Production method of cold-rolled rare earth deep drawing steel DC04 steel strip
By adding Ti alloy and rare earth Ce elements to the cold-rolled deep-drawn steel DC04 steel strip, combining the strict control of the content of C, N and harmful elements, and using optimized hot-rolled cooling and annealing processes, the steel strip forming performance and The problem of insufficient mechanical properties achieves no timeliness and high tensile strength, meeting the forming requirements of automotive parts.
Patent Information
- Application Number
- CN202410915800.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-11-05
AI Technical Summary
The existing cold-rolled deep-drawn steel DC04 steel strips have shortcomings in forming performance and mechanical properties, especially in the fixation of low-carbon and gapless atomic steels and liquid steel purification, which are difficult to meet the high requirements of automotive parts.
By adding appropriate amounts of Ti alloy elements and rare earth Ce elements to ultra-low carbon steel, carbon and nitrogen compounds are formed, combined with strict control of the content of C, N and harmful elements, and different hot rolling cooling methods and continuous annealing processes are used to optimize the steel Metallographic structure and mechanical properties of the belt.
It realizes the agelessness and excellent forming performance of steel strips, improves plasticity and tensile strength, meets the forming requirements of automotive parts, and reduces energy consumption and steel strip surface roughness.
Smart Images

Figure CN118895461A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of material forming, and in particular relates to a production method of a cold-rolled rare earth deep-drawing steel DC04 steel strip. Background Art
[0002] Cold rolled deep drawing steel DC04 belongs to ultra-low carbon IF steel, i.e. interstitial atom-free steel. This product adopts smelting technology such as BOF blowing + RH vacuum treatment to keep the C and N contents in a low range (generally ≤0.0040%), and then adds a certain amount of strong carbonitride forming elements such as titanium (Ti) and niobium (Nb) to completely fix the interstitial atoms such as carbon and nitrogen in the ultra-low carbon steel into carbonitrides, thereby obtaining clean ferritic steel, so that the steel strip has the maximum work hardening index n, plastic strain ratio r value and low yield strength ratio, thus giving it extremely excellent deep drawing performance. It has been widely used in the automotive industry and can meet the forming requirements of automotive parts such as fenders and door inner panels.
[0003] Rare earth elements Rare earth elements are added to steel, and their main functions are manifested in three aspects. The first is to purify the molten steel: deoxidation, desulfurization, reducing inclusions in the steel and reducing the effects of harmful elements; the second is to modify inclusions: rare earth elements have a stronger affinity with sulfur than iron and manganese, and their addition to the molten steel changes the composition, type and structure of sulfides. Thus, the composition, form and properties of inclusions are changed; the third is microalloying: the interaction between rare earth and carbon, chlorine, hydrogen and other alloying elements, the co-solubility of rare earth in steel and its influence on solidification, grain boundaries, phase changes, organization, etc. Summary of the invention
[0004] The purpose of the present invention is to provide a production method of a cold-rolled rare earth deep-drawing steel DC04 strip. In order to ensure that the produced cold-rolled rare earth deep-drawing steel DC04 strip has more excellent forming performance, the present invention strictly controls C, N elements and harmful elements O, S at a lower level, adds a proper amount of Ti alloy element to ultra-low carbon steel (the remaining Ti calculation formula: Ti remaining = Ti-(3.4×N+1.5×S+4×C) to carry out composition design, and considering the titanium yield and composition change, the excess titanium control range is 0.02%-0.04%), combines with carbon and nitrogen interstitial atoms in the steel to form carbonitride, so that the steel strip has obvious timelessness and realizes performance stability; at the same time, rare earth elements are added to purify molten steel, improve the r value of the steel strip, and improve the plasticity and forming performance of the product. In terms of production technology, we explored the differences in the effects of different hot rolling cooling methods on yield and tensile strength. The hot rolling process uses a stronger cooling rate to refine the metallographic structure of the steel strip, achieve fine grain strengthening, and make the steel strip obtain higher tensile strength and elongation, thereby achieving a low yield ratio and improving the product's deformation capacity. The production process goes through smelting, 2250mm rolling mill, acid continuous rolling and continuous annealing processes, focusing on the design of composition, hot rolling and cold rolling core processes.
[0005] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0006] The present invention provides a production method of a cold-rolled rare earth deep-drawing steel DC04 strip, comprising:
[0007] Steelmaking process: molten iron → converter steelmaking → RH refining → slab continuous casting; molten iron is pre-treated for desulfurization before converter smelting, and the sulfur content of the molten iron entering the converter is required to be less than 0.004%, and the slag removal area of the molten iron is greater than 95%; converter smelting requires the tapping temperature to be ≥1670℃, and a turnover bag must be used for tapping, and the tapping temperature drop is required to be less than 70℃; the RH process requires deep decarburization treatment based on the composition and temperature of the molten steel supplied by the converter to RH. After decarburization, aluminum particles are added for deoxidation according to the oxygen determination situation. After circulating for more than 5 minutes, titanium iron alloy is added to adjust the composition; after the composition adjustment is completed, ensure that the vacuum cycle is not less than 4 minutes before temperature measurement and sampling. After the addition of titanium iron, the pure degassing time is guaranteed to be more than 6 minutes. In the later stage of RH furnace vacuum treatment, 5-80kg of rare earth cerium iron alloy is added, and the superheat of the molten steel is 20-60℃;
[0008] Hot rolling process: slab heating → high-pressure water descaling → fixed width press → E1R1 roughing mill rolling → E2R2 roughing mill rolling → flying shear → high-pressure water descaling → F1-F7 finishing mill rolling → encrypted laminar cooling → coiling → pallet transportation system → sampling and inspection; the slab heating temperature is 1150-1220℃; heating time is 150-300min; the rough rolling mode is 3+3; the finishing rolling temperature is ≥890℃, and the coiling temperature is 680-760℃;
[0009] Cold rolling process: pickling uncoiling → welding → straightening → pickling → rinsing → drying → trimming → continuous rolling mill cold rolling → slitting → coiling → offline inspection → weighing → marking → bundling → packaging → storage → continuous uncoiling → welding → cleaning → entrance looper → annealing furnace → exit looper → leveling → looper inspection → trimming → surface inspection → oiling → coiling → weighing → sampling and inspection; annealing process parameters: outlet temperature of heating and soaking section 770-850℃, outlet temperature of slow cooling section 600-700℃, outlet temperature of rapid cooling section ≤400℃, temperature of over-aging section ≤400℃, outlet temperature of final cooling section ≤180℃, elongation of flat mill 0.7-1.4%;
[0010] The chemical composition of the low yield ratio by mass percentage includes: C≤0.0040%, Si≤0.030%, Mn: 0.05-0.25%, P≤0.020%, Ti 0.040-0.080%, Al 0.020-0.070%, S≤0.015%, O≤0.0030%, N≤0.0040%, Ce≤0.0060%, and the balance is Fe and unavoidable impurities.
[0011] Furthermore, the content of C and N elements is not higher than 0.0040%, the steel is pure, and the inclusions of type D are ≤1.0 grade.
[0012] Furthermore, the uniformity of mechanical properties of products in each thickness group is achieved, and the surface roughness of the steel strip ranges from 0.6 to 1.9 μm.
[0013] Furthermore, the finished product properties meet the following requirements: yield strength 130-160 MPa, tensile strength 280-330 MPa, and elongation after fracture 42.0-50.0%.
[0014] Furthermore, the finished product has an n value of 0.24-0.25 and an r value of 2.70-3.30.
[0015] Compared with the prior art, the beneficial technical effects of the present invention are:
[0016] The invention introduces a production method of a cold-rolled rare earth deep-drawing steel DC04 strip. The steelmaking process adopts RH refining process plus vacuum degassing technology, the C and N element contents are not higher than 0.0040%, the steel is pure, and the inclusion D fine system is ≤1.0 level; Ti alloy element is adopted to fix C and N interstitial atoms to form interstitial atom-free steel, which has no timeliness and good performance stability; rare earth Ce element is added to purify the steel and improve the plasticity and r value of the steel strip; the hot rolling process adopts low heating temperature to advantageously control the generation of iron oxide scale and save energy consumption, and at the same time increases the descaling water pressure to remove the iron oxide scale on the surface of the slab and improve the surface quality of the steel strip after hot rolling; the continuous annealing process adopts high temperature annealing to realize rapid recrystallization, and different leveling machine elongation rates are set according to thickness group intervals to realize the uniformity of mechanical properties of products of each thickness group interval, and the surface roughness of the steel strip ranges from 0.6 to 1.9 μm.
[0017] A certain amount of alloy Ti and rare earth Ce elements are added to ultra-low carbon steel. Ti fixes the interstitial atoms of C and N to obtain interstitial atom-free IF steel, which makes the steel strip have significant non-aging characteristics. Rare earth Ce elements purify the molten steel and improve the plasticity of the product. When the content of C and N elements is extremely low, the content of strengthening elements such as P and Mn is strictly controlled to make the steel strip have a lower yield strength and a certain tensile strength. The steelmaking process strictly controls the oxygen blowing amount to reduce the generation of inclusions; the hot rolling process adopts low heating temperature, high descaling water pressure and faster cooling method to reduce the formation of oxides on the surface of the steel strip, optimize the surface quality of the steel strip, refine the grains, and improve the tensile strength of the product through fine grain strengthening; the continuous annealing process adopts high temperature annealing, and adopts different elongation rates of the leveler according to the thickness group interval to achieve a stable performance range for products of various thickness specifications. The finished product has a yield strength of 130-160MPa, a tensile strength of 280-330MPa, an elongation of 42.0-50.0% (transverse, tensile test: L0=80mm, b=20mm), an n value of 0.24-0.25, an r value of 2.70-3.30, and a surface roughness of 0.6-1.9μm. It ensures a high elongation and r value, thus having excellent stamping performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] The present invention will be further described below in conjunction with the accompanying drawings.
[0019] Figure 1 This is the metallographic structure of the finished product. DETAILED DESCRIPTION
[0020] A method for producing a cold-rolled rare earth deep-drawing steel DC04 strip, comprising:
[0021] 1. Smelting process
[0022] 1.1 Desulfurization pretreatment: KR hot metal desulfurization technology is used, and the final sulfur content after deep desulfurization is required to be within 0.004%. KR desulfurization is desulfurized by mechanical stirring. The stirring head is inserted into the molten iron and rotated to make the molten iron produce a vortex. Then the desulfurizer is added into the molten iron vortex to make the desulfurization reaction between the desulfurizer and the sulfur in the molten iron occur during continuous stirring. After desulfurization is completed, the desulfurization slag is thoroughly scraped off. The scraping area of the molten iron slag is required to be greater than 95% to prevent high-sulfur slag from being added to the converter and causing backsulfurization.
[0023] 1.2 Converter smelting: The molten iron is pre-treated for desulfurization before converter smelting. The converter dephosphorization process mainly relies on slag with high basicity, high oxidation and large slag volume for dephosphorization. However, in order to achieve deep dephosphorization, it is necessary to create conditions so that the phosphorus in the molten iron can be oxidized into the slag in large quantities to achieve the goal of deep dephosphorization. The phosphorus content of the molten iron entering the converter is ≤0.020%, oxygen is blown to decarburize and the temperature is raised to control the P and S components to prevent the molten steel from overoxidation. The converter terminal temperature is controlled at above 1670℃, and a turnover bag must be used for steel tapping. The temperature drop of steel tapping is required to be less than 70℃. Ferromanganese is added for alloying during the converter tapping process, and lime and modifiers are added for top slag modification.
[0024] 1.3 Refining: RH refining furnace carries out decarburization treatment according to the composition and temperature of molten steel. RH decarburization is the most important decarburization link in the production of ultra-low carbon steel. Due to the high temperature and strong stirring during vacuum treatment, all factors that are conducive to increasing the decarburization rate can accelerate the decarburization reaction. In the process of rapid pressure reduction in the vacuum chamber, as the lifting gas flow rate increases, the circulation flow rate and volume coefficient increase, the decarburization rate is increased, and the decarburization reaction is accelerated. After decarburization, deoxidizer and component aluminum are added according to the oxygen determination situation. After circulating for more than 5 minutes, titanium iron, niobium iron, metal manganese, micro-carbon silicon iron, phosphorus and other alloys are added to adjust the composition. After the adjustment of the composition, ensure that the vacuum cycle is 4 minutes before temperature measurement and sampling. After the addition of titanium iron, the pure degassing time is guaranteed to be more than 6 minutes to ensure the uniformity of the temperature and composition of the molten steel, which is also conducive to the floating of molten steel inclusions. In the later stage of vacuum treatment, 5-80kg of rare earth cerium iron alloy is added to improve the cleanliness of the molten steel.
[0025] 1.4 Continuous casting: Continuous casting protects pouring to prevent secondary oxidation of molten steel and avoid secondary oxidation of steel quality. Constant pulling speed is adopted, and the pulling speed is controlled at 0.8-2.0m / min. The appropriate superheat of pouring is controlled, and the superheat during pouring is controlled at about 20-60℃, which promotes the floating of inclusions and realizes multi-furnace pouring.
[0026] 2 Hot rolling process
[0027] The ingot is heated by a walking-beam heating furnace (the heating process is shown in Table 1). The rough rolling adopts double-stand R1 and R2 reciprocating rolling. The rough rolling mode is 3+3, and the descaling water pressure is not less than 180 bar. The finishing rolling adopts the F1-F7 continuous rolling process. The finishing rolling temperature is ≥890°C to ensure rolling in the austenite single-phase zone. The coiling temperature is 680-760°C to ensure the normal precipitation of carbonitrides and improve the deep drawing performance. The specific hot rolling process is shown in Table 2.
[0028] Table 1 Billet heating system
[0029]
[0030] Table 2 Rolling process
[0031]
[0032] 3 Annealing process
[0033] Annealing uses a vertical continuous annealing furnace, which is cooled by a reducing atmosphere and a nitrogen-hydrogen mixed protective atmosphere. The temperature range of the heating section and soaking section is 770-850℃ to ensure complete recrystallization of the grains. The temperature control of each section of the heating furnace is shown in Table 3, and the elongation control of the flattener at different thicknesses is shown in Table 4.
[0034] Table 3 Annealing process
[0035]
[0036] Table 4 Elongation of the flat-pass mill
[0037]
[0038] 4. Example Analysis
[0039] 4.1 Steelmaking ingredients
[0040] According to the above steelmaking process requirements, the actual slab chemical composition (mass percentage) is shown in Table 5 below.
[0041] Table 5 Chemical composition of examples wt.%
[0042]
[0043] 4.2 Hot rolling performance
[0044] According to the above designed chemical composition and hot rolling process, the room temperature tensile properties of the hot rolled plate are shown in Table 6, the tensile specimen L0 = 80 mm, b = 20 mm (transverse), and the test method refers to GB / T 228.1.
[0045] Table 6 Hot rolling tensile properties
[0046]
[0047] 4.3 Finished product performance
[0048] Cold rolling and annealing are carried out on the basis of the above hot rolling properties. The room temperature tensile mechanical properties of the finished product are shown in Table 7. The metallographic structure is equiaxed ferrite with a grain size of 7.5-9.0 and a microstructure of Figure 1 .
[0049] Table 7 Finished product tensile properties
[0050]
[0051] In summary, this product has passed the performance test and all performance requirements are met. It has met the forming requirements after user trial mold use. The supply of key parts has been achieved, with an annual supply of about 2,000 tons.
[0052] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A method for producing cold-rolled rare earth deep-drawing steel DC04 strip, characterized in that: include: Steelmaking process: molten iron → converter steelmaking → RH refining → slab continuous casting; molten iron is pre-treated for desulfurization before converter smelting, and the sulfur content of the molten iron entering the converter is required to be less than 0.004%, and the slag removal area of the molten iron is greater than 95%; converter smelting requires the tapping temperature to be ≥1670℃, and a turnover bag must be used for tapping, and the tapping temperature drop is required to be less than 70℃; the RH process requires deep decarburization treatment based on the composition and temperature of the molten steel supplied by the converter to RH. After decarburization, aluminum particles are added for deoxidation according to the oxygen determination situation. After circulating for more than 5 minutes, titanium iron alloy is added to adjust the composition; after the composition adjustment is completed, ensure that the vacuum cycle is not less than 4 minutes before temperature measurement and sampling. After the addition of titanium iron, the pure degassing time is guaranteed to be more than 6 minutes. In the later stage of RH furnace vacuum treatment, 5-80kg of rare earth cerium iron alloy is added, and the superheat of the molten steel is 20-60℃; Hot rolling process: slab heating → high-pressure water descaling → fixed width press → E1 R1 roughing mill rolling → E2R2 roughing mill rolling → flying shear → high-pressure water descaling → F1-F7 finishing mill rolling → encrypted laminar cooling → coiling → pallet transportation system → sampling and inspection; the slab heating temperature is 1150-1220℃; heating time is 150-300min; the rough rolling mode is 3+3; the finishing rolling temperature is ≥890℃, and the coiling temperature is 680-760℃; Cold rolling process: pickling uncoiling → welding → straightening → pickling → rinsing → drying → trimming → continuous rolling mill cold rolling → slitting → coiling → offline inspection → weighing → marking → bundling → packaging → storage → continuous uncoiling → welding → cleaning → entrance looper → annealing furnace → exit looper → leveling → looper inspection → trimming → surface inspection → oiling → coiling → weighing → sampling and inspection; annealing process parameters: outlet temperature of heating and soaking section 770-850℃, outlet temperature of slow cooling section 600-700℃, outlet temperature of rapid cooling section ≤400℃, temperature of over-aging section ≤400℃, outlet temperature of final cooling section ≤180℃, elongation of flat mill 0.7-1.4%; The chemical composition of the low yield ratio by mass percentage includes: C≤0.0040%, Si≤0.030%, Mn: 0.05-0.25%, P≤0.020%, Ti 0.040-0.080%, Al 0.020-0.070%, S≤0.015%, O≤0.0030%, N≤0.0040%, Ce≤0.0060%, and the balance is Fe and unavoidable impurities.
2. The method for producing cold-rolled rare earth deep-drawing steel DC04 strip according to claim 1, characterized in that: The content of C and N elements is not higher than 0.0040%, the steel is pure, and the inclusions of type D are ≤1.0 grade.
3. The method for producing cold-rolled rare earth deep-drawing steel DC04 strip according to claim 1, characterized in that: The uniformity of mechanical properties of products in each thickness group is achieved, and the surface roughness of the steel strip ranges from 0.6-1.9μm.
4. The method for producing the cold-rolled rare earth deep-drawing steel DC04 strip according to claim 1, characterized in that: The finished product performance meets the following requirements: yield strength 130-160MPa, tensile strength 280-330MPa, elongation after fracture 42.0-50.0%.
5. The method for producing the cold-rolled rare earth deep-drawing steel DC04 strip according to claim 4, characterized in that: Finished product: n value 0.24-0.25, r value 2.70-3.30.