and the B content is ≤0.0003%, and the end temperature is controlled to be 1620-1680°C.

[0008] As a preferred solution of the production process of the highly homogenized non-quenched and tempered steel described in the present invention, wherein: in the LF refining process, high-purity graphite carbon material is added to adjust the C element content to the target value, ferromanganese is added to adjust the Mn element content to the target value, ferrosilicon is added to adjust the Si element content to the target value, ferrochrome is added to adjust the Cr element content to the target value, and ferrovanadium is added to adjust the V element content to the target value.

[0009] As a preferred solution of the production process of the highly homogenized non-quenched and tempered steel of the present invention, wherein: nitrogen blowing and stirring are performed throughout the LF refining process, and the nitrogen pressure is 0.2-0.4 MPa.

[0010] As a preferred solution of the production process of highly homogenized non-quenched and tempered steel described in the present invention, in which: in the VD refining process, the vacuum treatment is greater than or equal to 15 minutes at a vacuum degree of less than or equal to 1 mbar, and sampling and analysis are carried out after static stirring for greater than or equal to 10 minutes after breaking the vacuum, and soft blowing of argon is greater than or equal to 5 minutes after the element content meets the requirements, and the soft blowing pressure is 0.15-0.25 MPa.

[0011] As a preferred solution of the production process of the highly homogenized non-quenched and tempered steel described in the present invention, in the continuous casting process, full protection casting is adopted, the superheat is 15-35°C, and the casting speed is 0.50m / min.

[0012] As a preferred solution of the production process of highly homogenized non-quenched and tempered steel described in the present invention, wherein: in the continuous casting process, electromagnetic stirring is adopted, the electromagnetic stirring intensity of the crystallizer is 200~350A×2Hz, the electromagnetic stirring intensity at the end is 500~700A×6Hz, and the reduction at the end of solidification is 8~13mm.

[0013] As a preferred embodiment of the production process of the highly homogenized non-quenched and tempered steel described in the present invention, the rolling process includes heating, start rolling and final rolling, the temperature of the soaking section in the heating process is 1200-1250°C, the start rolling temperature is 1050-1150°C, the final rolling temperature is 850-930°C, and the upper cooling bed temperature is 760-830°C.

[0014] The beneficial effects of the present invention are: (1) In the present invention, MnTe forms a coating on the surface of MnS when the molten steel solidifies after Te treatment during the smelting process, thereby inhibiting the precipitation and growth of long strips of MnS, reducing the aspect ratio of MnS, and promoting the spherical growth of MnS. The morphology of inclusions changes from chain-like to short rod-like and nearly spherical.

[0015] (2) The present invention promotes sulfide nucleation by increasing heterogeneous nucleation points. When the molten steel solidifies, Al2O3 provides a large number of heterogeneous nucleation points for the formation of MnS, which promotes the multi-point nucleation of sulfides, increases the number of sulfides formed, and promotes the discrete distribution of sulfides.

[0016] (3) The present invention reduces the expansion of the columnar crystal region by using the crystallizer electromagnetic stirring frequency of (200-300) ± 5A × 2HZ; increases the proportion of equiaxed crystals by using the end electromagnetic stirring of (500-650) ± 5A × 6Hz and the end solidification reduction of 7-15mm, thereby breaking the solid matter at the front of the columnar crystal and mixing it with the core molten steel, thereby reducing the micro-component segregation and sulfide aggregation caused by partial crystallization in the core region. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative labor.

[0018] Figure 1 This is a schematic diagram of the morphology of sulfides in general S-containing non-modulated steel; Figure 2 A schematic diagram of the morphology of the highly homogenized non-quenched and tempered steel MnS provided by the present invention; Figure 3 This is the SEM image of the MnS encapsulation mechanism of MnTe; Figure 4 This is the SEM composition surface scanning analysis diagram of MnTe encapsulating MnS mechanism; Figure 5 The electron microscope scanning image of Al2O3 as a heterogeneous nucleation point to form MnS; Figure 6 This is a surface scanning analysis diagram of MnS composition formed by Al2O3 as a heterogeneous nucleation point. DETAILED DESCRIPTION

[0019] In order to make the content of the present invention more clearly understood, the present invention is further described in detail below according to specific implementation modes and in combination with the accompanying drawings.

[0020] The present application provides a highly homogenized non-quenched and tempered steel, whose chemical composition and mass percentage are as follows: C: 0.36-0.42%; Si: 0.40-0.70%; Mn: 1.30-1.60%; S: 0.040-0.070%; Te: 0.0005-0.020%; P: ≤0.020%; Cr: 0.10-0.40%; V: 0.02-0.06; Ti: 0.010-0.040%; Al: 0.005-0.040%; N: 0.013-0.020%; B≤0.0005%; the rest is Fe and other inevitable impurities.

[0021] The present application also provides a production process for highly homogenized non-quenched and tempered steel, which includes EAF smelting, LF refining, VD refining, continuous casting, heating, and rolling in sequence, as follows: In the EAF smelting process, the electric furnace endpoint C is controlled at 0.05-0.35%, P≤0.010%, B≤0.0003%, and the endpoint temperature is controlled at 1620-1680°C. During the steelmaking process, the slag is strictly controlled and the steelmaking aluminum is adjusted to Alt at 0.010-0.030%.

[0022] In the LF refining process, the composition is point controlled according to the target value, and high-purity graphite carbon materials, ferromanganese, ferrosilicon, ferrochrome, and ferrovanadium are used to adjust C, Mn, Si, Cr, and V elements to the lower limit of the judgment range or the target value. Nitrogen blowing and stirring are carried out throughout the process, and the nitrogen pressure is 0.2-0.4MPa. Al wire or Al particles can be fed according to the aluminum content, and high-purity SiC and other diffusion deoxidation can be used to ensure slag fluidity and slag whitening, and the white slag time is ≥30min. The Al content at the end of the LF refining process is 0.020-0.035%, and FeS is used to adjust S to 0.040-0.070% before LF ends and enters vacuum; the composition is adjusted to the specified range, and VD vacuum degassing is carried out after the temperature is appropriate.

[0023] In the VD refining process, during the vacuum degassing process, the vacuum degree is ≤1mbar for ≥15min, and after breaking the vacuum and stirring for ≥10min, sampling and analysis can be performed. High-purity silicon nitride cored wire can be used to increase nitrogen by 1.5-2.5m / ton steel and Ti wire by 1.3-1.8m / ton steel. Al wire can be fed according to the target. After the soft blowing time is ≥10min, sulfur wire can be fed to adjust the sulfur composition. After the sulfur wire is fed and soft blown for ≥5min, sampling and analysis are performed, and fine-tuning is performed according to the analysis results. Calcium iron wire or silicon calcium wire 0.5-1m / ton steel and Te wire are fed. After all elements meet the requirements, soft blowing of argon is performed for ≥5min, and the soft blowing pressure is 0.15-0.25Mpa; the temperature reaches 1540-1570℃ (the temperature of the pouring furnace can be 10℃ higher), and ladle continuous casting can be performed.

[0024] In the continuous casting process, full protection pouring is adopted throughout the continuous casting process, the superheat is 15-35°C, and the pulling speed is 0.50m / min; electromagnetic stirring is used in the continuous casting process, the electromagnetic stirring intensity of the crystallizer is 200-350A×2Hz, the end electromagnetic stirring is 500-700A×6Hz, and the pressure reduction at the end of solidification is 8-13mm.

[0025] The rolling process includes heating, start rolling and final rolling; the temperature of the soaking section is 1200-1250°C, the start rolling temperature is 1050-1150°C, the final rolling temperature is 850-930°C, and the upper cooling bed temperature is 760-830°C.

[0026] The following is further described by means of specific examples.

[0027] Table 1 shows the chemical composition and mass percentage of the highly homogenized non-quenched and tempered steel in Examples 1 to 3.

[0028]

[0029] Table 1 Table 2 shows the C and S components at different positions of the round steel cross section obtained in Examples 1 to 3.

[0030]

[0031] Table 2 Table 3 shows the levels of non-metallic inclusions in the highly homogenized non-quenched and tempered steels obtained in Examples 1 to 3.

[0032]

[0033] Table 3 Table 4 shows the mechanical properties of the highly homogenized non-quenched and tempered steels obtained in Examples 1 to 3.

[0034]

[0035] Table 4 like Figures 2 to 6 As shown in Tables 2 to 4, the important components C and S in the round steel cross-section of Examples 1 to 3 have small segregation and are evenly distributed, and the sulfide distribution is fine and dispersed, which meets the use requirement of no aggregated "magnetic marks" on the surface of non-quenched and tempered steel forgings.

[0036] Therefore, the technical solution of the present application obtains a stable ferrite-pearlite non-quenched and tempered steel microstructure by optimizing the refining process, continuous casting process and hot rolling process. By controlling the nucleation and growth behavior of sulfides during the solidification of molten steel, a control technology for the spheroidization of sulfide morphology in steel is formed. During the solidification of molten steel, dual control is performed through the "wrapping + heterogeneous nucleation" principle, and MnTe forms a wrap around the surface of MnS to achieve the spheroidization effect of sulfides. At the same time, continuous casting electromagnetic stirring and dynamic light pressure at the end of solidification control the C and S deviations of the round steel section to obtain highly homogenized non-quenched and tempered steel.

[0037] In addition to the above embodiments, the present invention may also have other implementation modes; any technical solutions formed by equivalent replacement or equivalent transformation shall fall within the protection scope required by the present invention.

Claims

1. A highly homogenized non-quenched and tempered steel, characterized in that: Its chemical composition and mass percentage are as follows: C: 0.36-0.42%; Si: 0.40-0.70%; Mn: 1.30-1.60%; S:0.040~0.070%; Te: 0.0005~0.020%; P: ≤0.020%; Cr: 0.10~0.40%; V: 0.02~0.06; Ti: 0.010~0.040%; Al: 0.005~0.040%; N: 0.013~0.020%; B≤0.0005%; the rest are Fe and other inevitable impurities.

2. A production process for highly homogenized non-quenched and tempered steel according to claim 1, characterized in that: It includes EAF smelting, LF refining, VD refining, continuous casting, heating and rolling in sequence.

3. The production process of highly homogenized non-quenched and tempered steel according to claim 1, characterized in that: In the EAF smelting process, the C content at the end of the electric furnace is controlled to be 0.05-0.35%, the P content is ≤0.010%, and the B content is ≤0.0003%, and the end temperature is controlled to be 1620-1680°C.

4. The production process of highly homogenized non-quenched and tempered steel according to claim 1, characterized in that: In the LF refining process, high-purity graphite carbon material is added to adjust the C element content to the target value, ferromanganese is added to adjust the Mn element content to the target value, ferrosilicon is added to adjust the Si element content to the target value, ferrochrome is added to adjust the Cr element content to the target value, and ferrovanadium is added to adjust the V element content to the target value.

5. The production process of highly homogenized non-quenched and tempered steel according to claim 1, characterized in that: In the LF refining process, nitrogen blowing and stirring are performed throughout the process, and the nitrogen pressure is 0.2-0.4 MPa.

6. The production process of highly homogenized non-quenched and tempered steel according to claim 1, characterized in that: In the VD refining process, vacuum treatment is performed for 15 minutes or more at a vacuum degree of 1 mbar or less, and sampling and analysis are performed after static stirring for 10 minutes or more after breaking the vacuum. After the element content meets the requirements, argon is soft-blown for 5 minutes or more, and the soft-blowing pressure is 0.15-0.25 MPa.

7. The production process of highly homogenized non-quenched and tempered steel according to claim 1, characterized in that: In the continuous casting process, full protection pouring is adopted, the superheat is 15-35° C., and the casting speed is 0.50 m / min.

8. The production process of highly homogenized non-quenched and tempered steel according to claim 1, characterized in that: In the continuous casting process, electromagnetic stirring is adopted, the electromagnetic stirring intensity of the crystallizer is 200-350A×2Hz, the electromagnetic stirring intensity of the end is 500-700A×6Hz, and the reduction amount at the end of solidification is 8-13mm.

9. The production process of highly homogenized non-quenched and tempered steel according to claim 1, characterized in that: The rolling process includes heating, start rolling and final rolling. In the heating process, the soaking section temperature is 1200-1250°C, the start rolling temperature is 1050-1150°C, the final rolling temperature is 850-930°C, and the upper cooling bed temperature is 760-830°C.

Citation Information

Patent Citations

  • Bar material for non-quenched and tempered shaft part and manufacturing process of bar material

    CN103589970A

  • Medium carbon free-cutting non-quenched-and-tempered steel containing sulfur and tellurium and production technological method thereof

    CN107287504A

  • Smelting method of non-quenched and tempered steel

    CN110055450A

  • Sulfur-containing non-quenched and tempered steel for automobile crankshaft and production process of sulfur-containing non-quenched and tempered steel

    CN115011877A

  • High-quality non-quenched and tempered steel, crankshaft and preparation method

    CN115747634A