Method for assisting growth of 9, 10-diphenylethynyl anthracene single crystal by polymer additive
By introducing polyvinylpyrrolidone (PVP) as a polymer additive, the growth direction of BPEA crystals is controlled, and the problems of small growth size and poor quality of BPEA crystals are solved, and the stable growth and high transmittance of centimeter-level single crystals are achieved, which improves the Its performance in the field of X-ray detection.
Patent Information
- Application Number
- CN202410857027.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-11-05
AI Technical Summary
9,10-diphenylacetylene anthracene (BPEA) crystals have severe growth orientation along the π-π stacking direction, resulting in small growth size, high aspect ratio, and poor quality of single crystals, making it difficult to exert their advantages in the field of X-ray detection.
The method of assisting the single crystal growth of BPEA by polymer additive polyvinylpyrrolidone (PVP) is used to form hydrogen bonds with BPEA molecules to reduce the adhesion frequency of molecules, control the number of nucleations and growth rate, and combine temperature control to prepare centimeter-level, low length and width A single crystal with a high transmittance.
The stable growth of centimeter-level BPEA single crystal is achieved, which reduces costs, improves crystal purity and yield, enhances application potential in the field of X-ray detection, and provides excellent X-ray detection performance.
Smart Images

Figure CN118895556A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of organic semiconductor single crystal growth, and in particular relates to a method for assisting the growth of 9,10-diphenylethynyl anthracene single crystals with a polymer additive. Background Art
[0002] Since the discovery of X-rays, they have played an important role in medical diagnosis, industrial detection, safety inspection and other fields, making X-rays one of the indispensable tools in modern science and industry, and have made outstanding contributions to the development and progress of human society. Therefore, it is of great significance to develop low-cost and high-performance X-ray detectors for X-ray detection.
[0003] According to the different types of output signals, detectors can be divided into direct detectors and indirect detectors. For direct detectors, in the past few decades, inorganic compound semiconductor detectors represented by CdZnTe have been widely studied. They have the advantages of high sensitivity, excellent energy resolution and good stability, and have been widely used. However, their high manufacturing cost and toxic elements have also restricted their further development.
[0004] In recent years, organic semiconductor single crystals have attracted extensive attention from researchers due to their low manufacturing cost, lack of grain boundaries, high purity, 3D long-range order, and excellent electrical transport properties. Organic semiconductor single crystals grown by solution method have controllable size, low dark current, fast response speed, and tissue equivalence, and have great application potential in the field of X-ray detection.
[0005] 9,10-Bis(phenylethynyl)anthracene (BPEA) organic semiconductor single crystals have gradually emerged in the field of researchers due to their excellent optoelectronic properties. During the growth of BPEA, an orange α phase and a yellow β phase will grow simultaneously. Among them, in the α phase crystal, the organic molecules are in a planar configuration, and the molecules are stacked in a herringbone pattern, which is conducive to π-π stacking and has a higher mobility; while the β phase crystal molecules are in a non-planar configuration, which reduces the conjugated system of the crystal, so they have a lower mobility, but have a higher switching ratio than the α phase. Both phases have application potential in the fields of X-ray detection, ultraviolet detection, α particle detection, etc., but the BPEA crystal has a serious growth orientation along the π-π stacking direction (that is, the growth orientation in the long axis direction is serious), resulting in its single crystal growth size is small, the aspect ratio is high, and the quality is poor. At present, it is mainly used in nanowires and nanosheets, and it is difficult to give full play to its single crystal advantages.
[0006] To this end, the research team of the present invention believes that it is necessary to optimize its growth method to give full play to its single crystal advantages. Summary of the invention
[0007] The purpose of the present invention is to solve the shortcomings of BPEA crystals grown by existing methods, such as serious growth orientation along the π-π stacking direction, small single crystal growth size, high aspect ratio, poor quality, and difficulty in exerting the advantages of single crystals, and to provide a method for the growth of 9,10-diphenylethynyl anthracene single crystals assisted by polymer additives.
[0008] To achieve the above purpose, the technical solution provided by the present invention is:
[0009] A method for growing a 9,10-diphenylethynyl anthracene single crystal by using a polymer additive is characterized in that it comprises the following steps:
[0010] S1. Raw material purification:
[0011] Under a constant temperature environment of temperature T1, dissolving the 9,10-diphenylethynyl anthracene raw material in a first organic solvent to prepare a saturated solution, filtering to remove impurities, standing to volatilize, obtaining a 9,10-diphenylethynyl anthracene precipitate and drying it; wherein T1 is 40-60° C.;
[0012] S2. Solution preparation:
[0013] The 9,10-diphenylethynyl anthracene raw material purified by S1 is dissolved in a second organic solvent at a temperature of T2 to prepare an undersaturated solution, and polyvinyl pyrrolidone is added, and then stirred evenly under a constant temperature environment at a temperature of T3; wherein the concentration of polyvinyl pyrrolidone is 0.25-1.25 mg / ml; T2 is 20-35°C; T2≤T3≤T2+10°C;
[0014] Among them, the concentration of polyvinyl pyrrolidone is 0.25-1.25 mg / ml; PVP concentration is crucial for crystal growth. Too low a concentration has no effect on crystal growth, which is no different from the simple solvent evaporation method. The grown crystals are smaller in size and have a higher aspect ratio. Too high a concentration will increase the number of nuclei, which is also not conducive to crystal growth and will also have a greater impact on crystal purity.
[0015] In order to prevent the solution from precipitating or the solute from being completely dissolved, the stirring temperature should not be lower than the temperature when the solution is prepared;
[0016] S3, solution filtration:
[0017] In order to prevent the solute from precipitating during the filtration process, the solution prepared by S2 was filtered by an organic syringe filter under a constant temperature environment of temperature T4, and the filtrate was collected; wherein T2≤T4≤T2+10℃;
[0018] S4, solution evaporation:
[0019] The filtrate obtained from S3 is sealed with a sealing film provided with through holes (a suitable number of through holes can be pierced on the sealing film by a needle), and is allowed to stand for 3 to 20 days at the same constant temperature as the solution prepared in S2; as the solution evaporates, 9,10-diphenylethynyl anthracene crystals gradually nucleate and grow;
[0020] S5, Volatilization Crystallization:
[0021] After the growth of 9,10-diphenylethynyl anthracene crystals is completed, the crystals are taken out, cleaned and dried in a constant temperature environment at a temperature of T5 to obtain 9,10-diphenylethynyl anthracene single crystals; wherein, T2≤T5≤T2+10°C. The temperature requirement is mainly to prevent the solution from shaking and causing new crystals to precipitate when the crystals are taken out. Since the process of taking crystals out of the solution is also relatively fast, a slight increase in temperature will not affect the grown crystals. In the drying process, the cleaned crystals can be directly placed on a dust-free cloth to dry naturally.
[0022] Further, the first organic solvent is tetrahydrofuran, p-xylene, N,N-dimethylformamide, cyclopentanone, cyclohexanone or 1-bromonaphthalene;
[0023] The drying is carried out at 40 to 60° C. for 1 to 24 hours;
[0024] This raw material purification step was repeated 2 to 3 times.
[0025] Further, in S2, the second organic solvent is tetrahydrofuran, p-xylene, toluene, acetone or dichloromethane;
[0026] In order to fully dissolve the solute and stir the solution evenly, the time should be no less than 6 hours;
[0027] Further, in S3, the organic syringe filter is made of organic nylon 66, has a diameter of 13 to 25 mm, and a pore size of 0.22 to 0.45 μm;
[0028] The through holes are 1-3 pinholes with a diameter of 1 mm. The through holes are mainly used to control the volatilization rate of the solvent. The larger the total area of the holes, the faster the volatilization. The number of holes can be adjusted according to the actual situation of the solution.
[0029] Further, in S5, the cleaning process is repeated 1 to 3 times, and the crystal is taken out when the liquid level is about to cover the top of the crystal but has not yet covered it.
[0030] Furthermore, S1 to S5 are all carried out in a constant temperature environment, and the constant temperature equipment is a heating table, a heat collecting constant temperature heating magnetic stirrer or a blast drying oven.
[0031] At the same time, the present invention also provides a 9,10-diphenylethynylanthracene single crystal grown by the above method, and an X-ray detector using the 9,10-diphenylethynylanthracene single crystal as a detection material.
[0032] The advantages of the present invention are:
[0033] 1. The present invention introduces a polymer additive polyvinylpyrrolidone (PVP), which forms hydrogen bonds with BPEA molecules, reduces the attachment frequency of the molecules, inhibits BPEA nucleation (controls the number of nucleations) and the growth rate in the long axis direction, increases the supersaturation of the solution, and can effectively increase the growth rate of the crystal in the width direction; at the same time, combined with the control of temperature in the entire growth process, centimeter-level, low aspect ratio, and high transmittance BPEA single crystals are prepared, and the crystal growth is relatively stable, so as to give full play to its advantages in the field of X-ray detection.
[0034] 2. The growth method of the present invention has the advantages of simple operation, low crystal growth cost, high yield, and easy batch preparation; at the same time, the grown crystals can be recycled and regrown, further improving the crystal purity and reducing costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 The figure is a flow chart of the polymer additive-assisted volatilization method for growing BPEA crystals according to the present invention.
[0036] Figure 2 Figures are pictures of crystal nucleation, where (a), (b), (c), (d), and (e) are pictures of crystal nucleation when the PVP concentrations in Example 1 are 0.1, 0.25, 0.75, 1.25, and 1.5 mg / ml, respectively, and (f) is a picture of yellow β-phase BPEA crystals obtained when the PVP concentration is 0.75 mg / ml.
[0037] Figure 3 This is a picture of the orange α-phase BPEA crystals described in Example 2.
[0038] Figure 4 This is a picture of the BPEA crystals described in Example 3.
[0039] Figure 5 This is a picture of the BPEA crystal described in Comparative Example 1.
[0040] Figure 6 This is a picture of the BPEA crystal described in Comparative Example 2.
[0041] Figure 7 Figure 2 shows the dual-phase BPEA crystal and its simulated XRD pattern.
[0042] Figure 8The photocurrent density diagram and the sensitivity change curve are shown in FIG. 2 , wherein (a) is the photocurrent density diagram of the X-ray detector prepared from the single crystal described in Example 2 under different bias voltages and different doses; (b) is the sensitivity change curve of the X-ray detector prepared from the single crystal described in Example 2 under different electric field strengths. DETAILED DESCRIPTION
[0043] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments:
[0044] The organic semiconductor 9,10-diphenylethynylanthracene (BPEA) raw material powder used in this embodiment has a purity of 98% (HPLC) and was purchased from Shanghai Yuanye Biotechnology Co., Ltd., K16-18 polyvinylpyrrolidone was purchased from Aladdin Biochemical Technology Co., Ltd., analytically pure dichloromethane was purchased from Aladdin Biochemical Technology Co., Ltd., and analytically pure tetrahydrofuran was purchased from Tianjin Fuyu Fine Chemical Co., Ltd.
[0045] The molecular formula of BPEA organic crystal is C 30 H 18 , the structural formula is:
[0046]
[0047] Example 1
[0048] like Figure 1 As shown in the flow chart, a method for polymer additive-assisted 9,10-diphenylethynyl anthracene single crystal growth comprises the following steps:
[0049] S1. Raw material purification:
[0050] BPEA powder was added to tetrahydrofuran solvent to prepare a saturated solution at 60°C, and the solution was filtered on a heating table to remove impurities. The solution was allowed to stand at 60°C for volatilization to obtain BPEA precipitate, which was dried in a forced air drying oven at 60°C for 12 hours. The above purification process was repeated 3 times;
[0051] S2. Solution preparation:
[0052] Dissolve 0.55 g of BPEA powder purified from S1 in 40 mL of tetrahydrofuran solvent at 23 °C to prepare 5 solutions, and add PVP at PVP concentrations of 0.1, 0.25, 0.75, 1.25, and 1.5 mg / ml. Stir evenly on a heat-collecting constant temperature heating magnetic stirrer at 28 °C.
[0053] S3, solution filtration:
[0054] The solution prepared by S2 was sucked out with a syringe and filtered into a beaker through an organic syringe filter. The above operation was carried out on a heating table at 28°C. The organic syringe filter was made of organic nylon 66, with a diameter of 25 mm and a pore size of 0.45 μm.
[0055] S4, solvent evaporation:
[0056] Use a sealing film to seal the beaker containing the filtrate in S3, and use a needle to pierce a hole with a diameter of 1 mm in the center of the sealing film. Let it stand at 23°C for 15 days to evaporate;
[0057] S5, Volatilization Crystallization:
[0058] In S4, as the solvent evaporates, BPEA crystals gradually nucleate and grow. When the liquid level is about to cover the top of the crystal but not yet, the crystal is picked out with clean tweezers on a heating table at 28°C, transferred to ethanol solvent for cleaning twice, and finally placed on a dust-free cloth to dry naturally. The crystallization is shown in Figure 2. Figure 2 shown.
[0059] By analyzing the crystallization of PVP additives with different concentrations, it can be found that when the concentration is between 0.25 and 1.25 mg / ml, the crystallization is good, and 0.75 mg / ml is the best. Too high or too low concentration will affect the number of nuclei.
[0060] Example 2
[0061] like Figure 1 As shown in the flow chart, a method for polymer additive-assisted 9,10-diphenylethynyl anthracene single crystal growth comprises the following steps:
[0062] S1. Raw material purification:
[0063] BPEA powder was added to tetrahydrofuran solvent to prepare a saturated solution at 60°C, and the solution was filtered on a heating table to remove impurities. The solution was allowed to stand at 60°C for volatilization to obtain BPEA precipitate, which was dried in a forced air drying oven at 60°C for 12 hours. The above purification process was repeated 3 times;
[0064] S2. Solution preparation:
[0065] Dissolve 0.55 g of BPEA powder purified from S1 in 40 mL of tetrahydrofuran solvent at 30°C to prepare a solution, add PVP at a concentration of 0.75 mg / ml, and stir evenly on a heat-collecting constant temperature heating magnetic stirrer at 30°C;
[0066] S3, solution filtration:
[0067] The solution prepared by S2 was sucked out with a syringe and filtered into a beaker through an organic syringe filter. The above operation was carried out on a heating table at 30°C. The organic syringe filter was made of organic nylon 66, with a diameter of 25 mm and a pore size of 0.22 μm.
[0068] S4, solvent evaporation:
[0069] Use a sealing film to seal the beaker containing the filtrate in S3, and use a needle to pierce a hole with a diameter of 1 mm in the center of the sealing film. Let it stand at 30°C for 10 days to evaporate;
[0070] S5, Volatilization Crystallization:
[0071] In S4, as the solvent evaporates, BPEA crystals gradually nucleate and grow. When the liquid level is about to cover the top of the crystal but not yet, the crystal is picked out with clean tweezers on a heating table at 30°C, transferred to ethanol solvent for cleaning twice, and finally placed on a dust-free cloth to dry naturally. Figure 3 The crystals shown.
[0072] Example 3
[0073] like Figure 1 As shown in the flow chart, a method for polymer additive-assisted 9,10-diphenylethynyl anthracene single crystal growth comprises the following steps:
[0074] S1. Raw material purification:
[0075] BPEA powder was added to tetrahydrofuran solvent to prepare a saturated solution at 60°C, and the solution was filtered on a heating table to remove impurities. The solution was allowed to stand at 60°C for volatilization to obtain BPEA precipitate, which was dried in a forced air drying oven at 60°C for 12 hours. The above purification process was repeated 3 times;
[0076] S2. Solution preparation:
[0077] Dissolve 0.25 g of BPEA powder purified from S1 in 40 mL of dichloromethane solvent at 23°C to prepare a solution, add PVP at a concentration of 0.75 mg / ml, and stir evenly on a heat-collecting constant temperature heating magnetic stirrer at 33°C;
[0078] S3, solution filtration:
[0079] The solution prepared by S2 was sucked out with a syringe and filtered into a beaker through an organic syringe filter. The above operation was carried out on a heating table at 33°C. The organic syringe filter was made of organic nylon 66, with a diameter of 25 mm and a pore size of 0.22 μm.
[0080] S4, solvent evaporation:
[0081] Use a sealing film to seal the beaker containing the filtrate in S3, and use a needle to pierce a hole with a diameter of 1 mm in the center of the sealing film. Let it stand at 23°C for 15 days to evaporate;
[0082] S5, Volatilization Crystallization:
[0083] In S4, as the solvent evaporates, BPEA crystals gradually nucleate and grow. When the liquid level is about to cover the top of the crystal but not yet covered, the crystal is picked out with clean tweezers on a heating table at 33°C, transferred to ethanol solvent for cleaning twice, and finally placed on a dust-free cloth to dry naturally. Figure 4 The crystals shown.
[0084] from Figure 2-Figure 4 It can be seen from the crystal picture that the crystals prepared by the method of the present invention have large growth size and high quality. At the same time, the volatilization rate can be controlled by controlling the volatilization temperature, and BPEA single crystals of different phases can be obtained in tetrahydrofuran solvent. When the temperature is low (Example 1), yellow β-phase single crystals are easy to obtain, and when the temperature is high (Example 2), orange α-phase single crystals are easy to obtain. In dichloromethane solvent, due to the low solubility, although larger single crystals can be obtained (Example 3), the success rate is low, and the low boiling point of dichloromethane (39.6°C) makes it difficult to increase the solubility by increasing the temperature.
[0085] Comparative Example 1
[0086] A method for growing a 9,10-diphenylethynylanthracene single crystal comprises the following steps:
[0087] S1. Raw material purification:
[0088] BPEA powder was added to tetrahydrofuran solvent to prepare a saturated solution at 60°C, and the solution was filtered on a heating table to remove impurities. The solution was allowed to stand at 60°C for volatilization to obtain BPEA precipitate, which was dried in a forced air drying oven at 60°C for 12 hours. The above purification process was repeated 3 times;
[0089] S2. Solution preparation:
[0090] Dissolve 0.25 g of BPEA powder purified from S1 in 40 mL of dichloromethane solvent at 23°C to prepare a solution, and stir evenly on a heat-collecting constant-temperature heating magnetic stirrer at 33°C;
[0091] S3, solution filtration:
[0092] The solution prepared by S2 was sucked out with a syringe and filtered into a beaker through an organic syringe filter. The above operation was carried out on a heating table at 33°C. The organic syringe filter was made of organic nylon 66, with a diameter of 25 mm and a pore size of 0.22 μm.
[0093] S4, solvent evaporation:
[0094] Use a sealing film to seal the beaker containing the filtrate in S3, and use a needle to pierce a hole with a diameter of 1 mm in the center of the sealing film. Let it stand at 23°C for 15 days to evaporate;
[0095] S5, Volatilization Crystallization:
[0096] In S4, as the solvent evaporates, BPEA crystals gradually nucleate and grow. When the liquid level is about to cover the top of the crystal but not yet covered, the crystal is picked out with clean tweezers on a heating table at 33°C, transferred to ethanol solvent for cleaning twice, and finally placed on a dust-free cloth to dry naturally. Figure 5 The crystals shown.
[0097] Compared with Example 3 in which the PVP additive is introduced, the number of crystal nuclei obtained by using dichloromethane as the solvent is significantly increased, and the aspect ratio of the crystal is larger. It can be seen that PVP can effectively inhibit nucleation and reduce the aspect ratio of the crystal.
[0098] Comparative Example 2
[0099] A method for growing a 9,10-diphenylethynylanthracene single crystal comprises the following steps:
[0100] S1. Raw material purification:
[0101] BPEA powder was added to tetrahydrofuran solvent to prepare a saturated solution at 60°C, and the solution was filtered on a heating table to remove impurities. The solution was allowed to stand at 60°C for volatilization to obtain BPEA precipitate, which was dried in a forced air drying oven at 60°C for 12 hours. The purification process was repeated 3 times.
[0102] S2. Solution preparation:
[0103] Dissolve 0.55 g of BPEA powder purified from S1 in 40 mL of tetrahydrofuran solvent at 23°C to prepare a saturated solution, and stir evenly on a heat-collecting constant-temperature heating magnetic stirrer at 28°C;
[0104] S3, solution filtration:
[0105] The solution prepared by S2 was sucked out with a syringe and filtered into a beaker through an organic syringe filter. The above operation was carried out on a heating table at 28°C. The organic syringe filter was made of organic nylon 66, with a diameter of 25 mm and a pore size of 0.45 μm.
[0106] S4, solvent evaporation:
[0107] Use a sealing film to seal the beaker containing the filtrate in S3, and use a needle to pierce a hole with a diameter of 1 mm in the center of the sealing film. Let it stand at 23°C for 15 days to evaporate;
[0108] S5, Volatilization Crystallization:
[0109] In S4, as the solvent evaporates, BPEA crystals gradually nucleate and grow. When the liquid level is about to cover the top of the crystal but not yet, the crystal is picked out with clean tweezers on a heating table at 28°C, transferred to ethanol solvent for cleaning twice, and finally placed on a dust-free cloth to dry naturally. Figure 6 The crystals shown.
[0110] Compared with Example 1 in which the PVP additive is introduced, the number of crystal nuclei obtained using tetrahydrofuran as the solvent is significantly increased, and the crystal aspect ratio is larger, which once again confirms that PVP can effectively inhibit nucleation and reduce the crystal aspect ratio. It can be seen that the introduction of PVP can obtain crystals with a low aspect ratio, and the crystals can be directly used.
[0111] In order to verify the performance of the BPEA single crystal prepared by the method of the present invention, the present invention also analyzes ( Figure 7 ), proving that the prepared dual-phase crystal powder corresponds well to the simulated diffraction pattern, no impurity peaks appear, and the maximum exposed surfaces of the α-phase and β-phase single crystals belong to the {101} and {110} crystal plane families, respectively. At the same time, an X-ray detector was prepared and the sensitivity of the detector was characterized ( Figure 8 ), under different voltages, with the increase of dose rate, the photocurrent density increases continuously, and the sensitivity is fitted. It is found that with the increase of voltage, the detector sensitivity increases continuously and approaches saturation. Under the electric field strength of 1kV / cm, the detector sensitivity can reach 19.61μCGy air -1 cm -2 , showing excellent X-ray detection performance.
[0112] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can easily think of various equivalent modifications or substitutions within the technical scope disclosed in the present invention, and these modifications or substitutions should be included in the protection scope of the present invention.
Claims
1. A method for growing 9,10-diphenylethynyl anthracene single crystals assisted by polymer additives, characterized in that: The following steps are involved: S1. Raw material purification: Under a constant temperature environment of temperature T1, dissolving the 9,10-diphenylethynyl anthracene raw material in a first organic solvent to prepare a saturated solution, filtering to remove impurities, standing to volatilize, obtaining a 9,10-diphenylethynyl anthracene precipitate and drying it; wherein T1 is 40-60° C.; S2. Solution preparation: The 9,10-diphenylethynyl anthracene raw material purified by S1 is dissolved in a second organic solvent at a temperature of T2 to prepare an undersaturated solution, and polyvinyl pyrrolidone is added, and then stirred evenly under a constant temperature environment at a temperature of T3; wherein the concentration of polyvinyl pyrrolidone is 0.25-1.25 mg / ml; T2 is 20-35°C; T2≤T3≤T2+10°C; S3, solution filtration: Under a constant temperature environment of temperature T4, the solution prepared by S2 is filtered by an organic syringe filter, and the filtrate is collected; wherein T2≤T4≤T2+10°C; S4, solvent evaporation: The filtrate obtained in S3 is sealed with a sealing film provided with through holes, and is left to volatilize for 3 to 20 days in a constant temperature environment with the same temperature as the solution prepared in S2; S5, Volatilization Crystallization: After the growth of the 9,10-diphenylethynylanthracene crystal is completed, the crystal is taken out, cleaned and dried in a constant temperature environment at a temperature of T5 to obtain a 9,10-diphenylethynylanthracene single crystal; wherein T2≤T5≤T2+10°C.
2. The method for growing 9,10-diphenylethynyl anthracene single crystals using a polymer additive as described in claim 1, characterized in that: In S1, the first organic solvent is tetrahydrofuran, p-xylene, N,N-dimethylformamide, cyclopentanone, cyclohexanone or 1-bromonaphthalene; The drying is carried out at 40 to 60° C. for 1 to 24 hours; This raw material purification step was repeated 2 to 3 times.
3. The method for growing 9,10-diphenylethynyl anthracene single crystals assisted by polymer additives according to claim 1 or 2, characterized in that: In S2, the second organic solvent is tetrahydrofuran, p-xylene, toluene, acetone or dichloromethane; The stirring time is not less than 6 hours.
4. The method for growing 9,10-diphenylethynyl anthracene single crystals using a polymer additive as claimed in claim 3, characterized in that: In S3, the organic syringe filter is made of organic nylon 66, has a diameter of 13 to 25 mm, and a pore size of 0.22 to 0.45 μm; The through holes are 1-3 pinholes with a diameter of 1 mm.
5. The method for growing 9,10-diphenylethynyl anthracene single crystals using a polymer additive as claimed in claim 4, characterized in that: In S5, the cleaning process is repeated 1 to 3 times, and the crystal is taken out when the liquid level is about to cover the top of the crystal but has not yet covered it.
6. The method for growing 9,10-diphenylethynyl anthracene single crystals using a polymer additive as claimed in claim 5, characterized in that: S1 to S5 are all carried out in a constant temperature environment, and the constant temperature equipment is a heating table, a heat collecting constant temperature heating magnetic stirrer or a blast drying oven.
7. A 9,10-diphenylethynyl anthracene single crystal, characterized in that: The method is prepared by any one of claims 1 to 6.